Positive electrode material, preparation method thereof and sodium ion battery

By coating boron oxide and metal hydroxide on the positive electrode material of the sodium ion battery to form a dense protective layer, the problem of thermal runaway in the sodium ion battery is solved and high-safe battery performance is achieved.

CN118919713APending Publication Date: 2024-11-08LIYANG HINA BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966674.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Sodium ion batteries are prone to thermal runaway during charging and discharging, resulting in overheating, rising internal pressure, or even explosion or fire. The prior art is difficult to effectively suppress this risk.

Method used

Using the positive electrode material with the chemical formula of NaNiaFebMncCu(1-a-b-c)O2·xM(OH)α·yBO3/2, the residual alkali content and resistance of the surface are controlled by coating boron oxide and metal hydroxide on the surface of the layered oxide. The proportion of the combustion agent is to use the flame retardant mechanism of the flame retardant and the high thermal conductivity and high viscosity characteristics of boron oxide to form a dense protective layer to isolate the air, achieve the self-flame retardant effect and reduce the heat diffusion temperature.

Benefits of technology

Effectively suppress the occurrence of thermal runaway, improve the safety performance and discharge specific capacity of the battery, and reduce the risk of thermal runaway.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919713A_ABST
    Figure CN118919713A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sodium-ion batteries, in particular to a positive electrode material, a preparation method thereof and a sodium-ion battery. The invention provides a positive electrode material. The chemical general formula of the positive electrode material is NaNi Fe Mn < c > Cu (1-a-b-c) O < 2 >. XM (OH) < alpha >. YBO < 3 / 2 >, in the formula, 0 < a < = 0.5, 0 < b < = 0.4, 0 < c < = 0.4, 0.8 < = a + b + c < 1, 0.005 < = x < = 0.05, 0.0001 < = y < = 0.005, the element M comprises Mg and / or Al, and alpha is the valence value of M. According to the positive electrode material disclosed by the invention, the magnesium hydroxide and / or aluminum hydroxide and other flame retardants are combined with a small amount of boron oxide, and the content of residual alkali on the surface is controlled, so that the thermal diffusion temperature is reduced and effective heat conduction is realized when thermal runaway occurs, a compact protective layer is formed to isolate air, a self-flame-retardant effect is achieved, and thermal runaway is inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art

[0002] Energy storage batteries are batteries that convert chemical energy into electrical energy. They are batteries with energy storage functions. The principle is to store electrical energy through chemical reactions, and then release electrical energy through reverse chemical reactions when needed. This principle makes energy storage batteries a very important device in power systems.

[0003] Energy storage batteries face the risk of thermal runaway during the charging and discharging process. For example, when the design limit is exceeded, excessive heat may be generated, resulting in the battery system being unable to effectively dissipate heat and thermal runaway. Thermal runaway may cause the chemical reaction inside the battery to run away, further causing serious situations such as battery overheating, increased internal pressure, and even explosion or fire.

[0004] Sodium battery is an important energy storage battery, in which the positive electrode material accounts for more than 1 / 3 of the active components of the entire battery cell. Therefore, it is crucial to develop highly safe sodium battery layered oxide positive electrode materials.

[0005] In view of this, this invention is proposed. Summary of the invention

[0006] The first object of the present invention is to provide a positive electrode material with high safety and capable of effectively suppressing the occurrence of thermal runaway.

[0007] The second object of the present invention is to provide a method for preparing a positive electrode material.

[0008] A third object of the present invention is to provide a sodium ion battery.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] The present invention provides a positive electrode material, the chemical formula of which is NaNi a Fe b Mn c Cu (1-a-b-c) O2·xM(OH) α ·yBO 3 / 2 ; Wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.005≤x≤0.05, 0.0001≤y≤0.005, M element includes Mg and / or Al, and α is the valence value of M element.

[0011] Furthermore, the positive electrode material includes a layered oxide and a coating layer coated on the surface of the layered oxide;

[0012] The layered oxide includes NaNi a Fe b Mn c Cu (1-a-b-c) O2, where 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1;

[0013] The coating layer includes boron oxide and metal hydroxide, and the metal hydroxide includes Al(OH)3 and / or Mg(OH)2.

