Composition, crosslinked product, and sealing material
By using a composition of perfluoroelastomer and silicon carbide and graphite in the sealing material, the specific surface area and bulk density of the filler are optimized to form an island structure, and the existing sealing materials are solved to resist compression and permanent deformation and plasma in plasma treatment in plasma treatment. The problem of insufficient physical properties achieves excellent performance at high temperatures.
Patent Information
- Application Number
- CN202380029081.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-05
AI Technical Summary
The existing sealing materials have insufficient compression resistance and plasma resistance in plasma treatment, making it difficult to meet the requirements of high temperature and high pressure conditions of semiconductor manufacturing devices.
The composition of perfluoroelastic elastomer and silicon carbide and graphite as fillers was used to determine the area ratio of graphite to silicon carbide peaks to be above 0.7 by X-ray photoelectron spectroscopy, and the specific surface area of the filler was optimized by combining nitrogen adsorption and water vapor adsorption. and bulk density, the island structure is formed to improve the plasma resistance and compression-resistant permanent deformation characteristics of the crosslinked substance.
The excellent compression-resistant permanent deformation and plasma resistance of the crosslinked substance at high temperatures are achieved. The compression-resistant permanent deformation of the crosslinked substance is less than 50% when it is placed at 300°C for 70 hours. It is suitable for sealing materials for semiconductor manufacturing devices.
Smart Images

Figure BDA0005051976970000131 
Figure BDA0005051976970000161 
Figure BDA0005051976970000162
Abstract
Description
Technical Field
[0001] The invention relates to a composition, a crosslinked product and a sealing material. Background Art
[0002] Perfluoroelastomers are used as materials for sealing materials because of their excellent sealing properties and heat resistance. Sealing materials used in semiconductor manufacturing equipment are required to have plasma resistance, so there is a known technique for imparting plasma resistance to sealing materials by mixing fillers into perfluoroelastomers.
[0003] For example, Patent Document 1 describes a cross-linkable elastomer composition comprising a cross-linkable elastomer and non-oxide ceramics such as carbide and nitride.
[0004] Patent Document 2 describes a cross-linkable fluorinated elastomer having a bulk density of 0.15 g / cm 3 The following cross-linkable fluorinated elastomer composition containing silicon carbide particles.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 03 / 051999
[0008] Patent Document 2: Japanese Patent Application No. 2012-509975 Summary of the invention
[0009] Problems to be solved by the invention
[0010] An object of the present invention is to provide a composition capable of obtaining a cross-linked product having excellent plasma resistance and excellent compression set resistance.
[0011] Means for solving problems
[0012] According to the present invention, there is provided a composition comprising a perfluoroelastomer and a filler, wherein the filler comprises silicon carbide and graphite, and the ratio of the area (C) of the peak derived from the graphite in the filler to the area (SiC) of the peak derived from the silicon carbide in the filler measured by X-ray photoelectron spectroscopy (XPS) (area (C) / area (SiC)) is 0.7 or more.
[0013] In the composition of the present invention, the filler preferably has a BET specific surface area of 15 m 2 / g~200m 2 / g.
[0014] In the composition of the present invention, the ratio of the BET specific surface area of the filler determined by a water vapor adsorption method to the BET specific surface area of the filler determined by a nitrogen adsorption method (water vapor / nitrogen) is preferably 1% to 60%.
[0015] In the composition of the present invention, the bulk density of the filler is preferably 0.10 g / cm 3 above.
[0016] In the composition of the present invention, the content of the filler is preferably 0.1 to 100 parts by mass based on 100 parts by mass of the perfluoroelastomer.
[0017] The composition of the present invention preferably further contains at least one selected from the group consisting of an inorganic nitride, an organic tin compound, a compound that generates ammonia, and a cross-linking agent.
[0018] Furthermore, according to the present invention, there is provided a cross-linked product obtained by cross-linking the above composition.
[0019] The cross-linked product of the present invention can be suitably used as a sealing material.
[0020] The cross-linked product of the present invention preferably has a compression set of 50% or less when measured at a compression rate of 25% at 300°C for 70 hours.
[0021] Effects of the Invention
[0022] According to the present invention, a composition capable of obtaining a cross-linked product having excellent plasma resistance and excellent compression set resistance can be provided. DETAILED DESCRIPTION
[0023] Hereinafter, specific embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.
[0024] The composition of the present invention contains a perfluoroelastomer and a filler.
[0025] Patent Document 1 states that by using non-oxide ceramics such as carbides and nitrides as fillers mixed in a crosslinkable elastomer composition, a molded product with a small weight change can be obtained with respect to NF3 plasma treatment and O3 treatment exposed in the semiconductor manufacturing process. In addition, Patent Document 2 states that by using a bulk density of 0.15 g / cm 3 The following silicon carbide particles are blended as a filler in a cross-linkable fluorine-containing elastomer composition to obtain a molded article having a small weight change both in the O2 plasma treatment and in the O2 / CF4 plasma treatment.
[0026] In contrast, the composition of the present invention contains silicon carbide and graphite, and the ratio of the area (C) of the peak derived from graphite in the filler to the area (SiC) of the peak derived from silicon carbide in the filler measured by X-ray photoelectron spectroscopy (XPS) (area (C) / area (SiC)) is 0.7 or more. It was found that by using such a filler, a cross-linked product having excellent plasma resistance and excellent compression set resistance at high temperatures can be obtained.
[0027] <Packing>
[0028] The filler contained in the composition of the present invention contains silicon carbide and graphite, and the ratio (area (C) / area (SiC)) is 0.7 or more.
[0029] The area of the peak derived from silicon carbide in the filler (SiC) and the area of the peak derived from graphite in the filler (C) can be determined by analyzing the filler using X-ray photoelectron spectroscopy. The area of the peak (SiC) and the area of the peak (C) are the areas of the peaks of carbon 1s derived from silicon carbide and graphite in the filler.
[0030] From the perspective of further improving the plasma resistance and compression set resistance of the crosslinked product, the filler ratio (area (C) / area (SiC)) is preferably 1.0 or more, more preferably 1.6 or more, and is preferably 3.0 or less, more preferably 2.0 or less.
[0031] The filler of the present invention contains silicon carbide and graphite. The filler containing silicon carbide and graphite can be confirmed by, for example, obtaining a transmission electron microscope photograph of the filler and an element mapping image of carbon element using a transmission electron microscope (TEM) equipped with an energy dispersive X-ray analyzer (EDS) device.
[0032] The content of graphite is preferably 0% to 10% by mass relative to the mass of the filler, more preferably 0.1% by mass or more, further preferably 0.5% by mass or more, particularly preferably 1.0% by mass or more, more preferably 8.0% by mass or less, further preferably 6.0% by mass or less, and particularly preferably 5.0% by mass or less. The filler contained in the composition of the present invention also includes a filler containing a trace amount of graphite to the extent that the weight loss cannot be measured by differential thermal thermogravimetric simultaneous measurement.
[0033] The content of graphite can be measured by the following method. That is, using a differential thermal and thermogravimetric simultaneous measurement device, heat about 10 mg of filler in an air atmosphere, raise the temperature of the filler from room temperature to 1000°C at a rate of 10°C / minute, and measure the weight at the moment when the weight decreases the most. Next, by subtracting the weight at the moment when the weight decreases the most from the initial weight (the weight at room temperature before heating), the weight loss at the moment when the weight decreases the most is calculated. Then, as the weight reduction ratio, the ratio (%) of the weight reduction at the moment when the weight decreases the most to the initial weight is calculated. In the present invention, the normal temperature can be a temperature in the range of 10°C to 40°C. The temperature range of 10°C to 40°C will not have a significant impact on the calculated value of the weight reduction ratio.
[0034] When the filler contains silicon carbide and graphite, it is presumed that the weight loss caused by heating the filler is caused by the sublimation of graphite combined with oxygen in the air. Therefore, when the filler contains silicon carbide and graphite, the content of graphite in the filler can be understood by finding the weight loss ratio of the filler.
[0035] From the viewpoint of further improving the plasma resistance and compression set resistance of the obtained crosslinked product, the BET specific surface area of the filler determined by the nitrogen adsorption method is preferably 15 m 2 / g~150m 2 / g, more preferably 20m 2 / g or more, more preferably 40m 2 / g or more, more preferably 50m 2 / g or more, more preferably 100m 2 / g or less, more preferably 80m 2 / g or less.
[0036] The BET specific surface area of the filler obtained by the nitrogen adsorption method can be measured by a BET flow method (single point method) using nitrogen gas and a mixed gas (nitrogen 30%+helium 70%).
