Copolymer, rubber composition, and crosslinked rubber product

Through the combination of specific copolymers and fillers, the balance problem of rubber crosslinkers between damage resistance, wet grip and low heat generation is solved, and high-performance rubber crosslinkers are realized, suitable for high-load tires, etc. field.

CN118900875APending Publication Date: 2024-11-05ZEON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028685.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-13
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing rubber crosslinks are difficult to have both damage resistance, wet grip and low heat generation, especially in tire applications where environmental and safety requirements conflict.

Method used

A copolymer with specific structural units is generated by cross-metastatic reaction, combined with carbon material or silica as a filler to form a rubber crosslinker with excellent damage resistance, wet grip and low heat generation properties.

Benefits of technology

It has achieved a significant improvement in the damage resistance, wet grip and low heat generation of rubber crosslinked materials. It is suitable for applications such as high-load tires, and is also improved to wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900875A_ABST
    Figure CN118900875A_ABST
Patent Text Reader

Abstract

Provided is a copolymer represented by general formula (1). (In general formula (1), R1 to R4 are each independently a hydrogen atom, a halogen atom, an optionally substituted hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a silicon atom, an oxygen atom, or a nitrogen atom, x is 0 to 2 (excluding when all of R1 to R4 are hydrogen atoms and x = 0), R5 is a hydrogen atom or a methyl group, p is 30 to 2000, q is 0 to 2000, p + q is 30 to 2000, and n is 200 to 5000. R1 and R2, and R3 and R4 can each bond to form a ring. In general formula (1), the values of a plurality of R1-R5 and x may be the same as or different from each other. > # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a copolymer, a rubber composition and a cross-linked rubber, and more particularly to a copolymer capable of providing a cross-linked rubber having excellent damage resistance, wet grip and low heat build-up properties, and a rubber composition and a cross-linked rubber obtained using such a copolymer. Background Art

[0002] It is known that cyclopentene and norbornene compounds are generally subjected to metathesis ring-opening polymerization in the presence of a so-called Ziegler-Natta catalyst consisting of a transition metal compound of Group 6 of the periodic table such as WCl6, MoCl5, and an organometallic activator such as triisobutylaluminum, diethylaluminum chloride, and tetrabutyltin, thereby providing an unsaturated linear ring-opening polymer. In addition, it is known that a method for improving the affinity of a polymer for inorganic particles is introduced into the end of a polymer chain containing a functional group containing a heteroatom.

[0003] For example, Patent Document 1 discloses a composition for a material having a damage resistance property, which comprises an inorganic material and a ring-opening copolymer, wherein the ring-opening copolymer comprises a structural unit derived from a monocyclic cyclic olefin and a structural unit derived from a norbornene compound. According to the technology of Patent Document 1, a rubber cross-linked product having excellent damage resistance and chipping resistance and suitable for tire applications can be provided. On the other hand, in recent years, low fuel consumption (low heat generation) is strongly required for rubber cross-linked products used for tire applications from the perspective of environmental and resource issues, and excellent wet grip is also required from the perspective of safety.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent document 1: Japanese Patent Application Publication No. 2020-15832. Summary of the invention

[0007] Problem that the invention aims to solve

[0008] The present invention has been made in view of such actual circumstances, and an object of the present invention is to provide a copolymer capable of providing a rubber cross-linked product having excellent damage resistance, wet grip performance and low heat build-up properties.

[0009] Solutions for solving problems

[0010] The present inventors have conducted studies to achieve the above-mentioned object and, as a result, have found that the above-mentioned problems can be solved by a copolymer having specific structural units, thereby completing the present invention.

[0011] That is, according to the present invention, a copolymer represented by the following general formula (1) can be provided.

[0012] [Chemical formula 1]

[0013]

[0014] (In the above general formula (1), R 1 ~R 4 are each independently a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom, and x is 0 to 2 (wherein R 1 ~R 4 Except for the case where all of them are hydrogen atoms and x=0), R 5 is a hydrogen atom or a methyl group, p is 30 to 2000, q is 0 to 2000, p+q=30 to 2000, and n is 200 to 5000. 1 With R 2 , R 3 With R 4 In the above general formula (1), the plurality of R 1 ~R 5 The values ​​of and x may be the same or different. )

[0015] Furthermore, according to the present invention, there is provided a rubber composition comprising the above copolymer and a filler.

[0016] In the rubber composition of the present invention, the filler is preferably a carbon material.

[0017] In the rubber composition of the present invention, the filler is preferably silica.

[0018] According to the present invention, there is provided a cross-linked rubber obtained by cross-linking the above-mentioned rubber composition.

[0019] In addition, according to the present invention, a method for producing the above-mentioned copolymer can be provided, which comprises the following steps: subjecting a first ethylenically unsaturated polymer having an alicyclic structure and an unsaturated bond carbon content of 10 to 40 mol % and a second ethylenically unsaturated polymer not having an alicyclic structure and an unsaturated bond carbon content of 20 to 50 mol % to a cross-metathesis reaction in the presence of a metathesis catalyst, thereby obtaining a copolymer represented by the above-mentioned general formula (1).

[0020] Effects of the Invention

[0021] According to the present invention, there can be provided a copolymer capable of providing a rubber cross-linked product having excellent damage resistance, wet grip performance and low heat build-up properties. DETAILED DESCRIPTION

[0022] The copolymer of the present invention is represented by the following general formula (1).

[0023] [Chemical formula 2]

[0024]

[0025] In the above general formula (1), R 1 ~R 4 are each independently a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom, and x is 0 to 2 (wherein R 1 ~R 4 Except for the case where all of them are hydrogen atoms and x=0), R 5 is a hydrogen atom or a methyl group, p is 30 to 2000, q is 0 to 2000, p+q=30 to 2000, and n is 200 to 5000. 1 With R 2 , R 3 With R 4 In the above general formula (1), the plurality of R 1 ~R 5 The values ​​of and x may be the same or different.

[0026] The copolymer of the present invention is a copolymer represented by the general formula (1). As shown in the general formula (1), it is a random copolymer having p structural units A, q structural units B, and n structural units C, wherein these structural units A to C are randomly bonded. The randomness of the copolymer represented by the general formula (1) is not particularly limited. For example, the copolymer may be a copolymer having a block composed of about 2 to 40 structural units A in a row, a copolymer having a block composed of about 2 to 40 structural units B in a row, or a copolymer having a block composed of about 2 to 40 structural units C in a row. In addition, in the above general formula (1), the carbon-carbon double bond structure contained in the structural unit A, the carbon-carbon double bond structure contained in the structural unit B, and the carbon-carbon double bond structure contained in the structural unit C may not be either the cis structure or the trans structure, but may be either the cis structure or the trans structure, without any special limitation (in the above general formula (1), although the case of the trans structure is recorded as an example, it may be either the cis structure or the trans structure.).

[0027] In addition, the structural unit C is a structure having a double bond on the polymer main chain, but a part of the structural unit C can also be a structural unit having a double bond on the side chain represented by the following formula (C') or the following formula (C"). That is, the copolymer represented by the above general formula (1) can have the structural unit A, the arbitrarily included structural unit B, the structural unit C, and the structural unit represented by the following formula (C') and / or the structural unit represented by the following formula (C").

[0028] [Chemical formula 3]

[0029]

[0030] In the above general formula (1), R 1 ~R 4 Each is independently a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom, and is preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms which may have a substituent.

[0031] Examples of the halogen atom include a fluorine atom, a chlorine atom, and a bromine atom.

[0032] Examples of the hydrocarbon group having 1 to 20 carbon atoms which may have a substituent include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl, hexyl, heptyl, octyl, nonyl, and decyl; cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and cycloheptyl; alkenyl groups such as vinyl, 1-propenyl, allyl, 1-butenyl, 2-butenyl, pentenyl, hexenyl, and cyclohexenyl; alkynyl groups such as ethynyl, 1-propynyl, 2-propynyl (propargyl), 3-butynyl, pentynyl, and hexynyl; aryl groups such as phenyl, tolyl, xylyl, biphenyl, 1-naphthyl, 2-naphthyl, anthracenyl, and phenanthryl; and aralkyl groups such as benzyl and phenethyl. Examples of the substituents for these groups include halogen atoms such as fluorine atoms and chlorine atoms; and alkoxy groups such as methoxy and ethoxy.

[0033] In the above general formula (1), x is 0 to 2, preferably 0 or 1. In the above general formula (1), p is 30 to 2000, preferably 45 to 1900, and more preferably 60 to 1800. By setting p within the above range, the obtained rubber cross-linked product can be excellent in damage resistance, wet grip and low heat generation. In the above general formula (1), the plurality of R 1 ~R 4 The values ​​of and x may be the same or different. That is, in the general formula (1), two or more structural units A are included, and R 1 ~R 4 The values ​​of and x may be the same or different. For example, as the structural unit A, R 1 ~R 3 is a hydrogen atom, R 4 A structural unit in which x is 0 and R 1 ~R 4 A structural unit in which x is a hydrogen atom and x=1.

[0034] In the present invention, in the above general formula (1), R1 ~R 4 Except for the case where all are hydrogen atoms and x=0. That is, the copolymer represented by the general formula (1) must contain: a structural unit in which x is 1 or 2; or a structural unit in which x is 0 and R 1 ~R 4 At least one of the structural units is a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom (that is, excluding a hydrogen atom).

[0035] In the above general formula (1), q is 0 to 2000, preferably 0 to 1900, and more preferably 0 to 1800. By setting q within the above range, the obtained rubber cross-linked product can be excellent in fracture resistance, wet grip and low heat generation. 1 ~R 4 A structural unit in which all of the atoms are hydrogen and x=0.

[0036] p+q is 30 to 2000, preferably 45 to 1900, and more preferably 60 to 1800. When p+q is within the above range, the obtained rubber cross-linked product can be excellent in fracture resistance, wet grip performance, and low heat build-up properties.

[0037] In the above general formula (1), R 5 It is a hydrogen atom or a methyl group, and is preferably a hydrogen atom.

[0038] In the above general formula (1), n ​​is 200 to 5000, preferably 250 to 4500, and more preferably 300 to 4000. By setting n within the above range, the obtained rubber cross-linked product can be excellent in damage resistance, wet grip and low heat generation. 5 Can be the same or different, R 5 Preferably they are the same.

