Sliding material
By adding Cr-Fe-Si-based intermetallic compounds to the brass alloy, the nanoindentation hardness is within a specific range, and the inadequate hardness verification of Mn-Si-based intermetallic compounds in the brass matrix in the prior art is solved. The problem of this has achieved the improvement of wear resistance and low friction of sliding materials.
Patent Information
- Application Number
- CN202380028231.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art has not fully verified the accurate chemical composition, crystallization form and hardness of Mn-Si intermetallic compounds on friction wear in brass matrix, resulting in improved wear resistance but not clear enough.
Using brass alloy as the matrix, Cr-Fe-Si intermetallic compounds were added, and the hardness of the crystalline region was ensured by measuring the nano-indentation hardness to ensure that the hardness of the crystalline region was above 20GPa and below 28GPa. The matrix that dissolved brass was developed and only Cr-Fe- remained The corrosion method of Si-based intermetallic compounds is observed to verify the friction and wear effect.
It achieves the improvement of sliding characteristics of sliding materials, provides excellent wear resistance and low friction, and is suitable for harsh friction environments.
Smart Images

Figure CN118900923A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to sliding materials. Background Art
[0002] In order to improve the wear resistance, sliding materials are known in which various intermetallic compounds (such as silicide) are crystallized on a brass alloy matrix.
[0003] Patent Document 1 discloses a wear-resistant copper alloy, wherein the weight ratio of Fe to Mn is 0.3 to 14, and the content is 1 to 15 wt%. This ternary compound has excellent wear resistance compared to conventional compounds containing Mn5Si3 and Fe3Si. Patent Document 1 only discloses that adding Cr has a dispersing effect.
[0004] Patent Document 2 discloses Mn silicide of brass alloy. In Patent Document 2, Cr or Zr or a compound thereof acts as a nucleating agent for silicide precipitates, and the addition thereof suppresses the fine precipitation of eutectic of silicide. That is, in Patent Document 2, the crystal form of Mn silicide can be changed by adding a trace amount of Cr or Zr.
[0005] Patent Document 3 discloses that in a sintered material composed of a brass alloy, Cu, Zn, Al, and Si are used as base metals, and Ti, Zr, V, Cr, and other additives are used as selective elements to contribute to microstructural refinement and grain boundary strengthening. Since the sintered material using surface vacancies does not have a process of completely dissolving and alloying the additive components as in the molten material, even if the components are the same, the structure is non-uniform and different from that of the molten material.
[0006] Patent document 4 discloses the following material: the brass matrix is limited to the β phase, the composition of the Fe-Mn-Si intermetallic compound is assumed to be composed of Mn5Si3 and Fe3Si, the amount of Fe, Mn and Si added is limited, and the area ratio of the compound is made 3 to 20%.
[0007] Patent Document 5 discloses a material in which a brass matrix is limited to a β phase and contains Fe-based silicides such as Fe—Cr—Si-based intermetallic compounds, but the details of the compounds are not clear.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent document 1: Japanese Patent Application Publication No. 60-114545;
[0011] Patent document 2: Japanese Patent Application Publication No. 61-41738;
[0012] Patent document 3: Japanese Patent Application Laid-Open No. 1-252745;
[0013] Patent Document 4: Japanese Patent Application Publication No. 2010-159443;
[0014] Patent document 5: Japanese Patent Application Publication No. 2010-265500. Summary of the invention
[0015] Technical problem to be solved by the invention
[0016] As shown in the prior art literature, as the friction and wear environment becomes more severe, the effective use of Mn-Si intermetallic compounds, improved Mn-Fe-Si intermetallic compounds, etc. in the brass matrix contributes to the improvement of wear resistance. However, the exact chemical composition, crystal morphology, hardness, etc. of the intermetallic compounds have not been fully verified for their effects on friction and wear.
[0017] The present invention has been made to solve the problems of the prior art, and an object of the present invention is to provide a sliding material having improved sliding properties.
