Thermoplastic resin and optical member comprising same

By using the copolymerization of specific repeat units in thermoplastic resins, the refractive index, Abbe number and heat resistance are optimized, and the optical lens performance problems that are difficult to meet simultaneously in the prior art are solved, achieving a wider range of use and performance improvement.

CN118922469APending Publication Date: 2024-11-08TEIJIN LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029439.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-02-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In optical lenses, existing thermoplastic resins are difficult to meet the requirements of refractive index, Abbe number, heat resistance and birefringence simultaneously, resulting in limited use position.

Method used

Using a thermoplastic resin composed of more than 60 mol% of specific repeating units, the refractive index, Abbe number and heat resistance are optimized by copolymerization of formula (1), formula (2) and formula (3), and the refractive index, and the orientation birefractive is controlled. Below 3.0×10-3, meet the needs of optical components.

Benefits of technology

It realizes that the requirements of refractive index, ABE, heat resistance and birefringence are met simultaneously in optical lenses, and the performance and use range of optical components are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922469A_ABST
    Figure CN118922469A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a polycarbonate resin which satisfies all of the refractive index, Abbe number, heat resistance, and birefringence at the same time; and an optical member which contains the polycarbonate resin. This thermoplastic resin contains repeating units represented by formula (1), formula (2), and formula (3), the repeating units represented by formula (1) being 60 mol% or more, and the refractive index being greater than 1.600 and 1.660 or less. (In formula (1), R1 to R4 each independently represent a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms) (in formula (3), n is in the range of 1 to 8, R5 and R6 each independently represent a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and R7 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms). # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a novel thermoplastic resin and an optical component, particularly an optical lens, formed of the thermoplastic resin. Background Art

[0002] The present invention relates to a thermoplastic resin and an optical component comprising the same.

[0003] There is a strong demand for low birefringence and improved aberration correction capabilities for plastic imaging lenses used in devices such as smartphones. In the past, aberration correction was performed in such imaging lenses by combining multiple lenses with different optical properties (refractive index, Abbe number) and lens shapes.

[0004] In recent years, lens units are increasingly made by combining high refractive index, low Abbe number resins with cycloolefin-based low refractive index, high Abbe number resins. In addition, in order to make high-performance lens units, the range of lens design is expanded by using medium refractive index, medium Abbe number resins, and fine-tuning is possible to achieve high performance. Therefore, the demand for medium refractive index, medium Abbe number resins with a refractive index of about 1.600 to 1.660 is increasing.

[0005] However, when optical transparent resins are used as optical lenses, in addition to the refractive index and Abbe number, they are also required to have transparency, heat resistance, and low birefringence, so there is a disadvantage that the use locations are limited due to the balance of resin characteristics. For example, polystyrene has low heat resistance and large birefringence, poly-4-methylpentene has low heat resistance, polymethyl methacrylate has a low glass transition temperature and low heat resistance, and polycarbonate composed of bisphenol A has weaknesses such as large birefringence, so the use locations are limited.

[0006] Patent Documents 1 to 3 describe polycarbonate resin compositions containing a compound having a fluorene skeleton.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 10-101786

[0010] Patent Document 2: International Publication No. 2017 / 010318

[0011] Patent Document 3: Japanese Patent Application Publication No. 2020-19922 Summary of the invention

[0012] The polycarbonate resins described in Patent Documents 1 and 2 propose copolymerized resins of a compound having a fluorene skeleton and one other component, and although any of the refractive index, Abbe number, heat resistance, and birefringence can be satisfied, it is difficult to satisfy all of them.

[0013] The polycarbonate resin described in Patent Document 3 has a low content of the compound having a fluorene skeleton, and therefore can satisfy any one of the refractive index, Abbe number, heat resistance, and birefringence, but cannot satisfy all of them.

[0014] Therefore, an object of the present invention is to provide a polycarbonate resin that satisfies all of the requirements of refractive index, Abbe number, heat resistance, and birefringence, and an optical component comprising the polycarbonate resin.

[0015] The present inventors have found that the above-mentioned problems can be solved by the present invention having the following aspects.

[0016] Method 1

[0017] A thermoplastic resin comprising repeating units represented by formula (1), formula (2) and formula (3), wherein the repeating unit represented by formula (1) accounts for 60 mol % or more and the refractive index is greater than 1.600 and is less than 1.660.