[0039] In the general formula (1), the ratio of p+q to n is preferably p+q:n=10:90 to 70:30, more preferably 15:85 to 65:35, and even more preferably 20:80 to 60:40. By making the ratio of p+q:n within the above range, the obtained rubber cross-linked product can be made more excellent in fracture resistance, wet grip and low heat build-up properties.

[0040] In the general formula (1), the ratio of the sum of the structural unit A and the structural unit B to the structural unit C is preferably 30:70 to 75:25, more preferably 35:65 to 70:30, and even more preferably 40:60 to 65:35, in terms of the weight ratio of structural unit A+structural unit B:structural unit C. By setting the ratio of the sum of the structural unit A and the structural unit B to the structural unit C within the above range, the obtained rubber cross-linked product can be made more excellent in fracture resistance, wet grip and low heat build-up properties.

[0041] The weight average molecular weight (Mw) of the copolymer represented by the general formula (1) of the present invention is not particularly limited, but is preferably 50,000 to 1,000,000, more preferably 100,000 to 500,000, and further preferably 140,000 to 260,000. By making the weight average molecular weight (Mw) within the above range, the obtained rubber cross-linked product can be made more excellent in damage resistance, wet grip and low heat generation. In addition, the molecular weight distribution (Mw / Mn) of the copolymer represented by the general formula (1) is not particularly limited, but is preferably 1.0 to 5.0, and more preferably 1.5 to 3.0. In the present invention, the weight average molecular weight (Mw), the number average molecular weight (Mn) and the molecular weight distribution (Mw / Mn) can be measured by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent and obtained as polystyrene conversion values.

[0042] The glass transition temperature (Tg) of the copolymer represented by the general formula (1) of the present invention is preferably -80 to 10° C., more preferably -70 to 0° C., and further preferably -65 to -5° C. When the glass transition temperature (Tg) is within the above range, the obtained rubber cross-linked product can be made more excellent in fracture resistance, wet grip and low heat build-up properties.

[0043] The manufacturing method of the copolymer shown in the general formula (1) used in the present invention is not particularly limited, and a first ethylenically unsaturated polymer having an alicyclic structure and an unsaturated carbon content of 10 to 40 mol% and a second ethylenically unsaturated polymer having no alicyclic structure and an unsaturated carbon content of 20 to 50 mol% can be subjected to a cross metathesis reaction in the presence of a metathesis catalyst, thereby appropriately manufacturing. The unsaturated carbon content of the first ethylenically unsaturated polymer is preferably 10 to 38 mol%, more preferably 11 to 35 mol%, and the unsaturated carbon content of the second ethylenically unsaturated polymer is preferably 25 to 50 mol%, more preferably 30 to 50 mol%. In addition, the unsaturated carbon content is the ratio of carbon atoms constituting carbon-carbon double bonds and carbon-carbon triple bonds among the carbon atoms constituting the first ethylenically unsaturated polymer and the second ethylenically unsaturated polymer. Here, the unsaturated carbon content does not include carbon atoms constituting aromatic double bonds.

[0044] As mentioned above, the copolymer shown in the general formula (1) of the present invention can be suitably manufactured by making the first ethylenically unsaturated polymer and the second ethylenically unsaturated polymer undergo cross-metathesis reaction in the presence of a metathesis catalyst. According to the cross-metathesis reaction, by the effect of a metathesis catalyst, an exchange reaction of carbon-carbon double bonds is carried out between the carbon-carbon double bonds constituting the first ethylenically unsaturated polymer and the carbon-carbon double bonds constituting the second ethylenically unsaturated polymer, thus the copolymer shown in the general formula (1) can be obtained.

[0045] For example, as the first ethylenically unsaturated polymer, a polymer represented by the following general formula (2) can be preferably used, and as the second ethylenically unsaturated polymer, a polymer represented by the following general formula (3) can be preferably used. Hereinafter, the case of using the polymer represented by the following general formula (2) and the polymer represented by the following general formula (3) will be described.

[0046] [Chemical formula 4]

[0047]

[0048] (In the above general formula (2), R 1 ~R 4 are each independently a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom, and x is 0 to 2 (wherein R 1 ~R 4 (except the case where all are hydrogen atoms and x=0), p' is 100 to 10000, q' is 0 to 10000, and p'+q' is 100 to 10000. 1 With R 2 , R 3 With R 4 In the above general formula (2), the multiple R 1 ~R 4 The values ​​of and x may be the same or different. )

[0049] [Chemical formula 5]

[0050]

[0051] (In the above general formula (3), R 5 is a hydrogen atom or a methyl group, and n' is 500 to 20000. 5 They can be the same or different.)

[0052] Then, when the polymer represented by the general formula (2) is reacted with the polymer represented by the general formula (3) in the presence of a metathesis catalyst, a carbon-carbon double bond exchange reaction occurs between the carbon-carbon double bonds contained in the polymer represented by the general formula (2) (the carbon-carbon double bonds in the p' structural units contained and the carbon-carbon double bonds in the q' structural units contained) and the carbon-carbon double bonds contained in the polymer main chain of the polymer represented by the general formula (3) (the carbon-carbon double bonds in the n' structural units contained), thereby obtaining the following polymer, wherein the structural unit corresponding to the structural unit A in the general formula (1) and the structural unit corresponding to the structural unit B in the general formula (1) among the structural units constituting the polymer represented by the general formula (2) are randomly bonded to the structural units constituting the polymer represented by the general formula (3). In addition, at this time, since the polymer represented by the above general formula (2) and the polymer represented by the above general formula (3) are used, it can be a polymer having a block composed of about 2 to 40 structural units derived from the polymer represented by the above general formula (2) in succession, and it can also be a polymer having a block composed of about 2 to 40 structural units derived from the polymer represented by the above general formula (3) in succession.

[0053] In the above general formula (2), R 1 ~R 4 Each independently represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and the preferred range and specific examples thereof are the same as those of the above general formula (1) (wherein R 1 ~R 4 All of them are hydrogen atoms and x=0). x is 0 to 2, preferably 0 or 1. p' is 100 to 10000, preferably 150 to 7500, more preferably 200 to 5000, q' is 0 to 10000, preferably 0 to 7500, more preferably 0 to 5000. In addition, p'+q' is 100 to 10000, preferably 150 to 7500, more preferably 200 to 5000.

[0054] The polymer represented by the general formula (2) can be produced, for example, by ring-opening polymerization of a compound represented by the following general formula (4).

[0055] [Chemical formula 6]

[0056]

[0057] In the above general formula (4), R 1 ~R 4Each is independently a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom, and the preferred range and specific examples thereof are the same as those of the above general formula (1). x is 0 to 2, preferably 0 or 1. Among them, as the compound represented by the above general formula (4), it is necessary to use: a compound in which x is 1 or 2; or a compound in which x is 0 and R 1 ~R 4 A compound in which at least one of the substituents is a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom (that is, other than a hydrogen atom).

[0058] Specific examples of the compound represented by the general formula (4) include the following compounds.

[0059] 2-norbornene, 5-methyl-2-norbornene, 5-ethyl-2-norbornene, 5-butyl-2-norbornene, 5-hexyl-2-norbornene, 5-decyl-2-norbornene, 5-cyclohexyl-2-norbornene, 5-cyclopentyl-2-norbornene, 5-ethylidene-2-norbornene, 5-vinyl-2-norbornene, 5-propenyl-2-norbornene, 5-cyclohexenyl-2-norbornene, 5-cyclopentenyl-2-norbornene, 5-phenyl-2-norbornene, tetracyclo[9.2.1.0 2,10 .0 3,8 ]tetradeca-3,5,7,12-tetraene (also known as 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene), tetracyclo[10.2.1.0 2,11 .0 4,9 ]pentadeca-4,6,8,13-tetraene (also known as 1,4-methano-1,4,4a,9,9a,10-hexahydroanthracene), dicyclopentadiene, methyldicyclopentadiene and dihydrodicyclopentadiene (tricyclo[5.2.1.0 2,6 ] dec-8-ene) and other unsubstituted or hydrocarbon-substituted bicyclo[2.2.1]hept-2-enes;

[0060] Four rings [6.2.1.1 3,6 .0 2,7 ] dodec-4-ene (tetracyclododecene), 9-methyltetracyclo[6.2.1.1 3,6 .0 2 ,7 ] dodec-4-ene, 9-ethyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-cyclohexyltetracyclo[6.2.1.1 3,6 .0 2 ,7] dodec-4-ene, 9-cyclopentyltetracyclo[6.2.1.1 3,6 .0 2,7 ]Dodec-4-ene, 9-methylenetetracyclo[6.2.1.1 3, 6 .0 2,7 ] dodec-4-ene, 9-ethylenetetracyclo[6.2.1.1 3,6 .0 2,7 ]Dodec-4-ene, 9-vinyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-propenyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-cyclohexenyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene, 9-cyclopentenyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene and 9-phenyltetracyclo[6.2.1.1 3,6 .0 2,7 ] unsubstituted or hydrocarbon-substituted tetracyclic rings such as dodec-4-ene [6.2.1.1 3,6 .0 2,7 ] Dodeca-4-enes;

[0061] Bicyclo[2.2.1]hept-2-enes having an alkoxycarbonyl group, such as methyl 5-norbornene-2-carboxylate, ethyl 5-norbornene-2-carboxylate, methyl 2-methyl-5-norbornene-2-carboxylate, and ethyl 2-methyl-5-norbornene-2-carboxylate;

[0062] Four rings [6.2.1.1 3,6 .0 2,7 ] methyl dodec-9-ene-4-carboxylate and 4-methyltetracyclo[6.2.1.1 3,6 .0 2,7 ] tetracyclic [6.2.1.1] having an alkoxycarbonyl group, such as methyl dodec-9-ene-4-carboxylate 3,6 .0 2,7 ] Dodeca-4-enes;

[0063] Bicyclo[2.2.1]hept-2-enes having a hydroxycarbonyl group or anhydride group, such as 5-norbornene-2-carboxylic acid, 5-norbornene-2,3-dicarboxylic acid and 5-norbornene-2,3-dicarboxylic anhydride;

[0064] Four rings [6.2.1.1 3,6 .0 2,7 ]Dodec-9-ene-4-carboxylic acid, tetracyclo[6.2.1.13,6 .0 2,7 ] dodec-9-ene-4,5-dicarboxylic acid and tetracyclo[6.2.1.1 3,6 .0 2,7 ] tetracyclic [6.2.1.1] having a hydroxycarbonyl group or anhydride group such as dodec-9-ene-4,5-dicarboxylic anhydride 3,6 .0 2,7 ] Dodeca-4-enes;