[0018] Means for solving technical problems
[0019] The present invention is a sliding material having a matrix composed of a brass alloy and a Cr-Fe-Si based intermetallic compound contained in the matrix, wherein the nanoindentation hardness of a region where the Cr-Fe-Si based intermetallic compound is crystallized is 20 GPa or more and 28 GPa or less.
[0020] Effects of the Invention
[0021] According to the sliding material of the present invention, it is possible to provide a sliding material having improved sliding properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic cross-sectional view of a sliding material according to an embodiment.
[0023] Figure 2 is a contour plot of nanoindentation hardness.
[0024] Figure 3 is a cross-sectional diagram of nanoindentation hardness.
[0025] Figure 4 It is a schematic cross-sectional view of a sliding material of a comparative example.
[0026] Figure 5 It is a schematic cross-sectional view of a sliding material of a comparative example.
[0027] Figure 6 It is a schematic cross-sectional view of a sliding material of a comparative example.
[0028] Figure 7This is a SEM photograph of the Cr—Fe—Si based intermetallic compound according to the embodiment.
[0029] Figure 8 It is a schematic diagram showing an enlarged cross-sectional structure of a sliding material according to an embodiment.
[0030] Fig. 9 This is a schematic diagram showing an enlarged cross-sectional structure of a sliding material of a comparative example.
[0031] Fig.10 It is a schematic diagram explaining the wear of the sliding material according to the embodiment.
[0032] Fig.11 It is a figure which shows the reciprocating sliding test apparatus. DETAILED DESCRIPTION
[0033] Hereinafter, the sliding material according to the embodiment will be described in detail.
[0034] Figure 1 It is a schematic diagram showing the cross-sectional structure of the sliding material 1 according to the embodiment. Figure 1 The three-dimensional structure of the intermetallic compound is shown when viewed from a cross section perpendicular to the sliding surface 1A. The sliding material 1 includes a matrix 2 and a Cr—Fe—Si-based intermetallic compound 3 .
[0035] The base 2 is made of a brass alloy and provides the sliding material 1 with a shape and mechanical strength in accordance with the intended use.
[0036] The sliding material 1 of the embodiment includes (Cr, Fe) 3 Si as a Cr-Fe-Si intermetallic compound 3 having Cr as a main component. The Cr-Fe-Si intermetallic compound 3 typically has (Cr 0.85 Fe 0.15 )3Si structure.
[0037] The Cr-Fe-Si intermetallic compound 3 is a compound composed of Cr, Fe and Si. The Cr-Fe-Si intermetallic compound 3 of the embodiment has a structure of (Cr, Fe)3Si. Each of the Cr-Fe-Si intermetallic compounds 3 has a curved outer shape with rounded corners.
[0038] The plurality of Cr-Fe-Si intermetallic compounds 3 contained in the matrix 2 are bonded to each other, thereby having a three-dimensional structure formed by connecting a plurality of Cr-Fe-Si intermetallic compounds 3. In the sliding material of the present embodiment, the nanoindentation hardness of the region where the Cr-Fe-Si intermetallic compound 3 is crystallized is 20 GPa or more and 28 GPa or less. In addition, the definition and determination method of the hardness of the Cr-Fe-Si intermetallic compound 3 are described below.
[0039] Regarding the identification of the Cr-Fe-Si intermetallic compound 3, the atomic bonding ratio of the compound is calculated from the atomic % composition based on SEM-EDS point analysis. For example, in the case of a simple Mn silicide, it is known that the bonding ratio is Mn:Si=5:3 and the chemical structure is Mn5Si3.
[0040] The description of the intermetallic compound is the same as that of the general alloy components, and is described in order from the most abundant component, and is described as a Mn-Si intermetallic compound. Therefore, the Cr-Fe-Si intermetallic compound 3 represents a compound composed of Cr, Fe and Si with Cr as the main component.
[0041] The present inventors have confirmed that when the compound is ternary like a Mn-Fe-Si based intermetallic compound, its main structure does not change to Mn5Si3, but a part of Mn is replaced (Mn x ,Fe y ) (where x+y=1), the substitution ratio is clearly determined. That is, by using these measuring devices and introducing the concept of determining the chemical structure, the accurate chemical structure can be obtained.