[0014] Furthermore, the positive electrode material satisfies the following relationship:

[0015]

[0016] In the formula, J is the theoretical calculated value of the residual alkali content in the positive electrode material, and the residual alkali is sodium hydroxide and sodium carbonate; z is the molar ratio of the metal hydroxide to the layered oxide; is the proportion of the metal element in the metal hydroxide.

[0017] Furthermore, in the positive electrode material, the content of sodium hydroxide is 0.001wt% to 0.1wt%, and the content of sodium carbonate is 0.1wt% to 2.5wt%.

[0018] The present invention also provides a method for preparing the positive electrode material as described above, comprising the following steps:

[0019] calcining the layered oxide, H3BO3 and metal hydroxide to obtain the positive electrode material;

[0020] Wherein, the layered oxide includes NaNi a Fe b Mn c Cu (1-a-b-c) O2, wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1; the metal hydroxide includes Al(OH)3 and / or Mg(OH)2.

[0021] Furthermore, the calcination includes: heating to 100-350° C. and calcining for 6-18 hours.

[0022] Furthermore, the method for preparing the layered oxide comprises:

[0023] After sintering the copper-nickel-iron-manganese quaternary precursor and the sodium source, the layered oxide is obtained;

[0024] or,

[0025] The layered oxide is obtained by sintering the nickel-iron-manganese ternary precursor, the copper source and the sodium source.

[0026] Furthermore, the average particle size of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor are independently 2.5 to 8.5 μm, and the specific surface area is independently 10 to 30 m 2 / g.

[0027] Furthermore, the sintering includes: heating to 900-1000° C. and sintering for 8-24 hours.

[0028] The present invention also provides a sodium ion battery, comprising the positive electrode material as described above or the positive electrode material prepared by the method for preparing the positive electrode material as described above.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The positive electrode material of the present invention controls the residual alkali content on the surface by combining flame retardants such as magnesium hydroxide and / or aluminum hydroxide with a small amount of boron oxide, and utilizes the flame retardant mechanism of the flame retardant in combination with the high thermal conductivity and high-temperature and high-viscosity properties of boron oxide to reduce the thermal diffusion temperature and effectively conduct heat when thermal runaway occurs, forming a dense protective layer to isolate the air, achieving a self-flame retardant effect, and inhibiting the occurrence of thermal runaway. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 This is a SEM image of the positive electrode material prepared in Example 6 of the present invention.

[0033] Figure 2 This is a SEM image of the positive electrode material prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0034] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0035] In some embodiments of the present invention, a positive electrode material is provided, the chemical formula of the positive electrode material is NaNi a Fe b Mn c Cu (1-a-b-c) O2·xM(OH) α ·yBO 3 / 2 ; Wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.005≤x≤0.05, 0.0001≤y≤0.005, M element includes Mg and / or Al, and α is the valence value of M element.

[0036] In some embodiments of the present invention, the value of x may be 0.005, 0.01, 0.015, 0.02, 0.025, 0.03, 0.035, 0.04, 0.045, 0.05 or a range consisting of any two of them.

[0037] In some embodiments of the present invention, the value of y may be 0.0001, 0.0005, 0.001, 0.0015, 0.002, 0.0025, 0.003, 0.0035, 0.004, 0.0045, 0.005 or a range consisting of any two of them.

[0038] The positive electrode material of the present invention controls the residual alkali content on the surface by combining flame retardants such as magnesium hydroxide and / or aluminum hydroxide with a small amount of boron oxide, and utilizes the flame retardant mechanism of the flame retardant (i.e., heat absorption and cooling, formation of a carbonized layer, inhibition of combustion reaction by oxides, high heat capacity of hydroxides and formation of a dense oxide protective layer to isolate oxygen, etc.) combined with the high thermal conductivity and high-temperature and high-viscosity characteristics of boron oxide to reduce the thermal diffusion temperature and effectively conduct heat when thermal runaway occurs, form a dense protective layer to isolate air, achieve a self-flaming retardant effect, and inhibit the occurrence of thermal runaway.