[0065] Bicyclo[2.2.1]hept-2-enes having a hydroxyl group, such as 5-hydroxy-2-norbornene, 5-hydroxymethyl-2-norbornene, 5,6-bis(hydroxymethyl)-2-norbornene, 5,5-bis(hydroxymethyl)-2-norbornene, 5-(2-hydroxyethoxycarbonyl)-2-norbornene and 5-methyl-5-(2-hydroxyethoxycarbonyl)-2-norbornene;

[0066] Four rings [6.2.1.1 3,6 .0 2,7 ] dodec-9-ene-4-methanol and tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodeca-9-en-4-ol and other tetracyclic rings having a hydroxyl group [6.2.1.1 3,6 .0 2,7 ] Dodeca-4-enes;

[0067] Bicyclo[2.2.1]hept-2-enes having a formyl group, such as 5-norbornene-2-carboxaldehyde;

[0068] Four rings [6.2.1.1 3,6 .0 2,7 ] tetracyclic [6.2.1.1] having a formyl group such as dodec-9-ene-4-carbaldehyde 3,6 .0 2 ,7 ] Dodeca-4-enes;

[0069] Bicyclo[2.2.1]hept-2-enes having an alkoxycarbonyl group and a hydroxycarbonyl group, such as 3-methoxycarbonyl-5-norbornene-2-carboxylic acid;

[0070] Bicyclo[2.2.1]hept-2-enes having a carbonyl group such as 5-norbornene-2-yl acetate, 2-methyl-5-norbornene-2-yl acetate, 5-norbornene-2-yl acrylate and 5-norbornene-2-yl methacrylate;

[0071] 9-Tetracyclic [6.2.1.1 3,6 .0 2,7 ] dodec-4-enyl acetate, 9-tetracyclo[6.2.1.1 3,6 .02,7 ] dodec-4-enyl acrylate and 9-tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-enyl methacrylate and the like, tetracyclic [6.2.1.1 3,6 .0 2,7 ] Dodeca-4-enes;

[0072] Bicyclo[2.2.1]hept-2-enes having a functional group containing a nitrogen atom, such as 5-norbornene-2-carbonitrile, 5-norbornene-2-carboxamide, and 5-norbornene-2,3-dicarboxylic acid imide;

[0073] Four rings [6.2.1.1 3,6 .0 2,7 ]Dodec-9-ene-4-carbonitrile, tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-9-ene-4-carboxamide and tetracyclo[6.2.1.1 3,6 .0 2,7 ] tetracyclic [6.2.1.1] having a functional group containing a nitrogen atom such as dodec-9-ene-4,5-dicarboxylic acid imide 3,6 .0 2,7 ] Dodeca-4-enes;

[0074] Bicyclo[2.2.1]hept-2-enes having a halogen atom such as 5-chloro-2-norbornene;

[0075] 9-Chlorotetracyclic [6.2.1.1 3,6 .0 2,7 ] tetracyclic rings having halogen atoms such as dodec-4-ene [6.2.1.1 3,6 .0 2,7 ] Dodeca-4-enes;

[0076] Bicyclo[2.2.1]hept-2-enes having a functional group containing a silicon atom, such as 5-trimethoxy-2-norbornene and 5-triethoxy-2-norbornene;

[0077] 4-Trimethoxysilyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-9-ene, 4-triethoxysilyltetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-9-ene and other tetracyclic rings having a functional group containing a silicon atom [6.2.1.1 3,6 .0 2,7 ] Dodeca-4-enes;

[0078] As the compound represented by the general formula (4), unsubstituted or hydrocarbon-substituted bicyclo[2.2.1]hept-2-ene, unsubstituted or hydrocarbon-substituted tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-enes, particularly preferably 2-norbornene, dicyclopentadiene, tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodec-4-ene (tetracyclododecene), tetracyclo[9.2.1.0 2 ,10 .0 3,8 ]Tetradecane-3,5,7,12-tetraene (1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene, MTHF). By using 2-norbornene as the compound represented by the above general formula (4), the polymer represented by the above general formula (2) can be made into a polymer with q'=1 or more. Where 2-norbornene is used as the compound represented by the above general formula (4), a compound other than 2-norbornene is also used as the compound represented by the above general formula (4) to prepare a copolymer.

[0079] The compound represented by the general formula (4) may be used alone or in combination of two or more. That is, it may be a compound obtained by copolymerizing two or more monomers.

[0080] There are no particular limitations on the method for ring-opening polymerization of the compound represented by the general formula (4), and examples thereof include a method for ring-opening polymerization of the compound represented by the general formula (4) in a solvent in the presence of a ring-opening polymerization catalyst. Examples of ring-opening polymerization catalysts include a combination of a transition metal compound of Group 6 of the periodic table as a main catalyst and an organic metal compound as a co-catalyst, and a metathesis catalyst such as a ruthenium carbene complex. When the compound represented by the general formula (4) is ring-opened, an olefin compound or a diolefin compound may be added to the polymerization reaction system as a molecular weight regulator.

[0081] The weight average molecular weight (Mw) of the polymer represented by the general formula (2) is not particularly limited, but is preferably 50,000 to 1,000,000, more preferably 50,000 to 750,000, and further preferably 100,000 to 500,000. In addition, the molecular weight distribution (Mw / Mn) of the copolymer represented by the general formula (2) is not particularly limited, but is preferably 1.0 to 5.0, and more preferably 1.5 to 3.0.

[0082] The polymer represented by the general formula (3) is not particularly limited, and examples thereof include polybutadiene, polyisoprene, and copolymers of butadiene and isoprene.

[0083] In the above general formula (3), R5 is a hydrogen atom or a methyl group, and n' is 500 to 20000. n' is preferably 750 to 20000, and more preferably 1000 to 15000.

[0084] For example, when polybutadiene, polyisoprene, or a copolymer of butadiene and isoprene is used as the polymer represented by the general formula (3), the amount of vinyl bonds therein is not particularly limited. As the copolymer of polybutadiene, polyisoprene, or butadiene and isoprene, for example, a material obtained by anion polymerization using an organic active metal capable of anion polymerization such as an organic alkali metal compound, an organic alkaline earth metal compound, or an organic lanthanide rare earth metal compound can be used. In addition, as the polyisoprene, in addition to using synthetic polyisoprene, natural rubber can also be used.

[0085] The weight average molecular weight (Mw) of the polymer represented by the general formula (3) is not particularly limited, but is preferably 50,000 to 1,000,000, more preferably 50,000 to 750,000, and further preferably 100,000 to 500,000. In addition, the molecular weight distribution (Mw / Mn) of the polymer represented by the general formula (3) is not particularly limited, but is preferably 1.0 to 5.0, and more preferably 1.5 to 3.0.

[0086] Then, the copolymer represented by the general formula (1) of the present invention is manufactured by making the polymer (first ethylenically unsaturated polymer) represented by the general formula (2) and the polymer (second ethylenically unsaturated polymer) represented by the general formula (3) cross metathesis reaction in the presence of a metathesis catalyst. In addition, as the polymer (first ethylenically unsaturated polymer) represented by the general formula (2) and the polymer (second ethylenically unsaturated polymer) represented by the general formula (3), two or more kinds of them can also be used in combination. In addition, as the first ethylenically unsaturated polymer, the ring-opening homopolymer of 2-norbornene can also be used in combination.

[0087] In addition, the amount of the polymer represented by the general formula (2) (first ethylenically unsaturated polymer) and the polymer represented by the general formula (3) (second ethylenically unsaturated polymer) used is not particularly limited and can be selected based on the ratio of p+q to n in the general formula (1). The weight ratio of "polymer represented by the general formula (2) (first ethylenically unsaturated polymer): polymer represented by the general formula (3) (second ethylenically unsaturated polymer)" is preferably 90:10 to 20:80, more preferably 80:20 to 30:70, and even more preferably 70:30 to 40:60.

[0088] As metathesis catalyst, a complex formed by bonding a transition metal atom as a central atom, a plurality of ions, atoms, polyatomic ions and / or compounds can be used. As a transition metal atom, an atom of the 5th, 6th and 8th families of the periodic table of elements (long period type periodic table of elements, the same below) can be used. As such a transition metal atom, it is not particularly limited, as an atom of the 5th family, for example vanadium, niobium, tantalum can be enumerated, as an atom of the 6th family, for example molybdenum, tungsten can be enumerated, as an atom of the 8th family, for example ruthenium, osmium can be enumerated.

[0089] Among these, as metathesis catalysts, it is preferred to use: complexes of molybdenum and tungsten of Group 6; complexes of ruthenium and osmium of Group 8, and particularly preferred: complex catalysts of molybdenum and tungsten; carbene complexes of molybdenum, tungsten and ruthenium. Ruthenium carbene complexes are relatively stable to oxygen and moisture in the air, are not easily deactivated, and have excellent catalytic activity, so they are preferred.

[0090] More specifically, examples of the complex catalyst containing a transition metal of Group 6 of the periodic table include tungsten hexachloride, tungsten tetrachloride, (ethylimide)(tetrachloride)(diethyl ether) tungsten, (ethylimide)(tetrachloride)(tetrahydrofuran) tungsten, (phenylimide)(tetrachloride)(diethyl ether) tungsten, (phenylimide)(tetrachloride)(tetrahydrofuran) tungsten, (2,6-dimethylphenylimide)(tetrachloride)(diethyl ether) tungsten, bis[3,3'-di(tert-butyl)imide)(tetrachloride)(tetrahydrofuran) tungsten, [3,3'-di(tert-butyl)-5,5',6,6'-tetramethyl-2,2'-biphenyloxy] tungsten oxide (VI), [3,3'-di(tert-butyl)-5,5',6,6'-tetramethyl-2,2'-biphenyloxy] tungsten dichloride (VI) oxide, etc.

[0091] When using the above-mentioned complex catalyst containing a transition metal of Group 6 of the periodic table as a metathesis catalyst, in order to improve the catalyst activity, it is preferred to use the above-mentioned complex catalyst containing a transition metal of Group 6 of the periodic table in combination with a catalyst other than the complex catalyst as a co-catalyst.