[0042] Conventionally, intermetallic compounds are often evaluated based on their cross-sectional shapes. However, in the case of friction and wear, it is necessary to understand the three-dimensional crystal morphology of the compound in accordance with the progress of wear.
[0043] The present inventors have developed an etching method for dissolving the brass matrix 2 and leaving only the Cr—Fe—Si intermetallic compound 3. This allows the three-dimensional crystal morphology of the Cr—Fe—Si intermetallic compound 3 to be observed by SEM (secondary electron imaging).
[0044] This method can be used to understand the three-dimensional structure of the Cr-Fe-Si based intermetallic compound 3. In this article, the morphologies of these intermetallic compounds are compared to verify the effects they have on friction and wear.
[0045] The hardness of the Cr—Fe—Si based intermetallic compound 3 can be measured by hardness measurement using a nano indenter.
[0046] The hardness measurement using a nanoindenter is based on "ISO 14577-1Metallic materials-Instrumented indentation test for hardness and materials parameters-" and its supplementary provisions "Annex A (normative) Materials parameters determined from the force / indentation depth data set". The hardness measurement using a nanoindenter uses a HYSITRONTI980 device manufactured by BRUKER.
[0047] The measurement conditions and measurement procedure of nanoindentation hardness are shown below.
[0048] Nanoindentation measurement conditions are as follows:
[0049] Test load: 800μN
[0050] Load: 1s
[0051] Hold: 0.4s
[0052] Uninstall: 1s
[0053] The ISO description of the test conditions is as follows:
[0054] HIT=HIT8×10 -4 / 1 / 0.4 / 1(Note: ISO 14577-1AnnexA)
[0055] The measurement procedure and the method for determining the nanoindentation hardness of the Cr-Fe-Si system intermetallic compound 3 are as follows:
[0056] 1. Grind the sample surface using an ion milling device to form a smooth surface.
[0057] 2. Use SEM / EDS to confirm the components in the field of view including the Cr-Fe-Si intermetallic compound 3. Next, use the camera of the nanoindentation measuring device to confirm that it is the same field of view as the Cr-Fe-Si intermetallic compound 3. In this way, the nanoindentation measurement field of view is determined.
[0058] 3. A grid with a grid spacing of 1.5 μm was set in a 13.5 μm×13.5 μm field of view including the Cr—Fe—Si-based intermetallic compound 3. The nanoindentation hardness of a total of 100 grid points in the grid was sequentially measured under the above-mentioned nanoindentation measurement conditions.
[0059] 4. Based on the above measurement results, a contour map is obtained by connecting points of the same nanoindentation hardness with lines. Figure 2 The contour map is obtained by connecting points of equal hardness with lines. Figure 2 The peak of nanoindentation hardness is parallel to the X-axis ( Figure 2 Take the section of the contour line in D-D'). Figure 3 It is a cross-sectional view showing the hardness distribution obtained by taking a cross section of contour lines.
[0060] 5. Figure 3 In the hardness cross-sectional view, A represents the region of the matrix 2, B represents the boundary region between the matrix 2 and the Cr—Fe—Si based intermetallic compound 3, and C represents the region of the Cr—Fe—Si based intermetallic compound 3.
[0061] The nanoindentation hardness in region A of the substrate 2 is about 4 GPa. In the boundary region B between the substrate 2 and the Cr-Fe-Si intermetallic compound 3, the Cr-Fe-Si intermetallic compound 3 is crystallized, and thus has a greater hardness than the substrate 2. The hardness increases sharply from the peripheral portion close to the substrate 2. In region C of the Cr-Fe-Si intermetallic compound 3, the nanoindentation hardness of the central portion is relatively flat. Figure 2 The nanoindentation hardness is 19.5 GPa or more and 24.4 GPa or less.
[0062] In this measurement method, the nanoindentation hardness can only obtain discrete values. Therefore, as a method of expressing the hardness of the Cr-Fe-Si system intermetallic compound 3, the high hardness region C with a flat center is regarded as the region where the Cr-Fe-Si system intermetallic compound 3 is crystallized. Then, the nanoindentation hardness of the region C is used as the hardness of the Cr-Fe-Si system intermetallic compound 3.