[0039] Aluminum hydroxide and magnesium hydroxide are both inorganic flame retardants. Their flame retardant mechanism is that during the decomposition process, the hydroxide decomposes to produce water vapor and oxides attached to the surface to prevent combustion. The decomposition temperature of aluminum hydroxide is 190-230°C, and the decomposition temperature of magnesium hydroxide is 340-490°C. The boric acid added during the calcination process can play the dual role of flux and network former in the low-temperature process, further bonding the flame retardant to the surface of the material to form a better coating structure, thereby preventing thermal runaway from further occurring. In addition, magnesium hydroxide and magnesium oxide have better thermal conductivity, which can quickly conduct heat, prevent local overheating, and prevent thermal runaway from occurring. Aluminum hydroxide can dehydrate and react to form γ-Al2O3 at a lower temperature of 100-150°C, which can delay heat release in the early stage of thermal runaway, and even prevent thermal runaway.

[0040] When the B element is not added to the positive electrode material or the B element content is low, the NaOH content in the residual alkali in the positive electrode material is significantly higher, and the battery prepared using it has a large capacity difference; when the B element content in the positive electrode material is high, the residual alkali NaOH content is high, and the battery capacity prepared using it is low and the capacity difference is large; when the metal hydroxide (M(OH) α ) content is high, the residual alkali NaOH and Na2CO3 content is high, the battery capacity made therefrom is low and the specific capacity difference is large.

[0041] In some embodiments of the present invention, the positive electrode material includes a layered oxide and a coating layer coated on the surface of the layered oxide;

[0042] Layered oxides include NaNi a Fe b Mn c Cu (1-a-b-c) O2, where 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1;

[0043] The coating layer includes boron oxide and metal hydroxide, and the metal hydroxide includes Al(OH)3 and / or Mg(OH)2.

[0044] The present invention covers the surface of the layered oxide with boron oxide and metal hydroxide, which can effectively inhibit the occurrence of thermal runaway.

[0045] In some embodiments of the present invention, the positive electrode material satisfies the following relationship:

[0046]

[0047] Wherein, J is the theoretical calculated value of the residual alkali content in the positive electrode material, the residual alkali is sodium hydroxide and sodium carbonate, J is 0.1% to 2.6%; z is the molar ratio of metal hydroxide to layered oxide, z is 0.005 to 0.05; is the proportion of metal elements in metal hydroxides.

[0048] 0.675% is the average value of the upper and lower limits of the sodium hydroxide content and the sodium carbonate content in the positive electrode material, which is used as the conversion coefficient of the residual alkali content; (1-z×10×5×lnz) is the effect of the amount of metal hydroxide added on the total residual alkali value.

[0049] When M in the positive electrode material is Mg, z is the molar ratio of Mg(OH)2 to layered oxide, is the ratio of the relative atomic mass of Mg to the relative molecular mass of Mg(OH)2;

[0050] When M in the positive electrode material is Al, z is the molar ratio of Al(OH)3 to layered oxide, It is the ratio of the relative atomic mass of Al to the relative molecular mass of Al(OH)3;

[0051] When M in the positive electrode material is Mg and Al, J = J Mg +J Al .

[0052] In some embodiments of the present invention, in the positive electrode material, the content of sodium hydroxide is 0.001wt% to 0.1wt%, and the content of sodium carbonate is 0.1wt% to 2.5wt%; typically but not limitatively, for example, in the positive electrode material, the content of sodium hydroxide can be 0.001wt%, 0.005wt%, 0.01wt%, 0.05wt%, 0.1wt% or a range consisting of any two thereof; in the positive electrode material, the content of sodium carbonate can be 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt% or a range consisting of any two thereof.

[0053] In some embodiments of the present invention, the average particle size D50 of the positive electrode material is 5 to 20 μm; typically but not limitatively, for example, the average particle size D50 of the positive electrode material can be 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or a range of any two thereof.

[0054] In some embodiments of the present invention, a method for preparing the above-mentioned positive electrode material is also provided, comprising the following steps:

[0055] calcining the layered oxide, H3BO3 and metal hydroxide to obtain a positive electrode material;

[0056] Among them, layered oxides include NaNi a Fe b Mn c Cu (1-a-b-c) O2, wherein 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1; the metal hydroxide includes Al(OH)3 and / or Mg(OH)2.

[0057] The present invention uses H3BO3 and metal hydroxide as raw materials and co-coats them on the surface of the positive electrode material at low temperature to obtain a high-safety positive electrode material that can suppress thermal runaway and self-ignite; wherein the metal hydroxide serves as an inorganic flame retardant, and H3BO3 plays a dual role as a flux and a network former in the low-temperature process, further bonding the flame retardant to the material surface to form a better coating structure.