[0092] As other catalysts, known organometallic compounds can be cited. As the organometallic compound, an organometallic compound of any one of Groups 1, 2, 12, 13 and 14 of the periodic table having a hydrocarbon group having 1 to 20 carbon atoms is preferred, and an organolithium compound, an organomagnesium compound, an organozinc compound, an organoaluminum compound, and an organotin compound are more preferred, and an organolithium compound and an organoaluminum compound are particularly preferred.

[0093] Examples of the organic lithium compound include n-butyl lithium, methyl lithium, phenyl lithium, neopentyl lithium, tert-butylphenyl (Neophyl) lithium, and the like.

[0094] Examples of the organic magnesium compound include butylethylmagnesium, butyloctylmagnesium, dihexylmagnesium, ethylmagnesium chloride, n-butylmagnesium chloride, allylmagnesium bromide, neopentylmagnesium chloride, and tert-butylphenylmagnesium chloride.

[0095] Examples of the organic zinc compound include dimethyl zinc, diethyl zinc and diphenyl zinc.

[0096] Examples of the organoaluminum compound include trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum chloride, diethylethoxyaluminum, ethylaluminum dichloride, and ethyldiethoxyaluminum.

[0097] Examples of the organic tin compound include tetramethyltin, tetra(n-butyl)tin, and tetraphenyltin.

[0098] The other catalysts may be used alone or in combination of two or more.

[0099] In addition, examples of the complex catalyst containing a transition metal of Group 6 of the periodic table include compounds represented by the following general formula (5).

[0100] [Chemical formula 7]

[0101]

[0102] In the general formula (5), M represents a molybdenum atom or a tungsten atom.

[0103] R 6 , R 7 Each independently represents: a hydrogen atom; an alkyl group having 1 to 12 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl; a cycloalkyl group having 3 to 20 carbon atoms, such as cyclopropyl, cyclopentyl, cyclohexyl; or an aryl group having 6 to 20 carbon atoms which may have a substituent. Examples of the aryl group of the aryl group which may have a substituent include phenyl, 1-naphthyl, 2-naphthyl, and the like. In addition, substituents for the aryl group include: alkyl groups having 1 to 12 carbon atoms, such as methyl and ethyl groups; halogen atoms, such as fluorine, chlorine and bromine atoms; alkoxy groups having 1 to 12 carbon atoms, such as methoxy, ethoxy and isopropoxy groups; halogenated alkyl groups having 1 to 12 carbon atoms, such as trifluoromethyl groups; halogenated alkoxy groups having 1 to 12 carbon atoms, such as trifluoromethoxy groups; and aryl groups having 6 to 12 carbon atoms which may have substituents, such as phenyl, 4-methylphenyl, 2,4-dimethylphenyl, 2-chlorophenyl and 3-methoxyphenyl groups.

[0104] L 1represents a nitrogen atom or an oxygen atom which may have a substituent selected from an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms which may have a substituent, and a cycloalkyl group having 3 to 20 carbon atoms which may have a substituent.

[0105] L 1 The alkyl group having 1 to 12 carbon atoms contained in the nitrogen atom or oxygen atom may be linear, branched or cyclic. Specific examples thereof include methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl and hexyl.

[0106] As L 1 The cycloalkyl group having 3 to 20 carbon atoms contained in the nitrogen atom or oxygen atom of the cycloalkyl group includes cyclopropyl, cyclopentyl, cyclohexyl, cyclooctyl and adamantyl groups.

[0107] In addition, as L 1 The aryl group having 6 to 12 carbon atoms contained in the nitrogen atom or oxygen atom of the aryl group includes phenyl, 1-naphthyl, 2-naphthyl and the like.

[0108] L 1 The substituents that may be possessed by the cycloalkyl group having 3 to 20 carbon atoms and the aryl group having 6 to 12 carbon atoms possessed by the nitrogen atom or oxygen atom of the cycloalkyl group having 3 to 20 carbon atoms and the aryl group having 6 to 12 carbon atoms are not particularly limited. Examples thereof include: alkyl groups having 1 to 12 carbon atoms such as methyl and ethyl groups; halogen atoms such as fluorine, chlorine, and bromine atoms; alkoxy groups having 1 to 12 carbon atoms such as methoxy, ethoxy, and isopropoxy groups; halogenated alkyl groups having 1 to 12 carbon atoms such as trifluoromethyl; halogenated alkoxy groups having 1 to 12 carbon atoms such as trifluoromethoxy; aryl groups having 6 to 12 carbon atoms that may be possessed by substituents such as phenyl, 4-methylphenyl, 2,4-dimethylphenyl, 2-chlorophenyl, and 3-methoxyphenyl; amino groups; monosubstituted amino groups such as methylamino; disubstituted amino groups such as dimethylamino; imino groups, and the like.

[0109] L 2 , L 3 It is a conjugated heterocyclic group having 5 to 15 ring members and having at least one nitrogen atom, which may have a substituent, or a group consisting of OR 8 The alkoxy group, R 8 It is a group selected from an alkyl group having 1 to 12 carbon atoms which may have a substituent and an aryl group having 6 to 30 carbon atoms which may have a substituent.

[0110] As L 2 , L 3 The conjugated heterocyclic group includes pyrrolyl, imidazolyl, pyrazolyl, Five-membered conjugated heterocyclic groups such as oxazolyl and thiazolyl; six-membered conjugated heterocyclic groups such as pyridyl, pyridazinyl, pyrimidinyl, pyrazinyl and triazinyl; condensed-ring conjugated heterocyclic groups such as quinazolinyl, phthalazinyl and pyrrolopyridinyl, etc.

[0111] The substituents that the above-mentioned conjugated heterocyclic group may have are not particularly limited. Examples thereof include: alkyl groups having 1 to 12 carbon atoms, such as methyl and ethyl groups; halogen atoms, such as fluorine atoms, chlorine atoms, and bromine atoms; alkoxy groups having 1 to 12 carbon atoms, such as methoxy groups, ethoxy groups, and isopropoxy groups; halogenated alkyl groups having 1 to 12 carbon atoms, such as trifluoromethyl groups; halogenated alkoxy groups having 1 to 12 carbon atoms, such as trifluoromethoxy groups; aryl groups having 6 to 12 carbon atoms, such as phenyl groups, 4-methylphenyl groups, 2,4-dimethylphenyl groups, 2-chlorophenyl groups, and 3-methoxyphenyl groups, which may have substituents; amino groups; monosubstituted amino groups, such as methylamino groups; disubstituted amino groups, such as dimethylamino groups; imino groups, and the like.

[0112] As the above R 8 The alkyl group having 1 to 12 carbon atoms which may have a substituent includes methyl, ethyl, propyl, isopropyl, butyl, tert-butyl, pentyl and the like. 2 , L 3 All by OR 8 In the case of R 8 The alkyl groups may be bonded to each other.

[0113] The above R 8 The substituents that the alkyl group having 1 to 12 carbon atoms may have are not particularly limited. Examples thereof include: halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms; alkoxy groups having 1 to 12 carbon atoms such as methoxy, ethoxy, and isopropoxy; halogenated alkyl groups having 1 to 12 carbon atoms such as trifluoromethyl; halogenated alkoxy groups having 1 to 12 carbon atoms such as trifluoromethoxy; aryl groups having 6 to 12 carbon atoms that may have substituents such as phenyl, 4-methylphenyl, 2,4-dimethylphenyl, 2-chlorophenyl, and 3-methoxyphenyl; amino groups; monosubstituted amino groups such as methylamino; disubstituted amino groups such as dimethylamino; imino groups, and the like.

[0114] As the above R 8Specific examples include 1,1,1,3,3,3-hexafluoro-2-propoxy, 2-methyl-2-propoxy, 1,1,1-trifluoro-2-methyl-2-propoxy, 1,1,1-trifluoro-2-trifluoromethyl-2-propoxy, and 2-trifluoromethyl-2-phenyl-1,1,1-trifluoroethoxy. Specific examples of the aryl group having 6 to 30 carbon atoms which may have a substituent include 2,6-bis(2,4,6-trimethylphenyl)phenoxy, 2,6-bis(2,4,6-triisopropylphenyl)phenoxy, 2,4,6-trimethylphenoxy, and 2,3,5,6-tetraphenolphenoxy. 8 When the alkyl groups are bonded to each other, 3,3'-di(tert-butyl)-5,5',6,6'-tetramethyl-2,2'-biphenyloxy can be mentioned.

[0115] L 4 It is a neutral conjugated heterocyclic ligand having at least one nitrogen atom, that is, a conjugated heterocyclic group having 12 to 24 ring members. Specific examples of neutral conjugated heterocyclic ligands having nitrogen atoms include pyridine, 2-methylpyridine, 2,4-lutidine, 2,6-lutidine, 2,2'-bipyridine, 5,5'-dimethyl-2,2'-bipyridine, 4,4'-dimethyl-2,2'-bipyridine, 4,4'-dibromo-2,2'-bipyridine, 2,2'-biquinoline, 1,10-phenanthroline, and terpyridine. 4 In the case of multiple nitrogen atoms, bidentate rather than monodentate ligands can be formed.

[0116] In addition, the above L 4 The conjugated heterocyclic group may have a substituent. Examples of the substituent include the same as L 2 The conjugated heterocyclic group may have a substituent which is the same as the substituent exemplified above.

[0117] Specific examples of the compound represented by the general formula (5) include bis(1,1,1,3,3,3-hexafluoro-2-propoxy)tert-butylphenylene tungsten(VI)(2,6-dimethylphenylimide), bis(1,1,1,3,3,3-hexafluoro-2-propoxy)tert-butylphenylene molybdenum(VI)(2,6-dimethylphenylimide), bis(1,1,1,3,3,3-hexafluoro-2-propoxy)tert-butylphenylene tungsten(VI)(2,6-diisopropylphenylimide), (2,3,5,6-tetraphenylphenoxy)2,6-dimethylphenylimide tungsten(VI)(2,5-dimethylpyrrolyl)(tert-butylphenylene), [3,3'-di(tert-butyl)-5,5',6,6'-tetramethyl- 2,2'-biphenyloxy] tert-butylphenylene molybdenum (VI) (2,6-dimethylphenylimide), (2-trifluoromethyl-2-phenyl-1,1,1-trifluoroethoxy) 2,6-dimethylphenylimide tungsten (VI) (2,5-dimethylpyrrolyl) (tert-butylphenylene) (1,10-phenanthroline), (2-trifluoromethyl-2-phenyl-1,1,1-trifluoroethoxy) 2,6-dimethylphenylimide tungsten (VI) (2,5-dimethylpyrrolyl) (tert-butylphenylene) (2,2'-bipyridine), (2-trifluoromethyl-2-phenyl-1,1,1-trifluoroethoxy) phenylimide tungsten (VI) (2,5-dimethylpyrrolyl) (tert-butylphenylene) (pyridine), etc., but are not limited to these.