[0037] From the viewpoint of further improving the plasma resistance and compression set resistance of the obtained cross-linked product, the BET specific surface area of the filler determined by the water vapor adsorption method is preferably 1 m 2 / g~15m 2 / g, more preferably 3m 2 / g or more, more preferably 4m 2 / g or more, more preferably 12m 2 / g or less, more preferably 10m 2 / g or less.
[0038] The BET specific surface area of the filler obtained by the water vapor adsorption method can be calculated by the BET method from the water vapor adsorption-desorption isotherm obtained by measuring the water vapor adsorption of the filler.
[0039] From the perspective of further improving the plasma resistance and compression set resistance of the obtained cross-linked product, the ratio of the BET specific surface area of the filler obtained by the water vapor adsorption method to the BET specific surface area of the filler obtained by the nitrogen adsorption method (water vapor / nitrogen) is preferably 1% to 60%, more preferably 3% to 40%, further preferably 4% or more, further preferably 5% or more, more preferably 30% or less, and further preferably 20% or less.
[0040] The ratio of the BET specific surface area of the filler obtained by the water vapor adsorption method to the BET specific surface area of the filler obtained by the nitrogen adsorption method (water vapor / nitrogen) is an indicator of the hydrophilicity of the filler. A higher ratio (water vapor / nitrogen) means a higher hydrophilicity of the filler.
[0041] The bulk density of the filler is preferably 0.10 g / cm 3 More preferably 0.12 g / cm 3 More preferably, 0.14 g / cm 3 More preferably, 0.30 g / cm 3 Below, more preferably 0.20 g / cm 3 the following.
[0042] The bulk density of the filler can be calculated as follows: 5 g of the powder is placed in a 100 ml graduated cylinder (inner diameter 28 mm), the scale is read after tapping 20 times from a height of 2 cm, and the bulk density is calculated from the volume.
[0043] From the perspective of further improving the plasma resistance and compression set resistance of the obtained cross-linked product, the average particle size of the filler is preferably 10 nm to 100 nm, more preferably 15 nm or more, further preferably 20 nm or more, more preferably 90 nm or less, further preferably 80 nm or less.
[0044] The average particle size (DBET) of the filler can be determined by the BET specific surface area of the filler using the nitrogen adsorption method and is given by the average particle size (nm) = 6000 / (specific surface area (m 2 / g)×true density (g / cm 3 )) is calculated. The true density can be set to the true density of silicon carbide, 3.22 g / cm 3 .
[0045] The filler used in the present invention is preferably manufactured by a thermal plasma method. The filler used in the present invention can be manufactured, for example, as follows: using an inert gas as a carrier gas, silicon powder or silicon carbide powder is introduced into a thermal plasma flame and evaporated to form a mixture in a gas phase, and the mixture in a gas phase is contacted with a hydrocarbon gas to manufacture. At this time, by using the method described in Japanese Patent Publication No. 2007-138287, Japanese Patent Publication No. 2011-213524, and non-patent literature (Ya-Li LI and Takamasa ISHIGAKI, "Synthesis and Structural Characterization of Core-Shell Si-SiC Composite Particles by Thermal Plasma In-Flight Carburization of Silicon Powder", Journal of the Ceramic Society of Japan, 2007, 115 (11), p. 717-723), the ratio of the obtained filler (area (C) / area (SiC)) can be adjusted.
[0046] From the viewpoint of further improving the plasma resistance and compression set resistance of the obtained cross-linked product, the content of the filler in the composition of the present invention is preferably 0.1 to 100 parts by mass, more preferably 0.5 parts by mass or more, further preferably 1.0 parts by mass or more, particularly preferably 5 parts by mass or more, more preferably 50 parts by mass or less, further preferably 30 parts by mass or less, and particularly preferably 25 parts by mass or less, based on 100 parts by mass of the perfluoroelastomer.
[0047] From the perspective of further improving the plasma resistance and compression set resistance of the cross-linked product, the composition of the present invention preferably has a sea-island structure formed by an island composed of a filler and a sea composed of a perfluoroelastomer. Such a sea-island structure contains silicon carbide and can be formed by mixing a filler showing the above-mentioned ratio (area (C) / area (SiC)) into a perfluoroelastomer. If conventional silicon carbide is mixed into a perfluoroelastomer, a composition having a network structure formed by highly dispersing silicon carbide in the perfluoroelastomer can be obtained, especially when the BET specific surface area (nitrogen adsorption method) or the average particle size of the silicon carbide is small. On the other hand, if a filler showing the above-mentioned ratio (area (C) / area (SiC)) is used, a composition having a sea-island structure can be obtained even when the BET specific surface area (nitrogen adsorption method) or the average particle size of the filler is small. The dispersion state of the filler in the composition can be confirmed, for example, by observing the surface or cross-section of the composition using a transmission electron microscope (TEM).
[0048] <Perfluoroelastomer>
[0049] The composition of the present invention contains a perfluoroelastomer.
[0050] In the present invention, the perfluoroelastomer refers to a fluoropolymer in which the content of perfluoromonomer units relative to all polymerized units is 90 mol% or more, preferably 91 mol% or more, has a glass transition temperature of 20°C or less, has a melting peak (ΔH) of 4.5 J / g or less, and further, is a polymer in which the concentration of fluorine atoms contained in the fluoropolymer is 71 mass% or more, preferably 71.5 mass% or more. In the present invention, the concentration of fluorine atoms contained in the fluoropolymer is obtained by calculating the concentration (mass%) of fluorine atoms contained in the fluoropolymer based on the type and content of each monomer constituting the fluoropolymer.
[0051] In the present invention, a perfluoromonomer refers to a monomer that does not contain a carbon atom-hydrogen atom bond in the molecule. The perfluoromonomer may be a monomer in which, in addition to carbon atoms and fluorine atoms, a number of fluorine atoms bonded to carbon atoms are replaced by chlorine atoms, or a monomer having nitrogen atoms, oxygen atoms, sulfur atoms, phosphorus atoms, boron atoms or silicon atoms in addition to carbon atoms. As the perfluoromonomer, a monomer in which all hydrogen atoms are replaced by fluorine atoms is preferred. The perfluoromonomer does not contain a monomer that provides a crosslinking site.
[0052] The monomer providing a crosslinking site refers to a monomer having a crosslinkable group that provides a crosslinking site for forming a crosslink with a curing agent to the fluoropolymer (curing site monomer).
[0053] In the present invention, the content of each monomer constituting the perfluoroelastomer can be calculated by appropriately combining NMR, FT-IR, elemental analysis, fluorescent X-ray analysis, and other known methods according to the types of monomers.
[0054] The perfluoromonomer providing the perfluoromonomer units constituting the perfluoroelastomer is preferably selected from
[0055] Tetrafluoroethylene [TFE],
[0056] Hexafluoropropylene [HFP],
[0057] General formula (13): CF2=CF-ORf 13
[0058] (Where Rf 13 represents a perfluoroalkyl group having 1 to 8 carbon atoms),
[0059] General formula (14): CF2=CFOCF2ORf 14
[0060] (Where Rf14 a fluorinated monomer represented by a linear or branched perfluoroalkyl group having 1 to 6 carbon atoms, a cyclic perfluoroalkyl group having 5 to 6 carbon atoms, or a linear or branched perfluorooxyalkyl group having 2 to 6 carbon atoms containing 1 to 3 oxygen atoms, and
[0061] General formula (15): CF2=CFO(CF2CF(Y 15 )O) m (CF2) n F
[0062] (Where Y 15 represents a fluorine atom or a trifluoromethyl group. m is an integer of 1 to 4. n is an integer of 1 to 4) is at least one of the group consisting of fluorinated monomers represented by.
[0063] The perfluoroelastomer is preferably a perfluoroelastomer containing TFE units, for example, preferably at least one selected from the group consisting of a copolymer of TFE / a fluorinated monomer represented by the general formula (13), (14) or (15) and a copolymer of TFE / a fluorinated monomer represented by the general formula (13), (14) or (15) / a monomer providing a crosslinking site.
[0064] Regarding the composition, in the case of TFE / perfluoro(methyl vinyl ether) (PMVE) copolymer, it is preferably 45 to 90 / 10 to 55 (mol %), more preferably 55 to 80 / 20 to 45, further preferably 55 to 70 / 30 to 45, and most preferably 56 to 69.5 / 30.5 to 44.
[0065] In the case of a copolymer of TFE / PMVE / a monomer providing a cross-linking site, the ratio is preferably 45-89.9 / 10-54.9 / 0.01-4 (mol %), more preferably 55-77.9 / 20-49.9 / 0.1-3.5, further preferably 55-69.8 / 30-44.8 / 0.2-3, and most preferably 55.3-69.5 / 30.3-44.5 / 0.2-2.8.