[0018]

[0019] (In formula (1), R 1 ~R 4 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms)

[0020]

[0021]

[0022] (In formula (3), n is in the range of 1 to 8, R 5 and R 6 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and R 7 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms)

[0023] Method 2

[0024] The thermoplastic resin according to Embodiment 1, wherein the repeating unit of the formula (1) accounts for 60 mol% to 80 mol%.

[0025] Method 3

[0026] The thermoplastic resin according to embodiment 1 or 2, wherein R in the formula (1) 1 ~R 4 A hydrogen atom.

[0027] Method 4

[0028] The thermoplastic resin according to any one of Embodiments 1 to 3, wherein the repeating unit of the formula (3) is a repeating unit derived from 4,4′-(3,3,5-trimethylcyclohexylidene)bisphenol.

[0029] Method 5

[0030] The thermoplastic resin according to any one of aspects 1 to 4, wherein the glass transition temperature is 130 to 160°C.

[0031] Method 6

[0032] The thermoplastic resin according to any one of aspects 1 to 5, wherein the absolute value of the orientation birefringence is 3.0×10 -3 the following.

[0033] Method 7

[0034] The thermoplastic resin according to any one of aspects 1 to 5, wherein the absolute value of the orientation birefringence is 1.0×10 -3 the following.

[0035] Method 8

[0036] The thermoplastic resin according to any one of aspects 1 to 7, wherein the Abbe number is 24.0 to 29.0.

[0037] Method 9

[0038] An optical component comprising the thermoplastic resin according to any one of aspects 1 to 8.

[0039] Method 10

[0040] The optical component according to Mode 9 is an optical lens. DETAILED DESCRIPTION

[0041] <Thermoplastic resin>

[0042] The thermoplastic resin of the present invention comprises repeating units represented by the above formula (1), the above formula (2) and the above formula (3), wherein the repeating unit represented by the above formula (1) accounts for 60 mol% or more. The thermoplastic resin of the present invention has a refractive index greater than 1.600 and not more than 1.660.

[0043] The present inventors have found that in the production of optical lens units, a thermoplastic resin containing 60 mol% or more of the repeating unit represented by the above formula (1) exhibits useful medium refractive index and medium Abbe number. Furthermore, the present inventors have found that by copolymerizing the above formulas (2) and (3), not only the refractive index and Abbe number but also the heat resistance and birefringence are satisfied, thereby completing the present application.

[0044] <Thermoplastic resin structure>

[0045] In the above formula (1), R 1 ~R 4 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and examples of the hydrocarbon group include an alkyl group, a cycloalkyl group, and an aryl group.

[0046] Examples of the alkyl group include methyl group, ethyl group, propyl group, isopropyl group, butyl group, tert-butyl group and the like, and methyl group and ethyl group are preferred.

[0047] Examples of the cycloalkyl group include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl and bicyclo[1.1.1]pentyl.

[0048] Examples of the aryl group include phenyl, tolyl, naphthyl, and xylyl, and a phenyl group is preferred.

[0049] R 1 ~R 4 Each of them is independently preferably a hydrogen atom, a methyl group, or a phenyl group, more preferably a hydrogen atom or a phenyl group, 1 and R 2 are each independently a hydrogen atom or a phenyl group, R 3 and R 4 A hydrogen atom is more preferred.

[0050] The repeating unit represented by the formula (1) is preferably a repeating unit derived from 9,9-bis(4-(hydroxyethoxy)phenyl)fluorene or 9,9-bis(4-(hydroxyethoxy)-3-phenylphenyl)fluorene, and more preferably a repeating unit derived from 9,9-bis(4-(hydroxyethoxy)phenyl).

[0051] The thermoplastic resin of the present invention may contain the repeating unit of the formula (1) in an amount of preferably 60 mol% to 99 mol%, more preferably 60 mol% to 85 mol%, further preferably 60 mol% to 80 mol%, particularly preferably 65 mol% to 80 mol%, and most preferably 70 mol% to 80 mol%.

[0052] When the repeating unit represented by the above formula (1) is within the above range, the refractive index and birefringence can be satisfied.

[0053] The repeating unit represented by the above formula (2) is a repeating unit derived from 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane.

[0054] The thermoplastic resin of the present invention may contain the repeating unit of the formula (2) in an amount of preferably 1 to 35 mol%, more preferably 5 to 30 mol%, further preferably 10 to 25 mol%, particularly preferably 10 to 20 mol%.