[0058] In some embodiments of the present invention, calcination includes: heating to 100-350°C and calcining for 6-18 hours; preferably, when the metal hydroxide is Al(OH)3, calcination includes: heating to 100-150°C and calcining for 6-18 hours; when the metal hydroxide is Mg(OH)2, calcination includes heating to 100-350°C and calcining for 6-18 hours; when the metal hydroxide is Al(OH)3 and Mg(OH)2, calcination includes heating to 100-150°C and calcining for 6-18 hours.

[0059] In some embodiments of the present invention, the heating rate during the calcination process is 1-10° C. / min.

[0060] In some embodiments of the invention, calcination is performed under an oxygen-containing atmosphere.

[0061] In some embodiments of the present invention, after calcination, the process further comprises crushing; preferably, the crushing is performed to a particle size D50 of 5 to 20 μm.

[0062] In some embodiments of the present invention, the method for preparing the layered oxide comprises:

[0063] After sintering the copper-nickel-iron-manganese quaternary precursor and the sodium source, a layered oxide is obtained;

[0064] or,

[0065] After sintering the nickel-iron-manganese ternary precursor, the copper source and the sodium source, a layered oxide is obtained.

[0066] In some embodiments of the present invention, the copper-nickel-iron-manganese quaternary precursor includes Ni a Fe b Mn c Cu (1-a-b-c)(OH)2; wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1.

[0067] In some embodiments of the present invention, the nickel-iron-manganese ternary precursor includes Ni u Fe v Mn 1-u-v (OH)2; wherein, 0<u≤0.5, 0<v≤0.4.

[0068] In some embodiments of the present invention, the average particle size D50 of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor are each independently 2.5 to 8.5 μm, and the specific surface area (BET) is each independently 10 to 30 m 2 / g; typically but not limiting, for example, the average particle size D50 of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor can be 2.5μm, 3.5μm, 4.5μm, 5.5μm, 6.5μm, 7.5μm, 8.5μm or a range of any two thereof; the specific surface area (BET) can be 10m 2 / g, 15m 2 / g, 20m 2 / g, 25m 2 / g, 30m 2 / g or a range consisting of any two of them.

[0069] The particle size of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor is too small, the reaction activity is strong, the side reaction is high, and the corrosion during the preparation process is serious; the particle size is too large, the reaction activity is low, and it is difficult to sinter fully; the specific surface area is too large, the reaction activity is strong, the adhesion is serious, and the fine powder is crushed to affect the yield; the specific surface area is too small, the reaction activity is low, and it is difficult to sinter fully.

[0070] In some embodiments of the present invention, the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor contain impurity elements; the impurity elements include at least one of Na, S, Ca, Mg, Al, Zn, Co and Li; the content of each impurity element is <5000ppm.

[0071] In some embodiments of the present invention, the sodium source includes but is not limited to Na2CO3 and / or NaHCO3.

[0072] In some embodiments of the present invention, the copper source includes, but is not limited to, CuO.

[0073] In some embodiments of the present invention, sintering includes: heating to 900-1000°C and sintering for 8-24h; typically but not limitatively, for example, the sintering temperature can be 900°C, 950°C, 1000°C or a range consisting of any two thereof; the sintering time can be 8h, 15h, 20h, 24h or a range consisting of any two thereof.

[0074] In some embodiments of the present invention, the heating rate during the sintering process is 1-10° C. / min.

[0075] In some embodiments of the present invention, sintering is performed in an oxygen-containing atmosphere.

[0076] In some embodiments of the present invention, after sintering, the process further comprises crushing; preferably, the crushing is performed to a particle size D50 of 5 to 20 μm.

[0077] In some embodiments of the present invention, a sodium ion battery is also provided, comprising the above-mentioned positive electrode material or the positive electrode material prepared by the above-mentioned method for preparing the positive electrode material.

[0078] The positive electrode material of the present invention is used in a sodium ion battery to improve the safety performance, first efficiency, discharge specific capacity and specific capacity range of the battery.