[0118] In addition, as the ruthenium carbene complex, a complex compound represented by the following general formula (6) or (7) is preferred.

[0119] [Chemical formula 8]

[0120]

[0121] In the above general formula (6) and general formula (7), R 9 , R 10 Each is independently: a hydrogen atom; a halogen atom; or a hydrocarbon group having 1 to 20 carbon atoms which may contain a halogen atom, an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom or a silicon atom. 1 , X 2 are each independently any anionic ligand, L 5 , L 6 Each is independently a heteroatom-containing carbene compound or a neutral electron-donating compound. 9 , R 10 , X 1 , X 2 , L 5 and L 6The respective combinations are arbitrary, and can be bonded to each other to form a multidentate chelate ligand. In addition, heteroatom refers to the atom of the 15th and 16th families of the periodic table of elements, specifically, N, O, P, S, As, Se atoms etc. can be enumerated. Among these, from the viewpoint that stable carbene compounds can be obtained, preferably N, O, P, S atoms etc., particularly preferably N atom.

[0122] As the heteroatom-containing carbene compound, it is preferred that heteroatoms are bonded adjacently on both sides of the carbene carbon, and more preferably a heterocycle comprising the carbene carbon atom and the heteroatoms on both sides thereof is further formed. In addition, it is preferred that a bulky substituent is present on the heteroatom adjacent to the carbene carbon. As such a heteroatom-containing carbene compound, a compound represented by the following general formula (8) or general formula (9) is preferred.

[0123] [Chemical formula 9]

[0124]

[0125] In the above general formula (8) and general formula (9), R 13 ~R 16 Each is independently: a hydrogen atom; a halogen atom; or a hydrocarbon group having 1 to 20 carbon atoms which may contain a halogen atom, an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom or a silicon atom. 13 ~R 16 The respective combinations are arbitrary, and they can be bonded to each other to form a multidentate chelating ligand.

[0126] In the above general formula (6) and general formula (7), the anionic ligand X 1 , X 2 It is a ligand that has a negative charge when separated from the central metal, and examples thereof include halogen atoms such as F, Cl, Br, and I; diketonate, substituted cyclopentadienyl, alkoxy, aryloxy, and carboxyl groups, etc. Among these, halogen atoms are preferred, and chlorine atoms are more preferred.

[0127] In addition, the neutral electron-donating compound may be any compound as long as it is a ligand with a neutral charge when separated from the central metal, and examples thereof include carbonyl, amines, pyridines, ethers, nitriles, esters, phosphines, thioethers, aromatic compounds, olefins, isocyanides, thiocyanates, etc. Among these, phosphines, ethers and pyridines are preferred, and trialkylphosphines are more preferred.

[0128] Specific examples of the complex compounds represented by the general formula (6) and the general formula (7) include benzal (1,3-di-mesitylene imidazolidin-2-ylidene) (tricyclohexylphosphine) ruthenium dichloride, (1,3-di-mesitylene imidazolidin-2-ylidene) (3-methyl-2-butene-1-ylidene) (tricyclopentylphosphine) ruthenium dichloride, benzal (1,3-di-mesitylene-2,3-dihydrobenzimidazol-2-ylidene) (tricyclohexylphosphine) ruthenium dichloride, tricyclohexylphosphine [1,3-bis (2,4,6-trimethylphenyl) -4,5-dihydroimidazolidin-2-ylidene] [3-methyl-2-butenyl] dichloride, etc. 5 , L 6 Ruthenium complex compounds containing heteroatom carbene compounds and neutral electron-donating compounds; benzylidenebis(tricyclohexylphosphine)ruthenium dichloride, dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium, (3-methyl-2-butene-1-ylidene)bis(tricyclopentylphosphine)ruthenium dichloride, etc. 5 , L 6 Ruthenium compounds are all neutral electron-donating compounds; benzylidenebis(1,3-dicyclohexylimidazolidin-2-ylidene)ruthenium dichloride, benzylidenebis(1,3-diisopropyl-4-imidazolin-2-ylidene)ruthenium dichloride, etc. 5 , L 6 All of them are ruthenium complex compounds containing heteroatom carbene compounds. Among these, L 5 , L 6 They are ruthenium complex compounds containing heteroatom carbene compounds and neutral electron-donating compounds.

[0129] Specific examples of the compounds represented by the general formula (8) and the general formula (9) include 1,3-dimesityl imidazolidin-2-ylidene, 1,3-dimesityl-4-imidazolin-2-ylidene, 1,3-di(1-phenylethyl)-4-imidazolin-2-ylidene, 1,3-dimesityl-2,3-dihydrobenzimidazol-2-ylidene, etc. Furthermore, in addition to the compounds represented by the general formula (8) and the general formula (9), heteroatom-containing carbene complex compounds such as 1,3,4-triphenyl-2,3,4,5-tetrahydro-1H-1,2,4-triazole-5-ylidene and 1,3,4-triphenyl-4,5-dihydro-1H-1,2,4-triazole-5-ylidene can also be used.

[0130] The metathesis catalyst can be used alone or in combination of two or more.

[0131] In the manufacturing method of the present invention, the amount of the metathesis catalyst is preferably 0.001 to 10 parts by weight, more preferably 0.002 to 5 parts by weight, and further preferably 0.005 to 1 part by weight relative to 100 parts by weight of the total of the polymer represented by the general formula (2) (the first ethylenically unsaturated polymer) and the polymer represented by the general formula (3) (the second ethylenically unsaturated polymer). By making the amount of the metathesis catalyst within the above range, the randomness and weight average molecular weight of the structural units constituting the copolymer represented by the general formula (1) obtained by the cross-metathesis reaction can be appropriately controlled.

[0132] In addition, in the production method of the present invention, it is preferred to carry out the cross-metathesis reaction in a state where the polymer represented by the general formula (2) (the first ethylenically unsaturated polymer), the polymer represented by the general formula (3) (the second ethylenically unsaturated polymer) and the metathesis catalyst are dispersed or dissolved in a solvent, or the cross-metathesis reaction can be carried out under stirring.

[0133] The solvent is not particularly limited as long as it can disperse or dissolve the polymer represented by the general formula (2) (first ethylenically unsaturated polymer), the polymer represented by the general formula (3) (second ethylenically unsaturated polymer) and the metathesis catalyst. Examples thereof include aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; aliphatic hydrocarbons such as hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclohexane, cyclopentane, and methylcyclohexane; halogenated alkanes such as dichloromethane and chloroform; and aromatic halides such as chlorobenzene and dichlorobenzene.

[0134] When the cross metathesis reaction is carried out in a state where the polymer represented by the above general formula (2) (the first ethylenically unsaturated polymer), the polymer represented by the above general formula (3) (the second ethylenically unsaturated polymer) and the metathesis catalyst are dispersed or dissolved in a solvent, the reaction temperature is preferably 0 to 100°C, more preferably 10 to 80°C, more preferably 20 to 70°C, and the reaction time is preferably 1 minute to 100 hours, more preferably 10 minutes to 24 hours.

[0135] Then, a reaction terminator is added to the reaction system as needed to terminate the cross-metathesis reaction, thereby obtaining the copolymer represented by the general formula (1) in the form of a polymer solution dispersed or dissolved in a solvent. The copolymer represented by the general formula (1) can be isolated from the polymer solution thus obtained by conventional methods such as filtration, distillation, extraction, extractive distillation, and adsorption.

[0136] <Rubber composition>

[0137] The rubber composition of the present invention is prepared by blending a filler into the copolymer represented by the general formula (1) of the present invention.

[0138] The filler may be either an organic filler or an inorganic filler, but is preferably a carbon material or silica.

[0139] By using a carbon material as a filler, the obtained rubber cross-linked product can be made excellent not only in fracture resistance, wet grip and low heat build-up properties but also in wear resistance, and thus can be suitably used in heavy-load tire applications, for example.

[0140] As the carbon material, carbon black is preferred, and examples of carbon black include furnace black, acetylene black, thermal black, channel black, graphite, etc. Among these, furnace black is preferred, and specific examples thereof include SAF, ISAF, ISAF-HS, ISAF-LS, IISAF-HS, HAF, HAF-HS, HAF-LS, FEF, etc. These carbon blacks can be used alone or in combination of two or more.

[0141] The nitrogen adsorption specific surface area (N2SA) of carbon black is preferably 5 to 200 m 2 / g, more preferably 70 to 120 m 2 / g, and the adsorption amount of dibutyl phthalate (DBP) is preferably 5 to 300 ml / 100 g, more preferably 80 to 160 ml / 100 g.

[0142] In addition, as silica, for example, dry-process silica, wet-process silica, colloidal silica, and precipitated silica disclosed in Japanese Patent Publication No. 62-62838 can be cited. Among these, wet-process silica containing hydrous silicic acid as a main component is preferred. In addition, a carbon-silica dual-phase filler in which silica is supported on the surface of carbon black can also be used. These silicas can be used alone or in combination of two or more.

[0143] The nitrogen adsorption specific surface area of ​​silicon dioxide (measured by the BET method according to ASTM D3037-81) is preferably 50 to 400 m 2 / g, more preferably 100 to 220 m 2 / g. In addition, the pH of silica is preferably less than pH 7, and more preferably pH 5 to 6.9.

[0144] When silica is used as a filler, it is preferred to further add a silane coupling agent in order to further improve the affinity between the copolymer represented by the general formula (1) and silica. As the silane coupling agent, for example, vinyl triethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl trimethoxysilane, bis(3-(triethoxysilyl)propyl)tetrasulfide, bis(3-(triethoxysilyl)propyl)disulfide, γ-trimethoxysilylpropyldimethylthiocarbamoyl tetrasulfide, γ-trimethoxysilylpropylbenzothiazolyl tetrasulfide and other tetrasulfides described in Japanese Patent Laid-Open No. 6-248116 can be cited. Tetrasulfides are particularly preferred. These silane coupling agents can be used alone or in combination of two or more. The amount of the silane coupling agent blended is preferably 0.1 to 30 parts by weight, more preferably 1 to 15 parts by weight, based on 100 parts by weight of silica.