[0055] In the above formula (3), n represents a range of 1 to 8, preferably 1 to 5, more preferably 1 to 3, and even more preferably 3. 5 , R 6 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and examples of the hydrocarbon group include an alkyl group, a cycloalkyl group, and an aryl group.

[0056] Examples of the alkyl group include methyl group, ethyl group, propyl group, isopropyl group, butyl group, tert-butyl group and the like, and methyl group and ethyl group are preferred.

[0057] Examples of the cycloalkyl group include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl and bicyclo[1.1.1]pentyl.

[0058] Examples of the aryl group include phenyl, tolyl, naphthyl and xylyl, and phenyl is preferred.

[0059] R 5 , R 6 Each independently is preferably a hydrogen atom, a methyl group or a phenyl group, more preferably a hydrogen atom or a phenyl group, and further preferably a hydrogen atom.

[0060] R 7 It represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and is preferably a methyl group or an ethyl group, and more preferably a methyl group.

[0061] R 5 , R 6 When the substituents of are as described above, the amount of the above-mentioned formula (3) introduced can be increased without significantly increasing the refractive index, and high heat resistance can be achieved. 7 When the substituent of is as described above, higher heat resistance can be achieved.

[0062] The repeating unit represented by the formula (3) is preferably a repeating unit derived from 4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol, 4,4'-cyclohexylidenebisphenol, or 4,4'-(3-methylcyclohexylidene)bisphenol, and more preferably a repeating unit derived from 4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol or 4,4'-cyclohexylidenebisphenol.

[0063] The thermoplastic resin of the present invention may contain the repeating unit of the formula (3) in an amount of preferably 1 mol% to 35 mol%, more preferably 5 mol% to 30 mol%, further preferably 5 mol% to 20 mol%, particularly preferably 5 mol% to 15 mol%.

[0064] When the repeating units represented by the above formulae (2) and (3) are within the above ranges, the refractive index, Abbe number, heat resistance and birefringence can be satisfied.

[0065] The thermoplastic resin of the present invention may contain repeating units other than the repeating units represented by the above formula (1), the above formula (2) and the above formula (3) within a range that can obtain the above-mentioned advantageous effects of the present invention. Examples of dihydroxy compounds that provide such repeating units include ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, tricyclo[5.2.1.02,6]decanedimethanol, cyclohexane-1,4-dimethanol, decalin-2,6-dimethanol, norbornane dimethanol, pentacyclopentadecanedimethanol, cyclopentane-1,3-dimethanol, isosorbide, isomannide, isoidose Alcohol, hydroquinone, resorcinol, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfide, bisphenol, bisphenol fluorene, biscresol fluorene, etc. Such repeating units may account for 10 mol% or less of all repeating units.

[0066] The thermoplastic resin of the present invention preferably does not have a phenolic hydroxyl group at the terminal. That is, when the monomer that brings about the repeating unit represented by the above formula (3) is polymerized and bonded to the terminal, the terminal group becomes a phenolic hydroxyl group. Therefore, it is preferred to reduce the amount of terminal phenolic hydroxyl groups of the thermoplastic resin by, for example, using an excess of carbonic acid diester relative to the dihydroxy compound as a raw material during polymerization and making the terminal a phenyl group. The ratio of the terminal phenolic hydroxyl group can be calculated as follows:

[0067] Terminal phenolic hydroxyl group ratio=(terminal phenolic hydroxyl group amount / total terminal amount)×100.

[0068] In addition, all the terminals are composed of a terminal phenolic hydroxyl group, a terminal alcoholic hydroxyl group and a terminal phenyl group.

[0069] Specifically, the terminal phenolic hydroxyl group ratio can be determined by the following method, but the invention is not limited to this example.

[0070] (1) Through the thermoplastic resin 1The terminal phenolic hydroxyl group was observed by H NMR measurement, and the integral of the peak was read and set to 1. At this time, the integrated intensity (A) of the proton portion of the fluorene structure 1 was simultaneously determined from the integrated intensities of the peaks at positions 4 and 5 of the fluorene structure of the above formula (1).

[0071] Of course, when the peak of the terminal phenolic hydroxyl group is not observed, the terminal phenolic hydroxyl group ratio is 0.