[0079] Example 1

[0080] The chemical formula of the positive electrode material provided in this embodiment is:

[0081] NaCu 0.1 Mn 0.25 Ni 0.15 Fe 0.5 O2·0.05Al(OH)3·0.0001BO 3 / 2 ;

[0082] The specific preparation method comprises the following steps:

[0083] Weigh 1.652 kg of Na2CO3 (purity 99.72%), 0.291 kg of NaHCO3 (purity 99.68%) and 4 kg of spherical precursor Cu 0.1 Mn 0.25 Ni 0.15 Fe 0.5 (OH)2(particle size D 50 The BET specific surface area is 7.5 μm and 15.63 m 2 / g), after high-speed mixing, the temperature was raised to 900°C at a rate of 2°C / min in an oxygen atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 14.5μm to obtain a layered oxide;

[0084] 0.215 g of H3BO3 (purity of 99.21%) and 135.606 g of Al(OH)3 (purity of 99.34%) were added to the layered oxide and mixed at high speed. The mixture was heated to 150°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 14.6 μm was obtained, which was recorded as B1.

[0085] Example 2

[0086] The chemical formula of the positive electrode material provided in this embodiment is:

[0087] NaCu 0.01 Mn 0.45 Ni 0.44 Fe 0.1 O2·0.05Mg(OH)2·0.005BO 3 / 2 ;

[0088] The specific preparation method comprises the following steps:

[0089] Weigh 1.836 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.01 Mn 0.45 Ni 0.44 Fe 0.1 (OH)2(particle size D 50 The BET specific surface area is 18.62 m 2 / g) after high-speed mixing, the temperature was raised to 1000°C at a rate of 3°C / min in an air atmosphere for sintering for 18 hours, and then the material was crushed to a particle size D50 of 8.2 μm to obtain a layered oxide;

[0090] 10.768 g of H3BO3 (purity of 99.21%) and 101.513 g of Mg(OH)2 (purity of 99.26%) were added to the layered oxide and mixed at high speed. The mixture was heated to 350°C at a rate of 2°C / min in an air atmosphere and calcined for 6 hours. After crushing, a positive electrode material with a particle size D50 of 8.2 μm was obtained, which was recorded as B2.

[0091] Example 3

[0092] The chemical formula of the positive electrode material provided in this embodiment is:

[0093] NaCu 0.03 Mn 0.34 Ni 0.31 Fe 0.32 O2·0.02Al(OH)3·0.02Mg(OH)2·0.001BO 3 / 2 ;

[0094] The specific preparation method comprises the following steps:

[0095] Weigh 1.838 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.03 Mn 0.34 Ni 0.31 Fe 0.32 (OH)2(particle size D 50 The BET specific surface area is 19.54 m 2 / g) were mixed at high speed, heated to 980°C at a rate of 3°C / min in an air atmosphere for sintering for 10 h, and then the material was crushed to a particle size D50 of 9.6 μm to obtain a layered oxide;

[0096] 2.156 g of H3BO3 (purity of 99.21%), 54.321 g of Al(OH)3 (purity of 99.34%) and 40.646 g of Mg(OH)2 (purity of 99.26%) were added to the layered oxide and mixed at high speed. The mixture was heated to 150°C at a rate of 3°C / min in an air atmosphere and calcined for 18 hours. After crushing, a positive electrode material with a particle size D50 of 9.7 μm was obtained, which was recorded as B3.

[0097] Example 4

[0098] The chemical formula of the positive electrode material provided in this embodiment is:

[0099] NaCu 0.05 Mn 0.49 Ni 0.44 Fe 0.02 O2·0.005Mg(OH)2·0.0005BO 3 / 2 ;

[0100] The specific preparation method comprises the following steps:

[0101] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.05 Mn 0.49 Ni 0.44 Fe 0.02 (OH)2(particle size D 50 The BET specific surface area is 22.48 m 2 / g) after high-speed mixing, heating to 1000°C at a rate of 3°C / min in an air atmosphere for sintering for 18h, and then crushing the material to a particle size D50 of 6.6μm to obtain a layered oxide;

[0102] 1.074 g of H3BO3 (purity of 99.21%) and 10.128 g of Mg(OH)2 (purity of 99.26%) were added to the layered oxide and mixed at high speed. The mixture was heated to 300°C at a rate of 10°C / min in an air atmosphere and calcined for 18 hours. After crushing, a positive electrode material with a particle size D50 of 6.7 μm was obtained, which was recorded as B4.