[0145] The content of the filler in the rubber composition of the present invention is preferably 10 to 150 parts by weight, more preferably 20 to 100 parts by weight, and even more preferably 40 to 85 parts by weight, relative to 100 parts by weight of the rubber component containing the copolymer represented by the general formula (1). In addition, when a carbon material is used as the filler, the content of the carbon material is particularly preferably 40 to 60 parts by weight relative to 100 parts by weight of the rubber component containing the copolymer represented by the general formula (1). In addition, when silica is used as the filler, the content of silica is particularly preferably 60 to 85 parts by weight relative to 100 parts by weight of the rubber component containing the copolymer represented by the general formula (1).

[0146] In addition, the rubber composition of the present invention may also contain a rubber other than the copolymer represented by the above general formula (1) as a rubber component. In the present invention, the rubber component refers to the copolymer represented by the above general formula (1) and a rubber other than the copolymer represented by the above general formula (1). Examples of rubbers other than the copolymer represented by the above general formula (1) include natural rubber (NR), polyisoprene rubber (IR), emulsion-polymerized SBR (styrene-butadiene copolymer rubber), solution-polymerized random SBR (5 to 50% by weight of bonded styrene and 10 to 80% by weight of 1,2-bond content of the butadiene part), high trans SBR (trans bond content of the butadiene part is 70 to 95%), low cis BR (polybutadiene rubber), high cis BR, high trans BR (trans bond content of the butadiene part is 20 to 30%). The amount is 70-95%), ethylene-propylene-diene rubber (EPDM), styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, emulsion polymerization styrene-acrylonitrile-butadiene copolymer rubber, acrylonitrile-butadiene copolymer rubber, high vinyl SBR-low vinyl SBR block copolymer rubber, polyisoprene-SBR block copolymer rubber, polystyrene-polybutadiene-polystyrene block copolymer, acrylic rubber, epichlorohydrin rubber, fluororubber, silicone rubber, ethylene-propylene rubber, polyurethane rubber, etc. NR, BR, IR, EPDM, SBR are particularly preferably used, and solution polymerization random SBR is particularly preferably used. These rubbers can be used alone or in combination of two or more.

[0147] In addition to the above-mentioned ingredients, the rubber composition of the present invention can also be formulated with required amounts of crosslinking agents, crosslinking accelerators, crosslinking activators, fillers other than inorganic materials, antioxidants, activators, process oils, plasticizers, lubricants and other compounding agents according to conventional methods.

[0148] As crosslinking agents, there can be mentioned: sulfur such as powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, and highly dispersible sulfur; sulfur halides such as sulfur monochloride and sulfur dichloride; organic peroxides such as diisopropylbenzene peroxide and di-tert-butyl peroxide; quinone dioximes such as p-quinone dioxime and p,p'-dibenzoylquinone dioxime; organic polyamine compounds such as triethylenetetramine, hexamethylenediamine carbamate, and 4,4'-methylenebis(o-chloroaniline); alkylphenol-formaldehyde resins having methylol groups, etc. Among these, sulfur is preferred, and powdered sulfur is more preferred. These crosslinking agents can be used alone or in combination of two or more. The amount of the crosslinking agent is preferably 0.1 to 15 parts by weight, and more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition.

[0149] Examples of the crosslinking accelerator include: sulfonamide-based crosslinking accelerators such as N-cyclohexyl-2-benzothiazolesulfenamide, N-(tert-butyl)-2-benzothiazolesulfenamide, N-oxyethylene-2-benzothiazolesulfenamide, N-oxyethylene-2-benzothiazolesulfenamide, and N,N'-diisopropyl-2-benzothiazolesulfenamide; guanidine-based crosslinking accelerators such as 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, and 1-o-tolylbiguanide; Thiourea crosslinking accelerators such as diethylthiourea; thiazole crosslinking accelerators such as 2-mercaptobenzothiazole, dibenzothiazole disulfide, and 2-mercaptobenzothiazole zinc salt; thiuram crosslinking accelerators such as tetramethylthiuram monosulfide and tetramethylthiuram disulfide; dithiocarbamic acid crosslinking accelerators such as sodium dimethyldithiocarbamate and zinc diethyldithiocarbamate; xanthogenic acid crosslinking accelerators such as sodium isopropyl xanthogenate, zinc isopropyl xanthogenate, and zinc butyl xanthogen. It is particularly preferred to include a sulfonamide crosslinking accelerator, and it is particularly preferred to include N-(tert-butyl)-2-benzothiazole sulfonamide. These crosslinking accelerators can be used alone or in combination of two or more. The amount of the crosslinking accelerator is preferably 0.1 to 15 parts by weight, and more preferably 0.5 to 5 parts by weight relative to 100 parts by weight of the rubber component in the rubber composition.

[0150] As the crosslinking activator, for example, higher fatty acids such as stearic acid, zinc oxide, etc. can be used. The amount of the crosslinking activator can be appropriately selected, and the amount of the higher fatty acid is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition, and the amount of zinc oxide is preferably 0.05 to 10 parts by weight, more preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition.

[0151] As the process oil, mineral oil and synthetic oil can be used. Mineral oil can generally be aromatic oil, naphthenic oil, paraffin oil, etc. As other compounding agents, there can be mentioned: activators such as diethylene glycol, polyethylene glycol, silicone oil; fillers other than inorganic materials such as calcium carbonate, talc, clay; tackifiers such as petroleum resin, coumarone resin; wax, etc.

[0152] The rubber composition of the present invention can be obtained by kneading the components according to a conventional method. For example, the rubber composition can be obtained by kneading compounding agents other than the crosslinking agent and the crosslinking accelerator with a rubber component such as the copolymer represented by the above general formula (1), and then mixing the crosslinking agent and the crosslinking accelerator into the kneaded product. The kneading temperature of compounding agents other than the crosslinking agent and the crosslinking accelerator with the rubber component such as the copolymer represented by the above general formula (1) is preferably 20 to 200°C, more preferably 30 to 180°C, and the kneading time is preferably 30 seconds to 30 minutes. The mixing of the crosslinking agent and the crosslinking accelerator is usually carried out below 100°C, preferably below 80°C.

[0153] <Rubber cross-linked products>

[0154] The cross-linked rubber of the present invention is obtained by cross-linking the rubber composition of the present invention.

[0155] The rubber cross-linked product of the present invention can be manufactured as follows: using the rubber composition of the present invention, it is molded by a molding machine corresponding to the desired shape, such as an extruder, an injection molding machine, a compressor, a roller, etc., and a cross-linking reaction is carried out by heating to fix the shape to form a cross-linked product. In this case, cross-linking can be carried out after pre-molding, or it can be cross-linked while molding. The molding temperature is usually 10 to 200°C, preferably 25 to 120°C. The cross-linking temperature is usually 100 to 200°C, preferably 130 to 190°C, and the cross-linking time is usually 1 minute to 24 hours, preferably 2 minutes to 12 hours, and particularly preferably 3 minutes to 6 hours.

[0156] Furthermore, depending on the shape and size of the cross-linked rubber, even if the surface is cross-linked, the interior may not be sufficiently cross-linked. Therefore, further heating may be performed to perform secondary cross-linking.

[0157] As the heating method, any method generally used for crosslinking of rubber, such as press heating, steam heating, oven heating, hot air heating, etc., may be appropriately selected.

[0158] The rubber cross-linked product of the present invention thus obtained is obtained by using the rubber composition of the present invention, and therefore has excellent damage resistance, wet grip and low heat generation. Therefore, the rubber cross-linked product of the present invention can be used for various purposes such as: materials for various parts of tires such as tread caps, tread bases, carcasses, sidewalls, and bead parts in tires by effectively utilizing its excellent properties; materials for hoses, belts, pads, shockproof rubbers, and other various industrial products; impact resistance improvers for resins; resin film buffers; soles; rubber shoes; golf balls; toys, etc. In particular, the rubber cross-linked product of the present invention is suitable for tire materials because of its excellent damage resistance, wet grip and low heat generation. In addition, when the rubber cross-linked product of the present invention contains a carbon material as a filler constituting the rubber composition, it has excellent wear resistance in addition to damage resistance, wet grip and low heat generation, and can be used for heavy-load tire materials.

[0159] Example

[0160] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples. In addition, "parts" are based on mass unless otherwise specified.

[0161] The test methods performed in the present examples and comparative examples are as follows.

[0162] <Molecular weight of each polymer>

[0163] The weight average molecular weight (Mw) and number average molecular weight (Mn) of each polymer were measured using a gel permeation chromatography (GPC) system (product name "HLC-8220", manufactured by Tosoh Corporation) by connecting two H-type columns (product name "HZ-M", manufactured by Tosoh Corporation) in series, using tetrahydrofuran as a solvent, and measuring at a column temperature of 40° C., and the values ​​were obtained as polystyrene conversion values. In addition, a differential refractometer (product name "RI-8320", manufactured by Tosoh Corporation) was used as a detector.

[0164] <Ratio of the structural unit derived from the norbornene compound and the structural unit derived from the conjugated diene in the cross-metathesis copolymer>

[0165] The ratio of the structural unit derived from the norbornene compound to the structural unit derived from the conjugated diene in the cross-metathesis copolymer is determined by 1 H-NMR and 13 C-NMR was used to determine the result.

[0166] <Glass transition temperature (Tg) of each polymer>

[0167] The glass transition temperature (Tg) of each polymer was determined by measuring the temperature in the range of -150 to 100°C at a temperature increase rate of 10°C / min using a differential scanning calorimeter (product name "X-DSC7000", manufactured by Hitachi High-Technologies Corporation).

[0168] <Tensile test>

[0169] A sheet-shaped cross-linked rubber product is prepared by press-crosslinking a cross-linkable rubber composition as a sample, and the obtained sheet-shaped cross-linked rubber product is punched into a dumbbell-shaped No. 6 shape specified in JIS K6251:2010 in a direction parallel to the grain direction, thereby obtaining a dumbbell-shaped test piece. Then, the obtained dumbbell-shaped test piece is subjected to a tensile test at 23°C and 500 mm / min using a tensile tester (product name "TENSOMETER 10K", manufactured by ALPHATECHNOLOGIES) as a testing machine, and the tensile strength and elongation are measured in accordance with JIS K6251:2010. The higher the tensile strength, the better the fracture resistance.