[0072] (2) The average degree of polymerization of the thermoplastic resin is determined from the number average molecular weight, the molecular weight of each repeating unit and the molar ratio obtained by GPC measurement of the thermoplastic resin. The terminal molecular weight is determined using the following formula based on the molar % and the integrated intensity (A) of the above formula (1). 1 Integrated intensity in the H NMR spectrum (B).

[0073] (B) = (A) × 100 × 2 / ([mol% of the above formula (1)] × average degree of polymerization)

[0074] (3) The terminal phenolic hydroxyl group ratio was calculated as 1 / (B)×100.

[0075] The ratio of terminal phenolic hydroxyl groups to all terminals of the thermoplastic resin of the present invention is preferably 30% or less, 20% or less, 15% or less, 10% or less, 5% or less, 3% or less, 1% or less, or 0.5% or less.

[0076] <Thermoplastic resin properties>

[0077] The refractive index of the thermoplastic resin of the present invention, when measured at a temperature of 20° C. and a wavelength of 587.56 nm, is preferably greater than 1.600 and less than 1.660, more preferably greater than 1.600 and less than 1.650, further preferably greater than 1.600 and less than 1.630, particularly preferably greater than 1.600 and less than 1.620, and particularly preferably greater than 1.610 and less than 1.620.

[0078] The Abbe number of the thermoplastic resin of the present invention is preferably 24.0 to 29.0, more preferably 25.0 to 29.0, further preferably 24.0 to 28.0, particularly preferably 24.0 to 28.0, and most preferably 24.0 to 27.0.

[0079] Here, the Abbe number (νd) is calculated using the following formula from the refractive index at a temperature of 20° C. and wavelengths of 486.13 nm, 587.56 nm, and 656.27 nm.

[0080] νd=(nd-1) / (nF-nC)

[0081] nd: refractive index at a wavelength of 587.56nm,

[0082] nF: refractive index at a wavelength of 486.13nm,

[0083] nC: refractive index at a wavelength of 656.27nm.

[0084] The specific viscosity of the thermoplastic resin of the present invention is preferably 0.12 to 0.32, and more preferably 0.18 to 0.30. When the specific viscosity is 0.12 to 0.32, the balance between moldability and strength is excellent.

[0085] The specific viscosity was measured by using an Ostwald viscometer to measure the specific viscosity (ηSP) of a solution prepared by dissolving 0.7 g of a thermoplastic resin in 100 ml of dichloromethane at 20° C., and the specific viscosity was calculated by the following formula.

[0086] ηSP=(t-t0) / t0

[0087] [t0 is the falling seconds of dichloromethane, t is the falling seconds of the sample solution]

[0088] The absolute value of the orientation birefringence (Δn) of the thermoplastic resin of the present invention is preferably 3.0×10 -3 Below, more preferably 2.0×10 -3 Below, more preferably 1.0×10 -3 Below, particularly preferably 0.6×10 -3 Below, the most preferred is 0.4×10 -3 the following.

[0089] When the absolute value of the orientation birefringence is below the above value, the chromatic aberration is not greatly affected, and thus the performance as designed optically can be maintained. The orientation birefringence is measured at a wavelength of 589 nm after stretching a 100 μm thick cast film obtained from the thermoplastic resin by 2 times at Tg+10°C.

[0090] The total light transmittance of the thermoplastic resin of the present invention is preferably 1 mm thick and is 80% or more, more preferably 85% or more, particularly preferably 88% or more.

[0091] The saturated water absorption rate of the thermoplastic resin of the present invention may be 0.10% to 0.70%, 0.20% to 0.70%, or 0.30% to 0.65%.

[0092] The glass transition temperature of the thermoplastic resin of the present invention is preferably 130°C to 160°C, more preferably 135°C to 55°C, particularly preferably 140°C to 150°C.

[0093] Examples of the thermoplastic resin of the present invention include polycarbonates whose repeating units include carbonate structures represented by formula (1), formula (2) and formula (3), polyester carbonates whose repeating units include repeating units represented by formula (1), formula (2) and formula (3) and include ester structures other than these in the repeating units, etc. Among them, polycarbonates are preferred from the aspects of heat resistance and moisture-heat resistance.

[0094] <Production method of polycarbonate resin>

[0095] The polycarbonate resin of the present invention is produced by a known reaction method for producing a common polycarbonate resin, for example, a method of reacting a carbonate precursor such as a carbonic acid diester with a dihydroxy compound. Next, the basic method of producing the polycarbonate resin will be briefly described.