[0063] In addition, when determining the boundary region B, the nanoindentation hardness of a certain grid point is set to H n The nanoindentation hardness of adjacent grid points with a distance of 1.5 μm is set as H n+1 In the case of |H n+1 -H n The portion with the condition of |>6.0 GPa is defined as boundary region B, and the boundary line between regions C and B is set according to the contour line.
[0064] The region C having a hardness greater than that of the boundary region B determined in this way is regarded as a region where the Cr-Fe-Si based intermetallic compound 3 is crystallized. Figure 2 In the case of the Cr—Fe—Si-based intermetallic compound 3 shown, the nanoindentation hardness of the region C is 19.5 GPa or more and 24.4 GPa or less.
[0065] In addition, the measurement of nanoindentation hardness may also reflect multiple fields of view (for example, 5 fields of view). In this case, the nanoindentation hardness of each of fields of view 1 to field of view 5 is set from the minimum value to the maximum value as the nanoindentation hardness of the Cr-Fe-Si intermetallic compound 3. In addition, the measurement steps to determination methods of the nanoindentation hardness of other intermetallic compounds are also performed in the same process.
[0066] The sliding material 1 of the embodiment improves sliding properties by the three-dimensional bonded structure of particles of the Cr—Fe—Si-based intermetallic compound 3 and the nanoindentation hardness.
[0067] The sliding material 1 of the embodiment was compared with the sliding materials of the comparative example in terms of composition, structure, three-dimensional structure, and nanoindentation hardness, and the effect of the sliding material 1 of the embodiment was confirmed.
[0068] Figure 4 Schematic diagram of the three-dimensional shape of the sliding material including the Mn-Si system intermetallic compound of the comparative example observed from the cross section. Figure 4 As shown, the Mn-Si intermetallic compound has the chemical structure of Mn5Si3, has a preferred crystal growth direction, and has a morphology in which each is separated and grows into a hexagonal needle shape.
[0069] The nanoindentation hardness of the Mn—Si intermetallic compound is 16.8 GPa. The hexagonal needle-shaped Mn silicide compound has stress concentration at the corners and therefore lacks toughness.
[0070] Mn-Si intermetallic compounds have strong crystallinity and are easily broken. They are partially broken, freed, separated, and turned into foreign matter on the friction and wear surface. At this time, problems such as rolling on the sliding surface and damaging the other material also occur, which also becomes the cause of sintering. This will become a problem especially in sliding materials used under harsh conditions.
[0071] Figure 5 This is a schematic diagram of the three-dimensional shape of a sliding material including a Mn-Fe-Si-based intermetallic compound of a comparative example observed from a cross section. Figure 5 As shown, the Mn-Fe-Si intermetallic compound has a chemical structure of (Mn,Fe)5Si3. The Mn-Fe-Si intermetallic compound has a preferred growth crystal direction like the Mn-Si intermetallic compound, and has a morphology in which each is separated and grows into a hexagonal needle shape.
[0072] It was found that part of the Mn-Fe-Si intermetallic compound was eutecticized and changed into a granular continuous structure. In addition, the nanoindentation hardness of the Mn-Fe-Si intermetallic compound was 18.5 GPa. The nanoindentation hardness of the Mn-Fe-Si intermetallic compound was barely increased by ternary formation.
[0073] The sliding material 1 of the embodiment has a (Cr, Fe) 3 Si structure in a matrix 2 of a brass-based cast alloy, has a three-dimensional structure consisting of a curved surface with rounded corners and partially connected to a Cr-Fe-Si-based intermetallic compound 3, and the nanoindentation hardness of the region C of the Cr-Fe-Si-based intermetallic compound 3 has a hardness of 20 GPa or more and 28 GPa or less. The sliding material 1 of the embodiment has excellent wear resistance and low friction due to the Cr-Fe-Si-based intermetallic compound 3.