[0066] In the case of a copolymer of TFE / a fluorinated monomer represented by the general formula (13), (14) or (15) having 4 to 12 carbon atoms, the ratio is preferably 50 to 90 / 10 to 50 (mol %), more preferably 60 to 88 / 12 to 40, further preferably 65 to 85 / 15 to 35, and most preferably 66 to 84 / 16 to 34.
[0067] In the case of a copolymer of TFE / a fluorinated monomer represented by the general formula (13), (14) or (15) having 4 to 12 carbon atoms / a monomer providing a crosslinking site, the ratio is preferably 50 to 89.9 / 10 to 49.9 / 0.01 to 4 (mol %), more preferably 60 to 87.9 / 12 to 39.9 / 0.1 to 3.5, further preferably 65 to 84.8 / 15 to 34.8 / 0.2 to 3, and most preferably 66 to 84.3 / 15.5 to 33.8 / 0.2 to 2.8.
[0068] Outside this composition range, the properties as a rubber elastic body are lost and the properties close to those of a resin tend to be exhibited.
[0069] The perfluoroelastomer is preferably at least one selected from the group consisting of a copolymer of TFE / fluorinated monomer represented by the general formula (15) / a monomer providing a cross-linking site, a copolymer of TFE / fluorinated monomer represented by the general formula (15), a copolymer of TFE / fluorinated monomer represented by the general formula (13), and a copolymer of TFE / fluorinated monomer represented by the general formula (13) / a monomer providing a cross-linking site.
[0070] Examples of the perfluoroelastomer include perfluoroelastomers described in International Publication No. 97 / 24381, Japanese Examined Patent Publication No. 61-57324, Japanese Examined Patent Publication No. 4-81608, Japanese Examined Patent Publication No. 5-13961, and the like.
[0071] The monomer providing a crosslinking site refers to a monomer having a crosslinkable group that provides a crosslinking site for forming a crosslink with a crosslinking agent to the perfluoroelastomer (curing site monomer).
[0072] Examples of the monomer providing a crosslinking site include
[0073] General formula (16): CX 4 2=CX 5 R f 2 X 6
[0074] (Where X 4 , X 5 Each independently represents H, F or an alkyl group having 1 to 5 carbon atoms, Rf 2 is a linear or branched alkylene or oxyalkylene group which may have one or more ether-bonded oxygen atoms, may have an aromatic ring, and may have a part or all of hydrogen atoms substituted by fluorine atoms, X 6 The monomer is represented by an iodine atom, a bromine atom, a nitrile group, a carboxyl group, an alkoxycarbonyl group, a hydroxyl group, a vinyl group, an azido group, a sulfonylazido group, a carbonylazido group or an alkynyl group). The alkynyl group may be an ethynyl group.
[0075] As the monomer providing a crosslinking site, preferably selected from the group consisting of
[0076] General formula (17): CX 16 2=CX 16 -Rf 16 CHR 16 X 17
[0077] (Where X 16 Each independently is a hydrogen atom, a fluorine atom or CH3, Rf 16 is a fluoroalkylene group, a perfluoroalkylene group, a fluoro(poly)oxyalkylene group or a perfluoro(poly)oxyalkylene group, R 16 is a hydrogen atom or CH3, X 17 is an iodine atom or a bromine atom),
[0078] General formula (18): CX 16 2=CX 16 -Rf 17 X 17
[0079] (Where X 16 Each independently is a hydrogen atom, a fluorine atom or CH3, Rf 17 is a fluoroalkylene group, a perfluoroalkylene group, a fluoro(poly)oxyalkylene group or a perfluoro(poly)oxyalkylene group, X 17 is an iodine atom or a bromine atom),
[0080] General formula (19): CF2=CFO(CF2CF(CF3)O) m (CF2) n -X 18
[0081] (wherein, m is an integer from 0 to 5, n is an integer from 1 to 3, and X 18 is a fluorine-containing monomer represented by a cyano group, an azido group, a sulfonylazido group, a carbonylazido group, a carboxyl group, an alkoxycarbonyl group, an alkynyl group, an iodine atom, a bromine atom or CH2I),
[0082] General formula (20): CH2=CFCF2O(CF(CF3)CF2O) m (CF(CF3)) n -X 19
[0083] (wherein, m is an integer from 0 to 5, n is an integer from 1 to 3, and X 19 is a fluorine-containing monomer represented by a cyano group, a carboxyl group, an alkoxycarbonyl group, an iodine atom, a bromine atom, or CH2OH) and
[0084] General formula (21): CR 202=CR 20 -Z-CR 20 =CR 20 2
[0085] (Where R 20 Each is independently a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. Z is a linear or branched alkylene group having 1 to 18 carbon atoms, a cycloalkylene group having 3 to 18 carbon atoms, an at least partially fluorinated alkylene group having 1 to 10 carbon atoms, or an oxyalkylene group having 1 to 10 carbon atoms, which may or may not have an oxygen atom.
[0086] -(Q) p -CF2O-(CF2CF2O) m (CF2O) n -CF2-(Q) p -
[0087] (wherein, Q is an alkylene group or an oxyalkylene group. p is 0 or 1. m / n is 0.2 to 5) and a (per)fluoropolyoxyalkylene group having a molecular weight of 500 to 10000) is a monomer.
[0088] X 16 It is preferably a fluorine atom. 16 and Rf 17 It is preferably a perfluoroalkylene group having 1 to 5 carbon atoms. 16 Preferably, it is a hydrogen atom. 18 Preferably, it is a cyano group, an alkoxycarbonyl group, an iodine atom, a bromine atom or -CH2I. 19 Preferred is a cyano group, an alkoxycarbonyl group, an iodine atom, a bromine atom or -CH2OH.
[0089] The monomer providing a crosslinking site is preferably selected from CF2=CFOCF2CF(CF3)OCF2CF2CN, CF2=CFOCF2CF(CF3)OCF2CF2COOH, CF2=CFOCF2CF(CF3)OCF2CF2CH2I, CF2=CFOCF2CF2CH2I, CH2=CFCF2OCF(CF3)CF2OCF(CF3)CN, CH2=CFCF2OCF(CF3)CF2OCF(CF3)COOH, CH2=CFCF2OCF(CF3)CF2OCF(CF3)CH2OH, CH2=CHCF2CF2I , CH2=CH(CF2)2CH=CH2, CH2=CH(CF2)6CH=CH2, CF2=CFO(CF2)3CN and CF2=CFO(CF2)5CN, more preferably at least one selected from the group consisting of CF2=CFOCF2CF(CF3)OCF2CF2CN, CF2=CFO(CF2)5CN and CF2=CFOCF2CF2CH2I.
[0090] The glass transition temperature of the perfluoroelastomer is preferably -30°C or higher, more preferably -20°C or higher, and further preferably -10°C or higher, from the perspective of excellent compression set characteristics at high temperatures. In addition, from the perspective of good cold resistance, it is preferably 10°C or lower, more preferably 5°C or lower, and further preferably 0°C or lower.
[0091] The above-mentioned glass transition temperature can be calculated as follows: using a differential scanning calorimeter (manufactured by Mettler Toredo, DSC822e), 10 mg of the sample is heated at 10°C / min to obtain a DSC curve, and the temperature of the midpoint of the two intersections of the extended line of the baseline before and after the secondary phase transition of the DSC curve and the tangent line at the inflection point of the DSC curve is calculated, and the midpoint is taken as the above-mentioned glass transition temperature.
[0092] For the perfluoroelastomer, from the viewpoint of good heat resistance, the Mooney viscosity ML (1+20) at 170°C is preferably 30 or more, more preferably 40 or more, and further preferably 50 or more. From the viewpoint of good processability, it is preferably 100 or less, more preferably 90 or less, and further preferably 80 or less.
[0093] For the perfluoroelastomer, from the viewpoint of good heat resistance, the Mooney viscosity ML (1+20) at 140°C is preferably 30 or more, more preferably 40 or more, and further preferably 50 or more. From the viewpoint of good processability, it is preferably 180 or less, more preferably 150 or less, and further preferably 110 or less.
[0094] For the perfluoroelastomer, from the viewpoint of good heat resistance, the Mooney viscosity ML (1+10) at 100°C is preferably 10 or more, more preferably 20 or more, and further preferably 30 or more. From the viewpoint of good processability, it is preferably 120 or less, more preferably 100 or less, and further preferably 80 or less.
[0095] The Mooney viscosity can be measured at 170° C. or 140° C. or 100° C. in accordance with JIS K6300 using a Mooney viscometer MV2000E manufactured by ALPHA TECHNOLOGIES.