[0096] The transesterification reaction using carbonic acid diester as a carbonate precursor is carried out by heating and stirring a predetermined ratio of dihydroxy component and carbonic acid diester under an inert gas atmosphere to distill off the generated alcohol or phenol. The reaction temperature varies depending on the boiling point of the generated alcohol or phenol, and is usually in the range of 120 to 300° C. The reaction is terminated while distilling off the generated alcohol or phenol under reduced pressure from the initial stage of the reaction. In addition, a terminal terminator, an antioxidant, etc. may be added as required.

[0097] As the carbonic acid diester used in the above-mentioned transesterification reaction, esters of aryl groups, arylalkyl groups, etc. having 6 to 12 carbon atoms which may be substituted can be mentioned. Specifically, diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, and m-cresol carbonate can be exemplified. Among them, diphenyl carbonate is particularly preferred. The amount of diphenyl carbonate used is preferably 0.95 to 1.10 mol, more preferably 0.98 to 1.04 mol, relative to 1 mol of the total dihydroxy compound.

[0098] In the melt polymerization method, a polymerization catalyst may be used to increase the polymerization rate. Examples of the polymerization catalyst include alkali metal compounds, alkaline earth metal compounds, and nitrogen-containing compounds.

[0099] As such a compound, organic acid salts, inorganic salts, oxides, hydroxides, hydrides, alkoxides, quaternary ammonium hydroxides, etc. of alkali metals and alkaline earth metals are preferably used, and these compounds can be used alone or in combination.

[0100] Examples of the alkali metal compound include sodium hydroxide, potassium hydroxide, cesium hydroxide, lithium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, cesium carbonate, lithium carbonate, sodium acetate, potassium acetate, cesium acetate, lithium acetate, sodium stearate, potassium stearate, cesium stearate, lithium stearate, sodium borohydride, sodium benzoate, potassium benzoate, cesium benzoate, lithium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, disodium phenyl phosphate, disodium salt, dipotassium salt, dicesium salt, dilithium salt of bisphenol A, sodium salt, potassium salt, cesium salt, lithium salt of phenol, and the like.

[0101] Examples of the alkaline earth metal compound include magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, magnesium diacetate, calcium diacetate, strontium diacetate, and barium diacetate.

[0102] Examples of the nitrogen-containing compound include quaternary ammonium hydroxides having an alkyl group, an aryl group, and the like such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and trimethylbenzylammonium hydroxide. Examples include bases or basic salts such as tetramethylammonium borohydride, tetrabutylammonium borohydride, tetrabutyltetraphenylammonium borate, and tetraphenyltetraphenylammonium borate.

[0103] As other transesterification catalysts, salts of zinc, tin, zirconium, lead, titanium, germanium, antimony, and osmium can be mentioned, for example, zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin chloride (II), tin chloride (IV), tin acetate (II), tin acetate (IV), dibutyltin dilaurate, dibutyltin oxide, dibutyltin dimethoxy, zirconium acetylacetonate, zirconium oxyacetate, tetrabutoxy zirconium, lead acetate (II), lead acetate (IV), tetrabutoxytitanium (IV), etc. The catalysts used in International Publication No. 2011 / 010741 and Japanese Patent Application Publication No. 2017-179323 can also be used.

[0104] Alternatively, a catalyst composed of aluminum or a compound thereof and a phosphorus compound may be used. In this case, the amount is preferably 80 μmol to 1000 μmol, more preferably 90 μmol to 800 μmol, and even more preferably 100 μmol to 600 μmol per 1 mol of the dihydroxy component.

[0105] As aluminum salts, organic acid salts and inorganic acid salts of aluminum can be cited. As organic acid salts of aluminum, for example, carboxylates of aluminum can be cited, specifically, aluminum formate, aluminum acetate, aluminum propionate, aluminum oxalate, aluminum acrylate, aluminum laurate, aluminum stearate, aluminum benzoate, aluminum trichloroacetate, aluminum lactate, aluminum citrate and aluminum salicylate can be cited. As inorganic acid salts of aluminum, for example, aluminum chloride, aluminum hydroxide, aluminum hydroxide chlorohydrate, aluminum carbonate, aluminum phosphate and aluminum phosphonate can be cited. As aluminum chelate compounds, for example, aluminum acetylacetonate, aluminum acetoacetate, ethyl aluminum acetoacetate, and ethyl acetoacetate aluminum diisopropoxy can be cited.