[0074] Among the intermetallic compounds composed of Cr, Fe, and Si, there is a Cr-Fe-Si intermetallic compound 3 having Cr as the main component, namely (Cr,Fe)3Si (specifically, (Cr 0.85 Fe 0.15 )3Si), Fe-Cr-Si intermetallic compounds with Fe as the main component (Fe,Cr)3Si (specifically, (Fe 0.85 Cr 0.15 These two intermetallic compounds show completely different morphologies.
[0075] Figure 6 The morphology of Fe-Cr-Si intermetallic compounds is shown. 0.85 Cr 0.15 Fe-Cr-Si intermetallic compounds are compounds in which part of Cr (85%) in the Cr3Si compound is replaced by Fe which is also a transition metal.
[0076] Figure 7 3 is a SEM photograph showing the three-dimensional structure of the Cr-Fe-Si intermetallic compound 3. Figure 7 As shown, the Cr-Fe-Si based intermetallic compound 3 is composed of curved surfaces with rounded corners and has a three-dimensionally connected morphology.
[0077] The shape of this three-dimensional connection is not Figure 4 The comparative example shown is a form that provides excellent friction performance. On the other hand, the Fe-Cr-Si intermetallic compound is finely dispersed and crystallized in a block shape, so its contribution to the friction characteristics is small.
[0078] The Cr-Fe-Si intermetallic compound 3 and the Fe-Cr-Si intermetallic compound have a tendency to crystallize simultaneously. In order to effectively utilize only the Cr-Fe-Si intermetallic compound, the inventors tried to separate and solidify the two silicides. As a result, by controlling the solidification conditions, the Cr-Fe-Si intermetallic compound 3 and the Fe-Cr-Si intermetallic compound were successfully separated and solidified. As a result, the excellent friction and wear characteristics of the Cr-Fe-Si intermetallic compound can be grasped, and the embodiment can be achieved.
[0079] Even if the intermetallic compound has the same Cr, Fe, and Si as constituent components, the morphology and hardness of the Cr-Fe-Si intermetallic compound 3 and the Fe-Cr-Si intermetallic compound are completely different, and as a result, the friction and wear performance brought by the hard compound is different. In the embodiment, for the purpose of effectively utilizing the Cr-Fe-Si intermetallic compound 3, the Cr-Fe-Si intermetallic compound 3 is characterized in that it has a three-dimensional structure in which Cr is the main component and is composed of curved surfaces with rounded corners and partially connected.
[0080] In the brass-based cast alloy, wear resistance and low friction (low μ property) were evaluated according to the tribological basic formula (1).
[0081] μ=τ0 / P H ···(1)
[0082] Where, μ: friction coefficient, τ0: shear force of lubricating material, P H : Hardness (load / area).
[0083] The friction coefficient μ is proportional to the shear force of the lubricant and inversely proportional to the hardness of the substrate. H It is the value obtained by dividing the load by the contact area. In order to reduce the friction coefficient μ, it is necessary to increase the hardness of the intermetallic compound, which is the load point during friction, and reduce the contact area of the intermetallic compound.
[0084] That is, the shape of the compound is preferably close to a spherical shape so as to reduce the contact area, and if the compound is a hard compound, the friction coefficient can be reduced.
[0085] Figure 8 The Cr-Fe-Si intermetallic compound 3 of the embodiment is shown. Figure 8 As shown, the Cr-Fe-Si based intermetallic compound 3 of the embodiment is in the form of a compound composed of hard, rounded curved surfaces connected to each other.
[0086] Therefore, it can be said that the Cr—Fe—Si based intermetallic compound 3 of the embodiment is hard, has a small friction surface, and has an increased heat dissipation area, which is a form capable of reducing the friction coefficient.
[0087] Fig. 9 The Mn-Fe-Si intermetallic compound of the comparative example is shown. Fig. 9 As shown, the Mn—Fe—Si based intermetallic compound of the comparative example is square and the compounds are independent and not connected.
[0088] The effect of the Cr-Fe-Si intermetallic compound 3 of the embodiment is that, according to the above tribological basic formula (1), P H The increase in (hardness) reduces the friction coefficient, and the interposition of the lubricant reduces the friction work represented by μ×load×speed, thereby reducing the generation of frictional heat and exerting a low friction effect.