[0096] Perfluoroelastomer can be manufactured by conventional methods, but from the aspects of narrow molecular weight distribution of the obtained polymer, easy control of molecular weight, and ability to introduce iodine atoms or bromine atoms to the terminal, iodine compounds or bromine compounds can also be used as chain transfer agents. As a polymerization method using iodine compounds or bromine compounds, for example, a method of emulsification polymerization in an aqueous medium under pressure in the presence of iodine compounds or bromine compounds in a substantially oxygen-free state (iodine transfer polymerization method) can be cited. As a representative example of the iodine compounds or bromine compounds used, for example, the general formula can be cited:
[0097] R 21 I x Br y
[0098] (where x and y are integers from 0 to 2 and satisfy 1≤x+y≤2, R 21 is a saturated or unsaturated fluorocarbon or chlorofluorocarbon group having 1 to 16 carbon atoms, or a hydrocarbon group having 1 to 3 carbon atoms, wherein R 21 By using an iodine compound or a bromine compound, an iodine atom or a bromine atom is introduced into the polymer to function as a crosslinking point.
[0099] Examples of the iodine compound and the bromine compound include 1,3-diiodoperfluoropropane, 2-iodoperfluoropropane, 1,3-diiodoperfluoropropane, 1,4-diiodoperfluorobutane, 1,5-diiodoperfluoropentane, 1,6-diiodoperfluorohexane, 1,8-diiodoperfluorooctane, 1,12-diiodoperfluorododecane, 1,16-diiodoperfluorohexadecane, diiodomethane, 1,2-diiodoethane, 1,3-diiodoperfluoropropane, CF2Br2, BrCF2CF2Br, CF3CFBrCF2Br, CFClBr2, BrCF2CFClBr, CFBrClCFClBr, BrCF2CF2CF2Br, BrCF2CFBrOCF3, 1-bromo-2-iodoperfluoroethane, 1-bromo-3-iodoperfluoropropane, 1-bromo-4-iodoperfluorobutane, 2-bromo-3-iodoperfluorobutane, 3-bromo-4-iodoperfluoro-1-butene, 2-bromo-4-iodoperfluoro-1-butene, mono-iodine and mono-bromine substitution products of benzene, di-iodine and mono-bromine substitution products, and (2-iodoethyl) and (2-bromoethyl) substitution products, etc. These compounds can be used alone or in combination with each other.
[0100] Among these, 1,4-diiodoperfluorobutane, 1,6-diiodoperfluorohexane, and 2-iodoperfluoropropane are preferably used in view of polymerization reactivity, crosslinking reactivity, and availability.
[0101] The perfluoroelastomer preferably has a cyano group (-CN group). The perfluoroelastomer having a cyano group (-CN group) is, for example, a perfluoroelastomer in which the cyano group can be cross-linked by forming a triazine ring through cyclotrimerization, or a perfluoroelastomer in which a tetraamine compound can be used as a cross-linking agent to form an imidazole ring and cross-link, and can impart excellent compression set characteristics and heat resistance to the cross-linked product.
[0102] The above-mentioned perfluoroelastomer having a cyano group preferably has a cyano group (—CN group) at the main chain terminal and / or a side chain.
[0103] As a perfluoroelastomer having a cyano group (-CN group) at the main chain terminal and / or side chain, there can be mentioned a copolymer in which the monomer providing a crosslinking site is a monomer having a cyano group (-CN group) among the above-mentioned TFE / fluorine-containing monomers represented by the general formula (13), (14) or (15) / monomers providing a crosslinking site copolymers. In this case, from the perspective of good crosslinking characteristics and heat resistance, the content of the monomer units having a cyano group (-CN group) can be 0.1 mol% to 5 mol%, or 0.3 mol% to 3 mol% relative to the total amount of the TFE units and the fluorine-containing monomer units represented by the general formula (13), (14) and (15). The more preferred composition is as described above.
[0104] Examples of monomers having a cyano group (-CN group) include:
[0105] Formula: CY 1 2=CY 1 (CF2) n -CN
[0106] (Where Y 1 are each independently a hydrogen atom or a fluorine atom, and n is an integer of 1 to 8)
[0107] Formula: CF2=CFCF2Rf 8 -CN
[0108] (Where Rf 8 -(OCF2) n -or-(OCF(CF3)) n -, n is an integer from 0 to 5)
[0109] Formula: CF2=CFCF2(OCF(CF3)CF2) m (OCH2CF2CF2) n OCH2CF2-CN
[0110] (wherein m is an integer from 0 to 5, and n is an integer from 0 to 5)
[0111] Formula: CF2=CFCF2(OCH2CF2CF2) m (OCF(CF3)CF2) n OCF(CF3)-CN
[0112] (wherein m is an integer from 0 to 5, and n is an integer from 0 to 5)
[0113] Formula: CF2=CF(OCF2CF(CF3)) m O(CF2) n -CN
[0114] (wherein m is an integer from 0 to 5, and n is an integer from 1 to 8)
[0115] Formula: CF2=CF(OCF2CF(CF3)) m -CN
[0116] (wherein m is an integer from 1 to 5)
[0117] Formula: CF2=CFOCF2(CF(CF3)OCF2) n CF(-CN)CF3
[0118] (where n is an integer from 1 to 4)
[0119] Formula: CF2 = CFO (CF2) n OCF(CF3)-CN
[0120] (where n is an integer from 2 to 5)
[0121] Formula: CF2 = CFO (CF2) n -(C6H4)-CN
[0122] (where n is an integer from 1 to 6)
[0123] Formula: CF2=CF(OCF2CF(CF3)) n OCF2CF(CF3)-CN
[0124] (where n is an integer from 1 to 2)
[0125] Formula: CH2=CFCF2O(CF(CF3)CF2O) n CF(CF3)-CN
[0126] (where n is an integer from 0 to 5)
[0127] Formula: CF2 = CFO (CF2CF (CF3) O) m (CF2) n -CN
[0128] (wherein m is an integer from 0 to 5, and n is an integer from 1 to 3)
[0129] Formula: CH2=CFCF2OCF(CF3)OCF(CF3)-CN
[0130] Formula: CH2=CFCF2OCH2CF2-CN
[0131] Formula: CF2 = CFO (CF2CF (CF3) O) m CF2CF(CF3)-CN
[0132] (wherein m is an integer greater than 0)
[0133] Formula: CF2=CFOCF(CF3)CF2O(CF2) n -CN
[0134] (where n is an integer greater than 1)
[0135] Formula: CF2=CFOCF2OCF2CF(CF3)OCF2-CN
[0136] Formula: CF2=CFO(CF2)3CN
[0137] Formula: CF2=CFO(CF2)5CN
[0138] The monomers shown above can be used alone or in any combination.
[0139] Among the above, preferably
[0140] Formula: CF2=CF(OCF2CF(CF3)) m O(CF2) n -CN
[0141] (wherein m is an integer of 0 to 5, and n is an integer of 1 to 8), more preferably CF2=CFOCF2CF(CF3)OCF2CF2CN.
[0142] These perfluoroelastomers can be produced by conventional methods.
[0143] Specific examples of the perfluoroelastomer include fluororubbers described in International Publication No. 97 / 24381, Japanese Examined Patent Publication No. 61-57324, Japanese Examined Patent Publication No. 4-81608, Japanese Examined Patent Publication No. 5-13961, and the like.
[0144] <Other ingredients>
[0145] The composition of the present invention may further contain a filler other than the above-mentioned silicon carbide.
[0146] As fillers, there can be mentioned imide-based fillers having an imide structure, such as polyimide, polyamide-imide, and polyetherimide; organic fillers made of engineering plastics, such as polyarylate, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyetherketone, and polyoxybenzoate; metal oxide fillers, such as silicon oxide, aluminum oxide, and yttrium oxide; metal carbides, such as aluminum carbide; metal nitride fillers, such as silicon nitride and aluminum nitride; and inorganic fillers, such as carbon black, aluminum fluoride, and carbon fluoride.
[0147] Among these, carbon black, aluminum oxide, silicon oxide, yttrium oxide, silicon nitride, polyimide, and carbon fluoride are preferred from the viewpoint of shielding effects of various plasmas.
[0148] The above-mentioned inorganic fillers and organic fillers may be mixed alone or in combination of two or more.
[0149] In the field where high purity and non-polluting properties are not particularly required, conventional additives such as processing aids, plasticizers, colorants, etc. that are normally added to the composition as required may be mixed, and one or more conventional crosslinking agents or crosslinking aids different from the above may also be mixed.