[0103] Example 5

[0104] The chemical formula of the positive electrode material provided in this embodiment is:

[0105] NaCu 0.07 Mn 0.4 Ni 0.33 Fe 0.2 O2·0.005Al(OH)3·0.005BO 3 / 2 ;

[0106] The specific preparation method comprises the following steps:

[0107] Weigh 2.907 kg of NaHCO3 (99.68%) and 4 kg of spherical precursor Cu 0.07 Mn 0.4 Ni 0.33 Fe 0.2 (OH)2 Particle Size D 50 The BET specific surface area is 4.7 μm and 18.62 m 2 / g) were mixed at high speed, heated to 990°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 5.4μm to obtain a layered oxide;

[0108] 10.750 g of H3BO3 (purity of 99.21%) and 13.544 g of Al(OH)3 (purity of 99.34%) were added to the layered oxide and mixed at high speed. In an oxygen atmosphere, the temperature was raised to 100°C at a rate of 8°C / min and calcined for 15 hours. After crushing, a positive electrode material with a particle size D50 of 5.5 μm was obtained, which was recorded as B5.

[0109] Example 6

[0110] The chemical formula of the positive electrode material provided in this embodiment is:

[0111] NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2·0.01Al(OH)3·0.005Mg(OH)2·0.002BO 3 / 2 ;

[0112] The specific preparation method comprises the following steps:

[0113] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) were mixed at high speed, and then heated to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 10.1μm to obtain a layered oxide;

[0114] 4.298 g of H3BO3 (purity of 99.21%), 27.074 g of Al(OH)3 (purity of 99.34%) and 10.129 g of Mg(OH)2 (purity of 99.26%) were added to the layered oxide and mixed at high speed. The mixture was heated to 150°C at a rate of 5°C / min in an air atmosphere and calcined for 12 hours. After crushing, a positive electrode material with a particle size D50 of 10.0 μm was obtained, which was recorded as B6.

[0115] Example 7

[0116] The chemical formula of the positive electrode material provided in this embodiment is:

[0117] NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2·0.005Al(OH)3·0.01Mg(OH)2·0.002BO 3 / 2 ;

[0118] The specific preparation method comprises the following steps:

[0119] Weigh 1.999 kg of Na2CO3 (purity 99.72%), 310.986 g of CuO (purity 95.34%, D50 = 12.4 μm) and 4 kg of spherical precursor Mn 0.37 Ni 0.25 Fe 0.38 (OH)2(particle size D 50 The BET specific surface area is 4.5 μm and 12.74 m 2 / g) were mixed at high speed, heated to 980°C at a rate of 5°C / min in an air atmosphere for sintering for 24h, and then the material was crushed to a particle size D50 of 9.8μm to obtain a layered oxide;

[0120] 4.688 g of H3BO3 (purity of 99.21%), 14.767 g of Al(OH)3 (purity of 99.34%) and 22.099 g of Mg(OH)2 (purity of 99.26%) were added to the layered oxide and mixed at high speed. The mixture was heated to 150°C at a rate of 5°C / min in an air atmosphere and calcined for 12 hours. After crushing, a positive electrode material with a particle size D50 of 9.8 μm was obtained, which was recorded as B7.

[0121] Comparative Example 1

[0122] The chemical formula of the positive electrode material provided in this comparative example is:

[0123] NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2·0.01Al(OH)3·0.005Mg(OH)2·0.006BO 3 / 2 ;

[0124] The specific preparation method comprises the following steps:

[0125] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) were mixed at high speed, heated to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 9.8μm to obtain a layered oxide;

[0126] 12.894 g of H3BO3 (purity of 99.21%), 27.074 g of Al(OH)3 (purity of 99.34%) and 10.129 g of Mg(OH)2 (purity of 99.26%) were added to the layered oxide and mixed at high speed. The mixture was heated to 150°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 9.8 μm was obtained, which was recorded as A1.

[0127] Comparative Example 2

[0128] The chemical formula of the positive electrode material provided in this comparative example is:

[0129] NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34O2·0.015Ca(OH)2·0.002BO 3 / 2 ;

[0130] The specific preparation method comprises the following steps:

[0131] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) were mixed at high speed, and then heated to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 9.6μm to obtain a layered oxide;

[0132] 4.298 g of H3BO3 (purity of 99.21%) and 38.660 g of Ca(OH)2 (purity of 99.12%) were added to the layered oxide and mixed at high speed. The mixture was heated to 350°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 9.5 μm was obtained, which was recorded as A2.