[0089] The wear amount (V) of the sliding material is expressed by equation (2).
[0090] V=Z(P / P H )L···(2)
[0091] The wear volume (V) is proportional to the wear coefficient Z, load P, and friction distance L, and is also proportional to the hardness P. H Therefore, by increasing the hardness of the compound that crystallizes in the soft brass alloy, the amount of wear can be reduced.
[0092] The nanoindentation hardness of region C of the Cr—Fe—Si based intermetallic compound 3 of the embodiment is 20 GPa to 28 GPa, and is a structure excellent in wear resistance.
[0093] During friction, the intermetallic compound becomes a load point, generating strong friction heat. This friction heat is dissipated through the interface between the intermetallic compound and the copper alloy matrix. Therefore, by connecting the compounds three-dimensionally, the surface area of the intermetallic compound as a whole can be increased, and the heat dissipation efficiency can be greatly improved. In this way, the heat dissipation efficiency during friction is good, the rise of surface temperature can be prevented, and the severe friction conditions can be alleviated.
[0094] For example, when the needle-shaped Mn5Si3 compound of the comparative example crystallizes alone and becomes a load point and the friction heat increases, the temperature of the intermetallic compound rises, the compound / matrix interface softens, and there is a possibility that the compound interface becomes unstable and free.
[0095] On the other hand, the Cr-Fe-Si intermetallic compound 3 of the embodiment has a large surface area and is connected, so the heat exchange area is increased and the friction heat generated by the concentrated load can be appropriately diffused. Such a three-dimensional structure is an important element in the field of friction and wear.
[0096] The three-dimensionally connected structure plays a particularly favorable role in friction performance and wear resistance. Fig.10 As shown, even if wear occurs along the path A-A' → B-B' → CC', the Cr-Fe-Si based intermetallic compound 3 always exists, and wear resistance and low friction are continuously maintained.
[0097] Thus, the shape and continuity of the Cr-Fe-Si intermetallic compound 3 are of great significance, and as its use, it also functions effectively as a high-temperature and high-load bearing material. That is, the continuity of the Cr-Fe-Si intermetallic compound 3 can be said to be an excellent structure that promotes the formation of an optimal low-friction surface while wearing.
[0098] (Example)
[0099] Hereinafter, examples of the present invention will be described. In addition, the present invention is not limited to the following examples.
[0100] The composition of the intermetallic compound contained in the sliding materials of the examples and comparative examples is shown in Table 2. The sliding materials of the examples and comparative examples contain the intermetallic compounds shown in Table 1 in a brass-based cast alloy matrix of Cu-26Zn-5Al.
[0101] Example 1 is a sliding material in which Cr-Fe-Si intermetallic compound 3 is crystallized in the matrix. Comparative Example 1 is a sliding material in which Fe-Cr-Si intermetallic compound is crystallized in the matrix. Comparative Example 2 is a sliding material in which Mn5Si3, a so-called Mn-Si intermetallic compound, is crystallized in the matrix. Comparative Example 3 is a sliding material in which (Mn,Fe)5Si3, a so-called Mn-Fe-Si intermetallic compound, is crystallized in the matrix.
[0102] Table 1 shows the chemical formula of each intermetallic compound, the crystal form of the intermetallic compound (the shape of the intermetallic compound, the continuity (bonding, connection) of the intermetallic compound), and the nanoindentation hardness (GPa) of the region where the intermetallic compound exists. In addition, the addition amount of Si is set to 0.3%, and the addition amounts of Mn, Fe, Cr, etc. are determined according to the composition of the crystallized compound.
[0103] [Table 1]
[0104] Chemical formula shape Continuity Hardness(GPa) Example 1 <![CDATA[(Cr,Fe)3Si]]> Made of curved surfaces with rounded corners have 19.5~27.9 Comparative Example 1 <![CDATA[(Fe,Cr)3Si]]> Slightly angular none 9.5~14.3 Comparative Example 2 <![CDATA[Mn5Si3]]> Hexagonal needle none 11.4~16.8 Comparative Example 3 <![CDATA[(Mn,Fe)5Si3]]> Hexagonal needle granules Part 12.2~18.5
[0105] For any alloy, a pure Cu ingot is first melted at a melting temperature of 1100°C, a specified amount of Zn is then added to make a Cu-Zn alloy, Al is then added and melted, and then the temperature is raised to 1200°C, and a master alloy of the elements required for melting is added, and the alloy is melted and cast in a manner to obtain a specified composition, and processed into a test piece shape.