[0150] The above composition may also contain an organic alkaline compound. Examples of the organic alkaline compound include:
[0151] Formula: CH3(CH2)17 -NH2-octadecylamine;
[0152] Formula: H2N-C(O)-(CH2) 11 -Erucamide of CH=CH-(CH2)7CH3;
[0153] Oleamide of formula: H2N-C(O)-(CH2)7-CH=CH-(CH2)7CH3;
[0154] Formula: H2N-(CH2)6-NH2 1,6-hexanediamine
[0155] Mode:
[0156] [Chemistry 1]
[0157]
[0158] 1,8-diazabicycloundec-7-ene (DBU), etc.
[0159] <Crosslinking agent, etc.>
[0160] The composition of the present invention may further contain at least one selected from the group consisting of an inorganic nitride, an organic tin compound, a compound generating ammonia, and a crosslinking agent. By making the composition of the present invention contain such components as a crosslinking agent, a crosslinked product can be easily obtained from the composition of the present invention.
[0161] The inorganic nitride is not particularly limited, and examples thereof include silicon nitride (Si3N4), lithium nitride, titanium nitride, aluminum nitride, boron nitride, vanadium nitride, zirconium nitride, etc. Among these, silicon nitride is preferred because it can provide nano-scale fine particles.
[0162] Examples of the organic tin compound include tetraphenyltin and triphenyltin.
[0163] As the compound generating ammonia, a compound generating ammonia at 40°C to 330°C is preferred.
[0164] As the ammonia-generating compound, urea or its derivatives, ammonium salts are preferred, urea or ammonium salts are more preferred, and urea is further preferred. As the ammonium salt, it can be an organic ammonium salt or an inorganic ammonium salt. In addition, as the ammonia-generating compound, it can be a substance that reacts with a trace amount of water to generate ammonia.
[0165] Examples of urea derivatives include diurea, thiourea, urea hydrochloride, and biuret.
[0166] Examples of the organic ammonium salt include ammonium salts of non-fluorinated carboxylic acids or sulfonic acids such as ammonium benzoate, ammonium adipate, and ammonium phthalate.
[0167] Examples of the inorganic ammonium salt include compounds described in Japanese Patent Application Laid-Open No. 9-111081, for example, ammonium sulfate, ammonium carbonate, ammonium nitrate, ammonium phosphate, and the like.
[0168] In addition, examples of the ammonia-generating compound include acetaldehyde ammonia, hexamethylenetetramine, formamidine, formamidine hydrochloride, formamidine acetate, tert-butyl carbamate, benzyl carbamate, phthalamide, and the like.
[0169] As the crosslinking agent, there can be mentioned crosslinking agents used in peroxide crosslinking, polyol crosslinking, polyamine crosslinking, triazine crosslinking, oxazole crosslinking, imidazole crosslinking and thiazole crosslinking. In the case where the perfluoroelastomer has a cyano group (-CN group), the crosslinking agent is preferably at least one selected from the group consisting of an oxazole crosslinking agent, an imidazole crosslinking agent and a thiazole crosslinking agent.
[0170] The crosslinking agent used in the peroxide crosslinking may be any organic peroxide that can easily generate peroxide radicals in the presence of heat or a redox system. Specific examples thereof include 1,1-bis(tert-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-tert-butyl peroxide (Perbutyl D), tert-butylcumyl peroxide (Perbutyl C), dicumyl peroxide (Percumyl D, Percumyl D-40, Percumyl D-40MB (T)), α,α-bis(tert-butylperoxy)-p-diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (Perhexa 25B, Perhexa 25B-40), 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne (Perhexyne 25B, Perhexyne 25B-40), benzoyl peroxide, tert-butylbenzene peroxide, 2,5-dimethyl-2,5-di(benzoyl peroxide)hexane (Perhexa 25Z), tert-butyl peroxymaleate (t-butyl MA), tert-butyl peroxyisopropyl carbonate (Perbutyl I-75), methyl ethyl ketone peroxide (Permek D (DR), Permek H (HR, HY), Permek N (NR, NY), Permek S (SR), Permek F (FR), Permek G (GR, GY)), cyclohexanone peroxide (Perhexa H), acetylacetone peroxide (Percure AH, AL), 1,1-di(tert-hexylperoxy)-3,3,5-trimethylcyclohexane (Perhexa TMH), 1,1-di(tert-hexylperoxy)cyclohexane (Perhexa HC), 1,1-di(tert-butylperoxy)-2-methylcyclohexane (Perhexa MC), 1,1-di(tert-butylperoxy)cyclohexane (Perhexa C-80(S), Perhexa C-75(EB), Perhexa C(C), Perhexa C-40, Perhexa C-40MB(S)), 2,2-di(tert-butylperoxy)butane (Perhexa 22), 4,4-di(tert-butylperoxy)butyl valerate (Perhexa V, Perhexa V-40(F)), 2,2-di(4,4-di(tert-butylperoxy)cyclohexyl)propane (Pertetra A), terpene hydroperoxide (Permenta H), diisopropylbenzene hydroperoxide (Percumyl P), 1,1,3,3-Tetramethylbutyl hydroperoxide (Perocta H), cumene hydroperoxide (Percumyl H-80), tert-butyl hydroperoxide (Perbutyl H-69), di(2-tert-butylperoxyisopropyl)benzene (Perbutyl P, Perbutyl P-40, Peroximon F-40, Perbutyl P-40MB(K)), di-tert-hexyl peroxide (Perhexyl D), diisobutyryl peroxide (Peroyl IB), di(3,5,5-trimethylhexanoyl) peroxide (Peroyl 355(S)), dilauroyl peroxide (Peroyl L), succinyl peroxide (Peroyl SA), di(3-methylbenzoyl) peroxide, benzoyl (3-methylbenzoyl) peroxide and a mixture of dibenzoyl peroxide (NYPER BMT-K40, NYPER BMT-M), dibenzoyl peroxide (NYPER BW, NYPER BO, NYPER FF, NYPER BS, NYPER E, NYPER NS), di(4-methylbenzoyl) peroxide (NYPER PMB), di-n-propyl peroxydicarbonate (Peroyl NPP-50M), diisopropyl peroxydicarbonate (Peroyl IPP-50, Peroyl IPP-27), di(4-tert-butylcyclohexyl) peroxydicarbonate (Peroyl TCP), di(2-ethylhexyl) peroxydicarbonate (Peroyl OPP), di-sec-butyl peroxydicarbonate (Peroyl SBP), cumyl peroxyneodecanoate (Percumyl ND, Percumyl ND-50E), 1,1,3,3-tetramethylbutyl peroxyneodecanoate (Perocta ND, Perocta ND-50E), tert-hexyl peroxyneodecanoate (Perhexyl ND, Perhexyl ND-50E), tert-butyl peroxyneodecanoate (Perbutyl ND, Perbutyl ND-50E), tert-butyl peroxy neoheptanoate (Perbutyl NHP), tert-hexyl peroxy pivalate (Perhexyl PV, Perhexyl PV-50E), tert-butyl peroxy pivalate (PerbutylPV, Perbutyl PV-40E), 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate (Perocta O), 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane (Perhexa 25O), tert-hexyl peroxy(2-ethyl)hexanoate (PerhexylO, Percure HO(N)), tert-butyl peroxy(2-ethylhexanoate) (Perbutyl O, Percure O), tert-hexyl peroxyisopropyl monocarbonate (Perhexyl I), tert-butyl peroxy-3,5,5-trimethylhexanoate (Perbutyl355), tert-butyl peroxylaurate (Perbutyl L), tert-butyl peroxy-2-ethylhexyl monocarbonate (Perbutyl E), tert-hexyl peroxybenzoate (Perhexyl Z), tert-butyl peroxyacetate (Perbutyl A), a mixture of tert-butyl peroxy-3-methylbenzoate and tert-butyl peroxybenzoate (Perbutyl ZT), tert-butyl peroxybenzoate (Perbutyl Z), tert-butyl peroxyallyl monocarbonate (Peromer AC), 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone (BTTB-25), 2,3-dimethyl-2,3-diphenylbutane (NOFMER BC-90), etc. Among them, dialkyl-type substances are preferred. In addition, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane is particularly preferred. The type and amount of organic peroxides are usually selected in consideration of the amount of active -OO-, decomposition temperature, etc.