[0170] <Resilience test>

[0171] The cross-linkable rubber composition as a sample was pressurized and molded using a metal mold to obtain a cylindrical cross-linked rubber product with a diameter of 29 mm and a thickness of 12.5 mm. Then, the obtained cylindrical cross-linked rubber product was adjusted to 0°C or 60°C using a thermostatic bath, and immediately after being taken out, the rebound rate was measured using a Lupke type rebound resilience tester (manufactured by Kobunsu Keiki Co., Ltd.) as a tester in accordance with JIS K6255:1996 at 23°C and a holding force of 29 to 39N. The lower the rebound rate at 0°C, the better the wet grip. The higher the rebound rate at 60°C, the better the low heat generation.

[0172] <Wet Grip>

[0173] The test piece was prepared by press-crosslinking the crosslinkable rubber composition as a sample at 160°C for 20 minutes, and the tanδ at 0°C was measured using a dynamic viscoelasticity measuring device (product name "ARES", manufactured by Rheometrics Inc.) under the conditions of 0.5% dynamic strain and 10 Hz. Then, for Examples 1 to 4, the measurement results were calculated by an index with the measurement value of Comparative Example 1 as 100, and for Examples 5 to 8, the measurement results were calculated by an index with the measurement value of Comparative Example 3 as 100. The larger the index, the better the wet grip.

[0174] <Low heat generation>

[0175] The test piece was prepared by press-crosslinking the crosslinkable rubber composition as a sample at 160°C for 20 minutes, and the tan δ at 60°C was measured using a dynamic viscoelasticity measuring device (product name "ARES", manufactured by Rheometrics Inc.) under the conditions of dynamic strain 2.0% and 10 Hz. Then, for Examples 1 to 4, the measurement results were calculated by an index with the measurement value of Comparative Example 1 as 100, and for Examples 5 to 8, the measurement results were calculated by an index with the measurement value of Comparative Example 3 as 100. The smaller the index, the better the low heat build-up property.

[0176] <DIN abrasion test>

[0177] The cross-linkable rubber composition as a sample was pressurized and molded using a metal mold to obtain a cylindrical cross-linked rubber product with a diameter of 16 mm and a thickness of 6 mm. Then, the obtained cylindrical cross-linked rubber product was tested for relative wear volume using a DIN abrasion tester (product name "AB-6110", manufactured by Ueshima Seisakusho Co., Ltd.) as a testing machine in accordance with JIS K6264-2:2005, under the conditions of test method A, applied force of 10 N, friction distance of 40 m, 23° C., and reference test piece D1. In addition, the DIN abrasion test was performed on Examples 1 to 4 and Comparative Examples 1 and 2. The smaller the relative wear volume, the better the wear resistance.

[0178] <Polymerization Example 1>

[0179] In a nitrogen environment, 100 parts of dicyclopentadiene (DCPD) as a norbornene compound, 567 parts of cyclohexane and 0.070 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.025 parts of dichloro[1,3-bis(2,4,6-trimethylphenyl)-2-imidazolidinyl](benzylidene)(tricyclohexylphosphine)ruthenium(II) dissolved in 10 parts of toluene were added, and the polymerization reaction was carried out at room temperature for 30 minutes. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization. Then, the obtained polymer solution was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 100 parts of a ring-opening copolymer (2-A). The obtained ring-opening copolymer (2-A) had a number average molecular weight (Mn) of 125,000, a weight average molecular weight (Mw) of 268,000, a glass transition temperature (Tg) of 151°C, and an unsaturated carbon content of 40.0 mol%. 1 It can be determined by H-NMR.

[0180] <Polymerization Example 2>

[0181] The polymerization was carried out in the same manner as in Polymerization Example 1 except that 50 parts of dicyclopentadiene (DCPD) and 50 parts of 2-norbornene (NB) were used as norbornene compounds, thereby obtaining 100 parts of a ring-opening copolymer (2-B). The obtained ring-opening copolymer (2-B) had a number average molecular weight (Mn) of 199,000, a weight average molecular weight (Mw) of 439,000, a ratio of dicyclopentadiene structural unit / norbornene structural unit of 50 / 50 (weight ratio), a glass transition temperature (Tg) of 83°C, and an unsaturated bond carbon content of 33.3 mol%.

[0182] <Polymerization Example 3>

[0183] As the norbornene compound, 100 parts of tetracyclo[6.2.1.1 3,6 .0 2,7 ] Dodec-4-ene (tetracyclododecene, TCD), except for this, the same polymerization example 1 was carried out to obtain 100 parts of a ring-opening copolymer (2-C). The obtained ring-opening copolymer (2-C) had a number average molecular weight (Mn) of 129,000, a weight average molecular weight (Mw) of 277,000, a glass transition temperature (Tg) of 200°C, and an unsaturated bond carbon content of 16.7 mol%.

[0184] <Polymerization Example 4>

[0185] 100 parts of a ring-opening copolymer (2-D) was obtained in the same manner as in Polymerization Example 1 except that 100 parts of 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene (MTHF) was used as the norbornene compound. The obtained ring-opening copolymer (2-D) had a number average molecular weight (Mn) of 128,000, a weight average molecular weight (Mw) of 275,000, a glass transition temperature (Tg) of 201° C., and an unsaturated bond carbon content of 14.3 mol %.

[0186] <Polymerization Example 5>

[0187] In a nitrogen environment, 599 parts of 2-norbornene (NB) as a norbornene compound, 703 parts of cyclopentene (CPE) as a monocyclic cyclic olefin, 2411 parts of toluene and 1.05 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.154 parts of dichloro(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium (II) dissolved in 35 parts of toluene was added, and a polymerization reaction was carried out at room temperature for 3 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization. Then, the obtained polymer solution was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), and the precipitated polymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 833 parts of a ring-opening copolymer (1'-E). The obtained ring-opening copolymer (1'-E) had a number average molecular weight (Mn) of 127,000, a weight average molecular weight (Mw) of 234,000, a 2-norbornene structural unit / cyclopentene structural unit ratio of 62 / 38 (weight ratio), a glass transition temperature (Tg) of -23°C, and an unsaturated bond carbon content of 33.8 mol%.

[0188] <Polymerization Example 6>

[0189] Under nitrogen environment, 45 parts of dicyclopentadiene (DCPD) as a norbornene compound, 55 parts of cyclopentene (CPE) as a monocyclic cyclic olefin, 233 parts of toluene and 0.08 parts of 1-hexene were added to a glass reaction container with a stirrer. Next, 0.011 parts of dichloro(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium (II) dissolved in 6 parts of toluene were added, and the polymerization reaction was carried out at room temperature for 3 hours. After the polymerization reaction, an excess of vinyl ethyl ether was added to terminate the polymerization. Then, the obtained polymer solution was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), the precipitated polymer was recovered, washed with methanol, and vacuum dried at 50°C for 3 days to obtain 833 parts of a ring-opening copolymer (1'-F). The number average molecular weight (Mn) of the obtained ring-opening copolymer (1'-F) was 119,000, the weight average molecular weight (Mw) was 238,000, the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) (Mw / Mn) was 2.00, the ratio of the dicyclopentadiene structural unit / cyclopentene structural unit was 55 / 45 (weight ratio), the glass transition temperature (Tg) was -25°C, and the unsaturated bond carbon content was 40.0 mol%.

[0190] <Polymerization Example 7>

[0191] 2.0×10 -5 mole of cobalt octenate, 162.3 g of 1,3-butadiene, 900 ml of benzene and 0.18 g of 1,5-cyclooctadiene were added, followed by 8.0 × 10 -4 Then, 10 ml of 2.7×10 -3 1000ml of diethylaluminum chloride in benzene was polymerized at 50°C for 2 hours. 20ml of methanol was added to terminate the polymerization reaction, and the obtained polymer solution was injected into 5000ml of methanol, and the precipitated polymer was filtered and dried. Furthermore, the obtained polymer was dissolved in 1500ml of toluene, and the polymer solution was injected into 5000ml of methanol, and the precipitated polymer was filtered and dried to obtain polybutadiene rubber (3-A). The polymer yield was 85%. The vinyl bond content in the obtained polybutadiene rubber (3-A) was 0.2 mol%, and the unsaturated bond carbon content was 50.0 mol%.

[0192] <Example 1>

[0193] (Synthesis of Cross-Metathesis Copolymer (1-A))

[0194] In a nitrogen environment, 96 parts of the ring-opening copolymer (2-A) obtained in Polymerization Example 1, 104 parts of the polybutadiene rubber (3-A) obtained in Polymerization Example 7, and 1611 parts of toluene were added to a glass reaction container with a stirrer to dissolve them. Next, 0.91 parts of dichloro[1,3-bis(2,4,6-trimethylphenyl)-2-imidazolidinyl](benzylidene)(tricyclohexylphosphine)ruthenium(II) dissolved in 10 parts of toluene was added, and a cross-metathesis reaction was carried out at room temperature for 24 hours while stirring. After the reaction, an excess of vinyl ethyl ether was added to terminate the reaction. Then, the obtained cross-metathesis reaction solution was injected into a large excess of methanol containing 2,6-di-tert-butyl-p-cresol (BHT), the precipitated copolymer was recovered, washed with methanol, and then vacuum dried at 50°C for 3 days to obtain 164 parts of a cross-metathesis copolymer (1-A). The obtained cross-metathesis copolymer (1-A) had a number average molecular weight (Mn) of 130,000, a weight average molecular weight (Mw) of 251,000, a ratio of dicyclopentadiene structural unit / butadiene structural unit of 48 / 52 (weight ratio), and a glass transition temperature (Tg) of -22°C. In addition, the cross-metathesis copolymer (1-A) was a copolymer in which p=472, q=0, and n=1252 in the above general formula (1).