[0133] Comparative Example 3

[0134] The chemical formula of the positive electrode material provided in this comparative example is:

[0135] NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2·0.06Al(OH)3·0.002BO 3 / 2 ;

[0136] The specific preparation method comprises the following steps:

[0137] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) were mixed at high speed, heated to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size D50 of 10.2μm to obtain a layered oxide;

[0138] 4.298 g of H3BO3 (purity of 99.21%) and 162.443 g of Al(OH)3 (purity of 99.34%) were added to the layered oxide and mixed at high speed. The mixture was heated to 150°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 10.3 μm was obtained, which was recorded as A3.

[0139] Comparative Example 4

[0140] The chemical formula of the positive electrode material provided in this comparative example is:

[0141] NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2·0.01Al(OH)3·0.005Mg(OH)2;

[0142] The specific preparation method comprises the following steps:

[0143] Weigh 1.832 kg of Na2CO3 (purity 99.72%) and 4 kg of spherical precursor Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2(particle size D 50 The BET specific surface area is 6.7 μm and 13.41 m 2 / g) after high-speed mixing, the temperature was raised to 960°C at a rate of 3°C / min in an air atmosphere for sintering for 15h, and then the material was crushed to a particle size of D50 = 9.9μm to obtain a layered oxide;

[0144] 27.074 g of Al(OH)3 (purity of 99.34%) and 10.129 g of Mg(OH)2 (purity of 99.26%) were added to the layered oxide and mixed at high speed. The mixture was heated to 150°C at a rate of 3°C / min in an air atmosphere and calcined for 10 hours. After crushing, a positive electrode material with a particle size D50 of 9.8 μm was obtained, which was recorded as A4.

[0145] Test example

[0146] The positive electrode materials of Example 6 and Comparative Example 2 were tested by scanning electron microscope, and the results are as follows: Figure 1 and Figure 2 shown.

[0147] from Figure 1 The morphology of the positive electrode material of Example 6 is smooth and evenly distributed on the particle surface, without small particles attached; Figure 2 This is the morphology of the positive electrode material of Comparative Example 2, and there is uneven enrichment of precipitates on the particle surface.

[0148] The parameters of the positive electrode materials of Examples 1 to 7 and Comparative Examples 1 to 4 were tested, and the results are shown in Table 1.

[0149] In Comparative Example 2 of Table 1, J Ca =0.675%×(1-0.015×10×5×ln0.015)×(40 / 74).

[0150] In Table 1, z is the molar ratio of Mg(OH)2 to layered oxide, is the ratio of the relative atomic mass of Mg to the relative molecular mass of Mg(OH)2; z is the molar ratio of Al(OH)3 to layered oxide, J is the ratio of the relative atomic mass of Al to the relative molecular mass of Al(OH)3; 计算 =J Mg +J Al ;

[0151] The residual alkali content in the positive electrode material, that is, the NaOH content (mass percentage) and the Na2CO3 content (mass percentage) in the positive electrode material are converted by testing the hydroxide and carbonate with the Metrohm 888 / 905 instrument. The sum of the two is the test value of the residual alkali content in the positive electrode material, that is, J 测试 .

[0152] Table 1

[0153]

[0154]

[0155] The positive electrode materials of Examples 1 to 7 and Comparative Examples 1 to 4 were respectively used as positive electrode active materials to assemble button-type batteries. The performance of each battery was tested, and the results are shown in Table 2.

[0156] A method for preparing a button cell comprises the following steps:

[0157] The positive active material, SP and PVDF were mixed in a mass ratio of 90:5:5, and NMP was added to make a viscous glue, which was coated on an aluminum foil and baked in a vacuum drying oven at 120°C for 12 h to obtain a positive electrode. A 2032 button cell was assembled in an Ar protective glove box using a metal sodium sheet as the counter electrode, glass fiber (Waterman) as the separator, and 1 mol / LNaPF6 EC / DMC=1:1 (Alfa) as the electrolyte.

[0158] Test method: Test the battery in the voltage range of 2.5-4.0V, cycle at 0.1C for 100 weeks, and record the average discharge capacity, discharge capacity extreme value and first efficiency of 5 batteries at 0.1C in the first 3 weeks.