[0171] In addition, as the cross-linking aid that can be used at this time, any compound that is reactive with peroxide radicals and polymer radicals can be used, and examples include polyfunctional compounds having functional groups such as -CH=CH2, -CH2CH=CH2, -CF=CF2, -C(CF3)=CF2, -C(CH3)=CF2, -CF=CF(CF3), -CF=CF(CH3), -C(C6H5)=CF2, -CF=CF(C6H5), -CH=CF2, -CF=CHF, -C(CF3)=CHF, -CF=CH(CF3), and -CH=CF(CF3) ("C6H5" in each formula represents a phenyl group). Specific examples include triallyl cyanurate, triallyl isocyanurate (TAIC), 1,3,5-triacryloylhexahydro-1,3,5-triazine, triallyl trimellitate, N,N'-n-phenylene bismaleimide, diallyl terephthalate, diallyl phthalate, tetraallyl terephthalamide, triallyl phosphate, bismaleimide, fluorinated triallyl isocyanurate (1,3,5-tris(2,3,3-trifluoro-2-propenyl)-1,3,5-triazine-2,4,6-trione), tris(diallylamine)-s-triazine, triallyl phosphite, N,N-diallylacrylamide, and 1,6-divinyldodecafluorohexane.
[0172] In addition, as a crosslinking auxiliary agent used together with the peroxide crosslinking agent, the general formula (31) can also be mentioned:
[0173] [Chemistry 2]
[0174]
[0175] (In the formula, 6 R 31 are each independently H, a halogen atom, or an optionally halogenated group having 1 to 5 carbon atoms which may be interposed with an ether bond, 31 It is a compound represented by a linear or branched chain having 1 to 18 carbon atoms and optionally containing a hetero atom, and optionally halogenated alkylene, cycloalkylene or (per)fluoropolyoxyalkylene.
[0176] Examples of the compound represented by the general formula (31) include the compound represented by the general formula (32), the compound represented by the general formula (33), the compound represented by the general formula (34), and the like.
[0177] General formula (32):
[0178] [Chemistry 3]
[0179]
[0180] (wherein, j is an integer of 2 to 10, preferably an integer of 4 to 8, and 4 R 32 Each is independently H, F, or an alkyl group or a (per)fluoroalkyl group having 1 to 5 carbon atoms.
[0181] General formula (33):
[0182] [Chemistry 4]
[0183]
[0184] (Where Y 31 Each is independently F, Cl or H, Y 32 Each independently is F, Cl, H or OR 33 (Here, R 33 is a branched or straight chain alkyl group which may be substantially or completely fluorinated or chlorinated), Z 33 is a divalent group having 2 to 10 carbon atoms which may be interposed with an ether bond and may be fluorinated, preferably Z 33 -(CF2) where m is an integer from 3 to 5 m - group, the compound represented by the general formula (33) is preferably F2C=CF-O-(CF2)5-O-CF=CF2.)
[0185] General formula (34):
[0186] [Chemistry 5]
[0187]
[0188] (Where Y 31 , Y 32 and Z 33 As mentioned above, R 34 Each is independently H, F, or an alkyl group or a (per)fluoroalkyl group having 1 to 5 carbon atoms.
[0189] As the crosslinking aid used together with the crosslinking agent or the peroxide crosslinking agent, there can also be mentioned at least one compound having the general formula (35):
[0190] [Chemistry 6]
[0191]
[0192] (Where R 35 ~R 37 are each independently a hydrogen atom, a fluorine atom, an alkyl group, a fluoroalkyl group, or a substituted or unsubstituted aryl group, R 35 ~R 37 At least one of them is a fluorine atom or a group containing a fluorine atom. m is an integer of 1 to 5. When m is 2 or more, m R 35 ~R 37 They may be the same or different. A compound having a structure represented by (a) a hydrogen atom of a benzene ring may or may not have a substituent. When m is 1, it is preferred that there are two or more of the structure.
[0193] Examples of the compound having a structure represented by the general formula (36) include the compound represented by the general formula (36), the compound represented by the general formula (37), and the like.
[0194] General formula (36):
[0195] [Chemistry 7]
[0196]
[0197] (Where R 35 ~R 37 As described above. p is an integer from 0 to 2, and n is an integer from 2 to 6.)
[0198] General formula (37):
[0199] [Chemistry 8]
[0200]
[0201] (Where R 35 ~R 37 As above.38 is a single bond, -SO2-, -O-, -S-, -CO-, a heteroatom-containing group, a substituted or unsubstituted alkylene group, a substituted or unsubstituted cycloalkylene group, or a substituted or unsubstituted arylene group. m is an integer from 1 to 5. These groups may be partially or fully fluorinated.
[0202] The heteroatom-containing group is not particularly limited as long as it is a divalent group containing a heteroatom. Examples of the heteroatom include an oxygen atom, a nitrogen atom, a sulfur atom, a boron atom, and a phosphorus atom.
[0203] Examples of the crosslinking agent used for the polyol crosslinking include polyol compounds such as bisphenol A and bisphenol AF.
[0204] Examples of the crosslinking agent used for the polyamine crosslinking include polyamine compounds such as 1,6-hexanediamine carbamate, N,N′-dicinnamylidene-1,6-hexanediamine, and 4,4′-bis(aminocyclohexyl)methane carbamate.
[0205] Examples of the crosslinking agent used in oxazole crosslinking, imidazole crosslinking, and thiazole crosslinking include bisdiaminophenyl-based crosslinking agents represented by general formula (41), diaminophenol-based crosslinking agents, bisaminothiophenol-based crosslinking agents, bisaminohydrazone-based crosslinking agents represented by general formula (42), bisaminohydrazone-based crosslinking agents represented by general formula (43), bisamide oxime-based crosslinking agents represented by general formula (44), and compounds represented by general formula (45).
[0206] General formula (41):
[0207] [Chemistry 9]
[0208]
[0209] (Where R 41 is -SO2-, -O-, -CO-, an alkylene group having 1 to 6 carbon atoms, a perfluoroalkylene group having 1 to 10 carbon atoms, or a single bond, or
[0210] [Chemistry 10]
[0211]
[0212] The group shown, R 42 and R 43 One of them is -NH2 and the other is -NHR 44 , -NH2, -OH or -SH, R 44 is a hydrogen atom, a fluorine atom or a monovalent organic group, preferably R 42 -NH2, R 43 NHR 44Preferred specific examples of the alkylene group having 1 to 6 carbon atoms include methylene, ethylene, propylene, butylene, pentylene, hexylene, and the like. Preferred specific examples of the perfluoroalkylene group having 1 to 10 carbon atoms include
[0213] [Chemistry 11]
[0214]
[0215] It should be noted that these compounds are known as examples of bisdiaminophenyl compounds in Japanese Patent Publication No. 2-59177, Japanese Patent Publication No. 8-120146, etc.
[0216] [Chemistry 12]
[0217]
[0218] (R 41 As mentioned above, R 45 Each independently represents any one of the following groups.)
[0219] [Chemistry 13]
[0220]
[0221] General formula (43):
[0222] [Chemistry 14]
[0223]
[0224] (Where Rf 41 It is a perfluoroalkylene group having 1 to 10 carbon atoms. )
[0225] General formula (44):
[0226] [Chemistry 15]
[0227]
[0228] (In the formula, n is an integer from 1 to 10.)
[0229] General formula (45): HN=CR 45 R 46
[0230] (Where R 45 Selected from H, NH2 and NHR 47 In the group composed of 46 Selected from Ph, SO2H, NR 48 R 49 , 2-pyridine and CH2CONH2, R 47Selected from the group consisting of Ph, NH2 and CN, R 48 is selected from the group consisting of H, NHPh, CH2CONH2, a linear alkyl group having 1 to 8 carbon atoms, and a branched alkyl group having 1 to 8 carbon atoms, and R 49 Selected from Ph, COOC(CH3)3, NH2, CH2COOH, CSNH2, CNHNH3 + Cl - , p-phenyl CN,
[0231] [Chemistry 16]
[0232]
[0233] and COPh. )
[0234] These diaminophenol-based crosslinking agents, bisaminothiophenol-based crosslinking agents, or bisdiaminophenyl-based crosslinking agents have been used in crosslinking systems with cyano groups as crosslinking points, but react with both carboxyl groups and alkoxycarbonyl groups to form oxazole rings, thiazole rings, and imidazole rings to provide crosslinked products.