[0195] (Preparation of cross-linkable rubber composition)

[0196] 100 parts of the cross metathesis copolymer (1-A) obtained above, 50 parts of carbon black (trade name "Seast 9H", manufactured by Tokai Carbon Co., Ltd.), 3 parts of zinc oxide (zinc oxide No. 1), 2.0 parts of stearic acid (trade name "SA-300", manufactured by Aidi Co., Ltd.) and 2.0 parts of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (trade name "NOCRAC 6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd., antioxidant) were added to a Banbury mixer, and kneaded for 4 minutes at a starting temperature of 80°C, and the rubber composition was discharged from the Banbury mixer. The temperature of the rubber composition at the end of kneading was 160°C. Next, the obtained rubber composition was kneaded with 1.75 parts of sulfur and 1 part of N-cyclohexylbenzothiazole-2-sulfenamide (trade name "NOCCELER-CZ-G (CZ)", manufactured by Ouchi Shinko Chemical Industry Co., Ltd., a crosslinking accelerator) using an open roll at 50° C. to obtain a sheet-like crosslinkable rubber composition.

[0197] Then, the above-mentioned various measurements were performed using the obtained cross-linkable rubber composition. The results are shown in Table 1.

[0198] <Example 2>

[0199] (Synthesis of Cross-Metathesis Copolymer (1-B))

[0200] 152 parts of a cross-metathesis copolymer (1-B) were obtained in the same manner as in Example 1 except that 96 parts of the ring-opening copolymer (2-B) polymerized in Polymerization Example 2 were used instead of 96 parts of the ring-opening copolymer (2-A) polymerized in Polymerization Example 1. The obtained cross-metathesis copolymer (1-B) had a number average molecular weight (Mn) of 121,000, a weight average molecular weight (Mw) of 244,000, a ratio of 2-norbornene structural unit / dicyclopentadiene structural unit / butadiene structural unit of 27 / 27 / 44 (weight ratio), and a glass transition temperature (Tg) of -23°C. In addition, the cross-metathesis copolymer (1-B) was a copolymer in which p=248, q=348, and n=986 in the above general formula (1).

[0201] (Preparation of cross-linkable rubber composition)

[0202] Then, a cross-linkable rubber composition was prepared in the same manner as in Example 1 except that 100 parts of the cross-metathesis copolymer (1-B) obtained above was used, and the measurement was performed in the same manner.

[0203] <Example 3>

[0204] (Synthesis of Cross-Metathesis Copolymer (1-C))

[0205] 147 parts of a cross-metathesis copolymer (1-C) were obtained in the same manner as in Example 1 except that 96 parts of the ring-opening copolymer (2-C) polymerized in Polymerization Example 3 were used instead of 96 parts of the ring-opening copolymer (2-A) polymerized in Polymerization Example 1. The obtained cross-metathesis copolymer (1-C) had a number average molecular weight (Mn) of 119,000, a weight average molecular weight (Mw) of 241,000, a ratio of tetracyclododecene structural unit / butadiene structural unit of 44 / 56 (weight ratio), and a glass transition temperature (Tg) of -23°C. In addition, the cross-metathesis copolymer (1-C) was a copolymer in which p=327, q=0, and n=1234 in the above general formula (1).

[0206] (Preparation of cross-linkable rubber composition)

[0207] Then, a cross-linkable rubber composition was prepared in the same manner as in Example 1 except that 100 parts of the cross-metathesis copolymer (1-C) obtained above was used, and the measurement was performed in the same manner.

[0208] <Example 4>

[0209] (Synthesis of Cross-Metathesis Copolymer (1-D))

[0210] 147 parts of a cross-metathesis copolymer (1-D) were obtained in the same manner as in Example 1 except that 96 parts of the ring-opening copolymer (2-D) polymerized in Polymerization Example 4 was used instead of 96 parts of the ring-opening copolymer (2-A) polymerized in Polymerization Example 1. The obtained cross-metathesis copolymer (1-D) had a number average molecular weight (Mn) of 117,000, a weight average molecular weight (Mw) of 239,000, a ratio of 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene (MTHF) structural unit / butadiene structural unit of 43 / 57 (weight ratio), and a glass transition temperature (Tg) of -24°C. In addition, the cross-metathesis copolymer (1-D) was a copolymer in which p=202, q=0, and n=1235 in the above general formula (1).

[0211] (Preparation of cross-linkable rubber composition)

[0212] Then, a cross-linkable rubber composition was prepared in the same manner as in Example 1 except that 100 parts of the cross-metathesis copolymer (1-D) obtained above was used, and the measurement was performed in the same manner.

[0213] <Comparative Example 1>

[0214] A cross-linkable rubber composition was prepared in the same manner as in Example 1 except that 100 parts of the ring-opening copolymer (1′-E) obtained in Polymerization Example 5 was used instead of 100 parts of the cross-metathesis copolymer (1-A), and the measurement was performed in the same manner.

[0215] <Comparative Example 2>

[0216] A cross-linkable rubber composition was prepared in the same manner as in Example 1 except that 100 parts of the ring-opening copolymer (1′-F) obtained in Polymerization Example 6 was used instead of 100 parts of the cross-metathesis copolymer (1-A), and the measurement was performed in the same manner.

[0217] [Table 1]

[0218]

[0219] As shown in Table 1, according to the rubber composition containing the copolymer represented by the above general formula (1) and a filler, the obtained rubber cross-linked product has high tensile strength, excellent fracture resistance, excellent wet grip and low heat generation, and further, due to the use of carbon material as a filler, it also has excellent wear resistance (Examples 1 to 4).

[0220] On the other hand, when a ring-opening copolymer of a norbornene compound and cyclopentene was used instead of the copolymer represented by the general formula (1), the obtained rubber cross-linked product had low tensile strength, insufficient fracture resistance, and insufficient wet grip performance and low heat build-up properties (Comparative Examples 1 and 2).

[0221] <Example 5>

[0222] 100 parts of the cross-metathesis copolymer (1-A) obtained in Example 1 and 50 parts of silica (trade name "Zeosil 1165MP", manufactured by Rhodia, nitrogen adsorption specific surface area (BET method): 163 m2) were added to a Banbury mixer. 2 / g) and 10 parts of process oil (trade name "Aromax T-DAE", manufactured by Nippon Oil & Gas Co., Ltd.), 6.0 parts of silane coupling agent (bis(3-(triethoxysilyl)propyl)tetrasulfide, trade name "Si69", manufactured by Degussa), and kneading was performed for 1.5 minutes at a starting temperature of 110°C. Next, 25 parts of silica (trade name "Zeosil 1165MP", manufactured by Rhodia), 3 parts of zinc oxide (zinc oxide No. 1), 2.0 parts of stearic acid (trade name "SA-300", manufactured by Asahi Denka Kogyo Co., Ltd.) and 2.0 parts of antioxidant (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, trade name "NOCRAC6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added to the kneaded product, and kneading was performed for 2.5 minutes, and the rubber composition was discharged from the Banbury mixer. The temperature of the rubber composition at the end of kneading was 150° C. After the rubber composition was cooled to room temperature, it was kneaded again in a Banbury mixer for 3 minutes, and then the rubber composition was discharged from the Banbury mixer. Next, the obtained rubber composition was kneaded with 1.5 parts of sulfur and a crosslinking accelerator (a mixture of 1.8 parts of N-tert-butyl-2-benzothiazole sulfenamide (trade name "NOCCELER NS", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) and 1.5 parts of diphenylguanidine (trade name "NOCCELER D", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)) using an open roll at 50° C. to obtain a sheet-like crosslinkable rubber composition.

[0223] Then, the above-mentioned various measurements were performed using the obtained cross-linkable rubber composition. The results are shown in Table 2.

[0224] <Examples 6 to 8>

[0225] A cross-linkable rubber composition was prepared in the same manner as in Example 1, except that 100 parts of the cross-metathesis copolymers (1-B) to (1-D) synthesized in Examples 2 to 4 were used instead of 100 parts of the cross-metathesis copolymer (1-A), and the measurement was performed in the same manner. The results are shown in Table 2.

[0226] <Comparative Example 3>

[0227] A cross-linkable rubber composition was prepared in the same manner as in Example 5 except that 100 parts of the ring-opening copolymer (1′-E) obtained in Polymerization Example 5 was used instead of 100 parts of the cross-metathesis copolymer (1-A), and the measurement was performed in the same manner.

[0228] <Comparative Example 4>

[0229] A cross-linkable rubber composition was prepared in the same manner as in Example 5 except that 100 parts of the ring-opening copolymer (1′-F) obtained in Polymerization Example 6 was used instead of 100 parts of the cross-metathesis copolymer (1-A), and the measurement was performed in the same manner.

[0230] [Table 2]

[0231]

[0232] As shown in Table 2, the rubber composition containing the copolymer represented by the general formula (1) and a filler can provide a rubber cross-linked product having high tensile strength and excellent fracture resistance even when silica is used as a filler (Examples 5 to 8).

[0233] On the other hand, when a ring-opening copolymer of a norbornene compound and cyclopentene was used instead of the copolymer represented by the general formula (1), the obtained rubber cross-linked product had low tensile strength, insufficient fracture resistance, and insufficient wet grip and low heat build-up properties (Comparative Examples 3 and 4).

Claims

1. A copolymer represented by the following general formula (1): In the general formula (1), R 1 ~R 4 are each independently a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent containing a silicon atom, an oxygen atom or a nitrogen atom, and x is 0 to 2, wherein, R 1 ~R 4 Except for the case where all are hydrogen atoms and x=0, R 5 is a hydrogen atom or a methyl group, p is 30 to 2000, q is 0 to 2000, p+q=30 to 2000, n is 200 to 5000, R 1 With R 2 , R 3 With R 4 can be bonded to form a ring, and the plurality of R 1 ~R 5 The values ​​of and x may be the same or different.

2. A rubber composition comprising the copolymer according to claim 1 and a filler.

3. The rubber composition according to claim 2, wherein The filler is a carbon material.

4. The rubber composition according to claim 2, wherein The filler is silicon dioxide. 5 . A cross-linked rubber product obtained by cross-linking the rubber composition according to claim 2 .

6. A method for producing a copolymer, wherein the copolymer is the copolymer according to claim 1, The method for producing the copolymer comprises the following steps: subjecting a first ethylenically unsaturated polymer having an alicyclic structure and an unsaturated bond carbon content of 10 to 40 mol % and a second ethylenically unsaturated polymer having no alicyclic structure and an unsaturated bond carbon content of 20 to 50 mol % to a cross-metathesis reaction in the presence of a metathesis catalyst, thereby obtaining the copolymer represented by the general formula (1).