[0106] In the case of the Cr-Fe-Si intermetallic compound 3 of Example 1, a region with a nanoindentation hardness of 19.5 GPa or more and 27.9 GPa or less was observed in region C of the Cr-Fe-Si intermetallic compound 3. On the other hand, in the case of the Fe-Cr-Si intermetallic compound of Comparative Example 1, a region of 9.5 GPa or more and 14.3 GPa or less was observed. In the case of the Mn-Si intermetallic compound of Comparative Example 2 and the Mn-Fe-Si intermetallic compound of Comparative Example 3, regions of 11.4 GPa or more and 16.8 GPa or less and regions of 12.2 GPa or more and 18.5 GPa or less were observed, respectively.
[0107] Thus, the Cr—Fe—Si based intermetallic compound 3 of Example 1 is an extremely hard intermetallic compound, and the hardness has a great influence on the friction performance.
[0108] Fig.11 The following is an overview of a reciprocating sliding test device. The wear amount can be measured using a so-called pin-disc type reciprocating sliding test device. 1 in the figure represents a pressurizing device, 2 represents the test material, and 3 represents the other material. 4 is a motor that causes the other material to reciprocate. The following are test conditions.
[0109] Testing machine: reciprocating load testing machine
[0110] Sliding speed: 2m / min
[0111] Reciprocating sliding distance: 150mm
[0112] Total sliding distance: 500m
[0113] Test temperature (bearing back temperature): 100°C
[0114] ·Other material: S45C surface hardened material, surface roughness Ra3.0
[0115] Lubricant: VG32
[0116] Wear test load: 30MPa constant load
[0117] Table 2 shows the wear amount of the sliding materials of Examples and Comparative Examples.
[0118] [Table 2]
[0119] Wear loss (μm) Example 1 0.7 Comparative Example 1 3.3 Comparative Example 2 12.9 Comparative Example 3 6.9
[0120] It is found that the sliding material of Example 1 can obtain significantly superior wear resistance compared with the sliding material of Comparative Example 1 and the sliding materials of Comparative Examples 2 and 3 which are conventionally used.
[0121] This confirmed that the sliding material of the example can obtain excellent friction performance improved by crystallization of the Cr—Fe—Si based intermetallic compound 3 having excellent tribological performance in terms of crystal morphology and nanoindentation hardness.
[0122] The sliding material of the embodiment can be used in harsh sliding environment conditions such as low speed and high load, high speed rotation or corrosive environment in engineering machinery parts, automobile engine parts, gearbox parts, hydraulic parts, aircraft parts, etc. The sliding material of the embodiment is useful for applications requiring wear resistance and low friction characteristics, and can provide a sliding material with high reliability.
[0123] In addition, the structure of the sliding material and the material and composition of the composition in the embodiment are merely examples, and the present invention is not limited thereto.
Claims
1. A sliding material, characterized in that: have: a base body composed of a brass alloy; and Cr-Fe-Si system intermetallic compound, which is contained in the matrix, The nanoindentation hardness of the region where the Cr—Fe—Si based intermetallic compound is crystallized is 20 GPa or more and 28 GPa or less.
2. The sliding material according to claim 1, wherein The Cr—Fe—Si based intermetallic compound has a three-dimensional structure in which the Cr—Fe—Si based intermetallic compounds are connected.
3. The sliding material according to claim 1 or 2, wherein: The Cr—Fe—Si based intermetallic compound has a shape consisting of a curved surface with rounded corners.
4. The sliding material according to any one of claims 1 to 3, wherein The Cr—Fe—Si system intermetallic compound has a chemical structure of (Cr, Fe) 3 Si.