[0235] In addition, the crosslinking agent may also be a compound of the general formula (46): X 41 -(CH2) n -R 50 -(CH2) m -X 41 (Where X 41 are each independently an alkynyl group, a nitrile group or Y 41 P N3(Y 41 is SO, SO2, C6H4 or CO, p is 0 or 1), n and m are independently integers of 1 to 4, R 50 Freedom to choose
[0236] i) a fluoroalkylene group having 3 to 10 carbon atoms,
[0237] ii) a fluoroalkyleneoxy group having 3 to 10 carbon atoms,
[0238] iii) substituted arylene,
[0239] iv) an oligomer comprising copolymerized units of vinylidene fluoride and perfluoro(methyl vinyl ether),
[0240] v) an oligomer comprising copolymerized units of vinylidene fluoride and hexafluoropropylene,
[0241] vi) oligomers comprising copolymerized units of tetrafluoroethylene and perfluoro(methyl vinyl ether) and
[0242] vii) a crosslinking agent as shown in the group consisting of oligomers comprising copolymerized units of tetrafluoroethylene and hydrocarbon olefins. The crosslinking agent is preferably used together with a perfluoroelastomer having a nitrile group, an azide group, a sulfonyl azide group, a carbonyl azide group or an alkyne group. For example, the nitrile group of the perfluoroelastomer reacts with the azide group of the crosslinking agent to form a tetrazole ring to provide a crosslinked product.
[0243] Particularly preferred crosslinking agents include compounds having two or more 3-amino-4-hydroxyphenyl groups or 3-amino-4-mercaptophenyl groups, or general formula (47):
[0244] [Chemistry 17]
[0245]
[0246] (Where R 41 , R 42 and R 43 As described above), specifically, for example, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (common name: bis(aminophenol) AF), 2,2-bis(3-amino-4-mercaptophenyl)hexafluoropropane, tetraaminobenzene, bis-3,4-diaminophenylmethane, bis-3,4-diaminophenyl ether, 2,2-bis(3,4-diaminophenyl)hexafluoropropane, 2,2-bis[3-amino-4-(N-phenylamino) Hexafluoropropane, 2,2-bis[3-amino-4-(N-methylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-ethylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-propylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-perfluorophenylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-benzylamino)phenyl]hexafluoropropane, etc.
[0247] Among these, as the crosslinking agent, 2,2-bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane is preferred from the viewpoint of heat resistance, steam resistance, amine resistance, and good crosslinking properties.
[0248] The content of at least one selected from the group consisting of an inorganic nitride, an organic tin compound, an ammonia generating compound and a crosslinking agent is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5.0 parts by mass, further preferably 0.2 to 2.0 parts by mass, and particularly preferably 0.3 to 1.0 parts by mass, based on 100 parts by mass of the perfluoroelastomer.
[0249] The above-mentioned composition can be prepared by mixing the above-mentioned components using a common polymer processing machine, such as an open mill, a Banbury mixer, a kneader, etc. In addition, it can also be prepared by using a method using a closed mixer. The above-mentioned composition can be suitably used as a molding material for cross-linking molding to obtain a cross-linked product.
[0250] <Crosslinked products>
[0251] The composition of the present invention is crosslinked to obtain a crosslinked product. The crosslinked product of the present invention has excellent durability against O2 plasma and durability against CF4 plasma, and has a small compression set even when used at a high temperature exceeding 300°C.
[0252] The cross-linked product of the present invention preferably has a compression set of 50% or less, more preferably 46% or less, when placed at 300°C for 70 hours at a compression rate of 25%. The compression set can be calculated by placing the cross-linked product at 300°C for 70 hours, further at 70°C for 24 hours, releasing the compression, placing at 20°C for 30 minutes, and measuring the thickness of the cross-linked product before and after compression.
[0253] As a method for obtaining a crosslinked product from a composition, there can be mentioned a method of obtaining a preform by molding the above composition as a molding material and then crosslinking the preform. The method for obtaining a preform from the above composition can be a common method, and can be carried out by a known method such as a method of heating and compressing with a mold, a method of pressing into a heated mold, and a method of extruding with an extruder. In the case of extruded products such as hoses or wires, a crosslinked product can be obtained by heating and crosslinking with steam or the like after extrusion.
[0254] The crosslinking can be performed in the order of primary crosslinking and secondary crosslinking. The primary crosslinking is preferably performed at 150°C to 250°C for 5 minutes to 120 minutes, more preferably at 170°C to 200°C for 5 minutes to 60 minutes. As the crosslinking means, known crosslinking means can be used, for example, press crosslinking, etc.
[0255] The secondary crosslinking is preferably carried out at 200°C to 320°C for 2 hours to 48 hours, more preferably at 250°C to 310°C for 5 hours to 24 hours. In addition, the temperature may be varied within this temperature range. As a crosslinking means, known crosslinking means may be used, for example, oven crosslinking may be cited. As a crosslinking atmosphere, an atmospheric atmosphere or an inert atmosphere such as nitrogen may be cited.
[0256] The crosslinked product of the present invention can be suitably used as a sealing material for semiconductor manufacturing equipment that particularly requires heat resistance, especially semiconductor manufacturing equipment that performs high-density plasma irradiation. Examples of the above-mentioned sealing material include O-rings, square rings, gaskets, sealing pads, oil seals, bearing seals, lip seals, etc.
[0257] In addition, it can be used as various polymer products used in semiconductor manufacturing equipment, such as diaphragms, tubes, hoses, various rubber rollers, belts, etc. In addition, it can also be used as a coating material and a lining material.
[0258] It should be noted that the semiconductor manufacturing equipment referred to in the present invention is not particularly limited to equipment for manufacturing semiconductors, but broadly includes all manufacturing equipment used in the semiconductor field requiring high cleanliness, such as equipment for manufacturing liquid crystal panels or plasma panels, for example, the following equipment can be cited.
[0259] (1) Etching equipment
[0260] Dry etching equipment
[0261] Plasma etching equipment
[0262] Reactive ion etching equipment
[0263] Reactive ion beam etching equipment
[0264] Sputtering Etching Equipment
[0265] Ion beam etching equipment
[0266] Wet etching equipment
[0267] Ashing device
[0268] (2) Cleaning device
[0269] Dry Etching Cleaning Equipment
[0270] UV / O3 cleaning device
[0271] Ion beam cleaning device
[0272] Laser beam cleaning device
[0273] Plasma cleaning device
[0274] Gas Etching Cleaning Device
[0275] Extraction and cleaning device
[0276] Soxhlet extraction cleaning device
[0277] High temperature and high pressure extraction and cleaning device
[0278] Microwave extraction cleaning device
[0279] Supercritical extraction cleaning device
[0280] (3) Exposure device
[0281] Lithography Machine
[0282] Coating machine and developer
[0283] (4) Grinding device
[0284] CMP equipment
[0285] (5) Film forming device
[0286] CVD equipment
[0287] Sputtering device
[0288] (6) Diffusion and ion implantation equipment
[0289] Oxidation diffusion device
[0290] Ion implantation device
[0291] The crosslinked product of the present invention can exhibit excellent performance as a sealing material for, for example, a CVD device, a plasma etching device, a reactive ion etching device, an ashing device, or an excimer laser exposure device.
[0292] Although the embodiments have been described above, it will be appreciated that various modifications may be made to the embodiments and details without departing from the spirit and scope of the claims.
[0293] Example
[0294] Next, embodiments of the present invention will be described with reference to examples, but the present invention is not limited to these examples.
[0295] Each numerical value in the examples was measured by the following method.
[0296] (Composition of perfluoroelastomer)
[0297] pass 19 It was determined by F-NMR analysis.
[0298] (Mooney viscosity of perfluoroelastomer)
[0299] The viscosity was measured at 170° C. in accordance with JIS K6300 using a Mooney viscometer MV2000 E manufactured by ALPHA TECHNOLOGIES.
[0300] (BET specific surface area of filler (nitrogen adsorption method, water vapor adsorption method))
[0301] The BET specific surface area of the filler determined by the nitrogen adsorption method was determined by the BET flow method (single point method) using nitrogen gas and a mixed gas (nitrogen 30% + helium 70%) using a fully automatic BET specific surface area measuring apparatus Macsorb HM-1208 manufactured by Mountech.
[0302] The BET specific surface area of the filler obtained by the water vapor adsorption method is calculated as follows: After the filler is vacuum degassed at 100°C for 3 hours, the adsorption isotherm of water vapor at 25°C is calculated using the high-precision gas / vapor adsorption measuring device BELLSORP-maxII manufactured by Microtrac BEL, and the isotherm is analyzed by the BET method.
[0303] (Ratio (water vapor / nitrogen))
[0304] The ratio (water vapor / nitrogen) is calculated from the BET specific surface area of the filler measured above according to the following formula: A filler having a high ratio (water vapor / nitrogen) has a high hydrophilicity.
[0305] Ratio (water vapor / nitrogen) (%) = (BET specific surface area determined by water vapor adsorption method) / (BET specific surface area determined by nitrogen adsorption method) × 100
[0306] (Graphite content (weight reduction ratio of filler))
[0307] The graphite content was determined by heating the filler at 10° C. / min to 1000° C. in air using a differential thermogravimetric simultaneous measuring apparatus STA7200 manufactured by Hitachi High-Tech Science Co., Ltd., and was the value at which the weight loss was the largest.