[0159] Table 2

[0160]

[0161]

[0162] It can be seen from Table 1 and Table 2 that, when Example 6 is compared with Comparative Example 1, the amount of B added in the positive electrode material exceeds the limit value, the NaOH content in the residual alkali is high, the charge capacity is low, and the specific capacity difference is large.

[0163] Comparing Example 6 with Comparative Example 2, Ca exceeds the metal element limit, the NaOH content in the residual alkali is significantly higher, its withholding capacity performance is low, and the specific capacity difference is large; in addition, the decomposition temperature of Ca(OH)2 is as high as 580°C, at which time thermal runaway can no longer be prevented. Alkali metal elements are harmful to processing performance, and the decomposition temperatures of hydroxides of other elements are relatively high, making it difficult to achieve this effect, and their elements may be harmful to the battery system.

[0164] Comparing Example 6 with Comparative Example 3, the amount of Al added to the positive electrode material exceeds the limit value, the NaOH content in the residual alkali is high, the Na2CO3 content is also significantly high, the charge capacity performance is low, and the specific capacity is extremely poor.

[0165] Comparing Example 6 with Comparative Example 4, the positive electrode material without adding element B has a significantly higher NaOH content in the residual alkali, a normal withholding capacity, but a large difference in specific capacity.

[0166] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A positive electrode material, It is characterized in that The chemical formula of the positive electrode material is NaNi a Fe b Mn c Cu (1-a-b-c) O 2 ·xM(OH) α ·yBO 3 / 2 ; Wherein, 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1, 0.005≤x≤0.05, 0.0001≤y≤0.005, M element includes Mg and / or Al, and α is the valence value of M element.

2. The positive electrode material according to claim 1, It is characterized in that The positive electrode material includes a layered oxide and a coating layer coated on the surface of the layered oxide; The layered oxide includes NaNi a Fe b Mn c Cu (1-a-b-c) O 2 , where 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1; The coating layer includes boron oxide and metal hydroxide, and the metal hydroxide includes Al(OH) 3 and / or Mg(OH) 2 .

3. The positive electrode material according to claim 2, It is characterized in that The positive electrode material satisfies the following relationship: In the formula, J is the theoretical calculated value of the residual alkali content in the positive electrode material, and the residual alkali is sodium hydroxide and sodium carbonate; z is the molar ratio of the metal hydroxide to the layered oxide; is the proportion of the metal element in the metal hydroxide.

4. The positive electrode material according to claim 1, It is characterized in that In the positive electrode material, the content of sodium hydroxide is 0.001wt% to 0.1wt%, and the content of sodium carbonate is 0.1wt% to 2.5wt%.

5. The method for preparing the positive electrode material according to any one of claims 1 to 4, It is characterized in that The steps include: The layered oxide, H 3 BO 3 and metal hydroxide to obtain the positive electrode material; Wherein, the layered oxide includes NaNi a Fe b Mn c Cu (1-a-b-c) O 2 , wherein 0<a≤0.5, 0<b≤0.4, 0<c≤0.4, 0.8≤a+b+c<1; the metal hydroxide includes Al(OH) 3 and / or Mg(OH) 2 .

6. The method for preparing the positive electrode material according to claim 5, It is characterized in that The calcination comprises: heating to 100-350° C. and calcining for 6-18 hours.

7. The method for preparing the positive electrode material according to claim 5, It is characterized in that The method for preparing the layered oxide comprises: After sintering the copper-nickel-iron-manganese quaternary precursor and the sodium source, the layered oxide is obtained; or, The layered oxide is obtained by sintering the nickel-iron-manganese ternary precursor, the copper source and the sodium source.

8. The method for preparing the positive electrode material according to claim 7, It is characterized in that The average particle size of the copper-nickel-iron-manganese quaternary precursor and the nickel-iron-manganese ternary precursor are independently 2.5 to 8.5 μm, and the specific surface area is independently 10 to 30 m 2 / g.

9. The method for preparing the positive electrode material according to claim 7, It is characterized in that The sintering comprises: heating to 900-1000° C. and sintering for 8-24 hours.

10. A sodium ion battery, It is characterized in that The invention comprises the positive electrode material according to any one of claims 1 to 4 or the positive electrode material prepared by the preparation method of the positive electrode material according to any one of claims 5 to 9.