[0308] (Bulk density of filler)
[0309] 5 g of the powder was placed in a 100 ml graduated cylinder (inner diameter 28 mm), and the scale was read after tapping 20 times from a height of 2 cm to calculate the volume.
[0310] (Average particle size of filler)
[0311] The specific surface area (BET value) obtained using the fully automatic BET specific surface area measuring device Macsorb HM-1208 manufactured by Mountech Co., Ltd. is calculated from the average particle size (nm) = 6000 / ((specific surface area (m 2 / g)×true density (g / cm 3 The true density of silicon carbide is 3.22 g / cm 3 .
[0312] (X-ray photoelectron spectroscopy)
[0313] The surface element analysis of the filler (SiC particles) was performed using an X-ray photoelectron spectroscopy analyzer ESCA-3400 (manufactured by Shimadzu Corporation). The measurement was performed with the filler attached to the carbon tape. The measurement conditions were X-ray: Mg-Kα ray, 10 mA, 8 kV, measurement area: Conducted. Peak separation processing was performed using data analysis software (Vision2 (VisionProcessing)). Background processing was performed using the Linear method, and peak separation used curve fitting based on the nonlinear least squares method. The structure of the spectrum was divided into a total of 4 peaks for fitting. For the C1s peak, the positions of the peaks were 283.5±0.5eV, 284.8±0.6eV, 286.0±0.5eV, and 289.1±0.5eV in order from small to large binding energy. The peak of 283.5±0.5eV was taken as the peak derived from SiC, and the peak of 284.8±0.6eV was taken as the peak derived from graphite. Based on the results of the peak separation processing, the ratio of the area of the peak belonging to graphite to the area of the peak belonging to SiC (peak area of graphite / peak area of SiC) was calculated.
[0314] (Compression set)
[0315] The compression set was measured according to the method described in ASTM D395 or JIS K6262. The O-rings prepared in Examples and Comparative Examples were compressed at room temperature to a compression rate of 25% using a compression device (O-rings with a thickness (wire diameter) of 3.5 mm were compressed to a thickness of 2.625 mm).
[0316] Next, the compression device with the compressed O-ring fixed thereon is placed in an electric furnace and placed at 300°C for 70 hours or 168 hours, and then the compression device is taken out of the electric furnace. Thereafter, the compression device with the compressed O-ring fixed thereon is placed in another electric furnace and placed at 70°C for 24 hours. The O-ring is removed from the compression device and placed in a constant temperature room at 23°C for 30 minutes, and the thickness (t2) of the O-ring is measured. The compression set is calculated using the following formula.
[0317] Compression set (%) = (t0-t2) / (t0-t1) × 100
[0318] t0: original thickness of O-ring (mm)
[0319] t1: Thickness of spacer (mm)
[0320] t2: Thickness of the O-ring after compression test (mm)
[0321] In the above test, t0 = 3.5 mm, t1 = 2.625 mm.
[0322] (Plasma resistance (weight reduction rate of cross-linked product before and after plasma treatment))
[0323] The O-rings (P24 size) prepared in the examples and comparative examples were placed in a processing chamber. Plasma generated by a free radical generator was introduced into the processing chamber, and the O-rings were irradiated with plasma under the following plasma irradiation conditions. The ICP plasma weight reduction rates of O2 and CF4 were calculated from the mass of the O-rings before and after plasma irradiation.
[0324] (Plasma irradiation conditions)
[0325] Free radical generator: ICP high-density plasma device (RIE-101iPH manufactured by SAMCO)
[0326] Gas flow rate: 16sccm
[0327] Power: 400W
[0328] Pressure: 2.66Pa
[0329] Irradiation time: 1 hour
[0330] (Plasma resistance (particle generation))
[0331] In the same manner as above, an O-ring (size P24) was irradiated with plasma. The mass of the O-ring after plasma irradiation was measured, and then the O-ring after plasma irradiation was wiped with a nonwoven fabric impregnated with ethanol to remove the particles on the surface, and then dried in an oven at 150°C for 1 hour, and the mass of the O-ring was measured again. The difference in mass before and after wiping is equivalent to the mass of the surface particles. The ratio of the mass of the surface particles to the mass before wiping (the amount of particles generated) was calculated.
[0332] The following materials were used in Examples and Comparative Examples.
[0333] Perfluoroelastomer:
[0334] TFE / PMVE / CF2=CFOCF2CF(CF3)OCF2CF2CN=59.3 / 39.9 / 0.8 (mol%), Mooney viscosity ML(1+20)(170°C)=66
[0335] Crosslinking agent:
[0336] 2,2-Bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane
[0337] filler
[0338] Filler 1~4: Graphite coated silicon carbide
[0339] Filler 5: Silicon carbide
[0340] Filler 6: Silicon carbide (DU A-1 manufactured by Showa Denko K.K.)
[0341] Table 1 shows the physical properties of each filler.
[0342] [Table 1]
[0343] Table 1
[0344] Packing 1 Packing 2 Packing 3 Packing 4 Packing 5 Packing 6 <![CDATA[BET specific surface area (nitrogen adsorption method) m 2 / g]]> 48.9 38.1 71.0 78.3 55.4 9.9 <![CDATA[BET specific surface area (water vapor adsorption method) m 2 / g]]> 6.44 4.25 8.06 10.28 6.22 6.02 Ratio (water vapor / nitrogen) % 13.17 11.16 11.35 13.13 11.20 61.10 Graphite content mass% 7.87 8.41 0 0.76 0 0 <![CDATA[Bulk density g / cm 3 > 0.13 0.29 0.16 0.14 0.06 0.69 Average particle size nm 38 49 26 24 34 189 Area of the peak derived from silicon carbide (SiC) 22 25 31 26 56 58 The area of the peak derived from graphite (C) 47 39 30 46 31 35 Ratio (Area (C) / Area (SiC)) 2.14 1.56 0.97 1.77 0.55 0.60
[0345] Examples 1 to 4, Comparative Examples 1 to 2
[0346] 100 parts by mass of the perfluoroelastomer, 15 parts by mass of the filler, and 0.8 parts by mass of the crosslinking agent were kneaded using an open roll mill to prepare a composition.
[0347] The obtained composition was cross-linked by pressurizing at 180°C for 30 minutes, and further cross-linked in an air oven at 290°C for 18 hours to produce an O-ring of size P24. The obtained O-ring was used to measure the compression set, ICP plasma weight loss rate, and particle generation amount by the above method. The results are shown in Table 2.
[0348] [Table 2]
[0349] Table 2
[0350]
Claims
1. A composition comprising a perfluoroelastomer and a filler, wherein: The filler contains silicon carbide and graphite, and the ratio of the area (C) of the peak derived from the graphite in the filler to the area (SiC) of the peak derived from the silicon carbide in the filler measured by X-ray photoelectron spectroscopy (XPS), i.e., area (C) / area (SiC) is greater than 0.
7.
2. The composition according to claim 1, wherein The BET specific surface area of the filler obtained by nitrogen adsorption method was 15 m 2 / g~200m 2 / g.
3. The composition according to claim 1 or 2, wherein The ratio of the BET specific surface area of the filler obtained by a water vapor adsorption method to the BET specific surface area of the filler obtained by a nitrogen adsorption method, that is, water vapor / nitrogen, is 1% to 60%.
4. The composition according to any one of claims 1 to 3, wherein The bulk density of the filler is 0.10 g / cm 3 above.
5. The composition according to any one of claims 1 to 4, wherein The content of the filler is 0.1 parts by mass to 100 parts by mass based on 100 parts by mass of the perfluoroelastomer. 6 . The composition according to claim 1 , further comprising at least one selected from the group consisting of an inorganic nitride, an organic tin compound, a compound that generates ammonia, and a crosslinking agent. 7 . A cross-linked product obtained by cross-linking the composition according to claim 1 . The cross-linked product according to claim 7 , which is a sealing material.
9. The cross-linked product according to claim 7 or 8, wherein The compression set measured at 300°C for 70 hours at a compression rate of 25% was 50% or less.
Citation Information
Patent Citations
Fluoroelastomer composition
JP1996120146A
Fluorine-containing elastomer composition
JP1997111081A
Process for producing ultrafine particles
JP2007138287A
Method for producing silicon / silicon carbide composite fine particle
JP2011213524A
Crosslinkable fluorine-containing elastomer composition and molded articles made from the composition
JP2012509975A