[0106] Examples of phosphorus compounds include phosphonic acid compounds, phosphinic acid compounds, phosphine oxide compounds, phosphinous acid compounds, phosphinous acid compounds, and phosphine compounds. Among them, phosphonic acid compounds, phosphinic acid compounds, and phosphine oxide compounds are particularly preferred, and phosphonic acid compounds are particularly preferred.

[0107] The amount of these polymerization catalysts used is preferably 0.1 μmol to 500 μmol, more preferably 0.5 μmol to 300 μmol, and further preferably 1 μmol to 100 μmol, based on 1 mol of the dihydroxy component.

[0108] In addition, a catalyst deactivator may be added in the later stage of the reaction. As the catalyst deactivator used, known catalyst deactivators can be effectively used, among which ammonium salts of sulfonic acids, Tetrabutyl dodecylbenzenesulfonate is further preferred. Salts of p-toluenesulfonic acid such as dodecylbenzenesulfonic acid salt and tetrabutylammonium p-toluenesulfonic acid salt.

[0109] As the ester of sulfonic acid, methyl benzenesulfonate, ethyl benzenesulfonate, butyl benzenesulfonate, octyl benzenesulfonate, phenyl benzenesulfonate, methyl p-toluenesulfonate, ethyl p-toluenesulfonate, butyl p-toluenesulfonate, octyl p-toluenesulfonate, phenyl p-toluenesulfonate and the like can be preferably used. Among them, tetrabutyl dodecylbenzenesulfonate is most preferably used. Salt.

[0110] The amount of these catalyst deactivators used is preferably 0.5 to 50 mol, more preferably 0.5 to 10 mol, and even more preferably 0.8 to 5 mol, relative to 1 mol of the catalyst when at least one polymerization catalyst selected from alkali metal compounds and / or alkaline earth metal compounds is used.

[0111] <Method for producing polyester carbonate resin>

[0112] The thermoplastic resin of the present invention may be a polyester carbonate resin. The polyester carbonate resin is produced by a conventional reaction method known per se for producing polyester carbonate resins, for example, by polycondensing a carbonate precursor such as a carbonic acid diester with a dicarboxylic acid or its ester derivative and a dihydroxy compound.

[0113] In the reaction of a dihydroxy compound, a dicarboxylic acid or its acid chloride with phosgene, the reaction is carried out in the presence of an acid binder and a solvent in a non-aqueous system. As the acid binder, for example, pyridine, dimethylaminopyridine, quaternary amine, etc. can be used. As the solvent, for example, a halogenated hydrocarbon such as dichloromethane and chlorobenzene can be used. As the molecular weight regulator, for example, a terminal terminator such as phenol and p-tert-butylphenol is preferably used. The reaction temperature is usually 0 to 40° C., and the reaction time is preferably several minutes to 5 hours.

[0114] In the transesterification reaction, a dihydroxy compound, a dicarboxylic acid or its diester and a diaryl carbonate are mixed under an inert gas atmosphere, and the reaction is carried out under reduced pressure at usually 120 to 350°C, preferably 150 to 300°C. The degree of reduced pressure is changed in stages, and finally reaches below 133 Pa, and the generated alcohols are distilled out of the system. The reaction time is usually about 1 to 4 hours. In addition, a polymerization catalyst can be used in the transesterification reaction to promote the reaction. As such a polymerization catalyst, it is preferred to use an alkali metal compound, an alkaline earth metal compound or a heavy metal compound as the main component, and a nitrogen-containing basic compound is further used as a secondary component as needed.

[0115] Examples of the alkali metal compound include sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate, sodium acetate, potassium acetate, lithium acetate, sodium stearate, potassium stearate, lithium stearate, sodium salt, potassium salt, lithium salt of bisphenol A, sodium benzoate, potassium benzoate, lithium benzoate, etc. Examples of the alkaline earth metal compound include calcium hydroxide, barium hydroxide, magnesium hydroxide, strontium hydroxide, calcium hydrogen carbonate, barium hydrogen carbonate, magnesium hydrogen carbonate, strontium hydrogen carbonate, calcium carbonate, barium carbonate, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, magnesium acetate, strontium acetate, calcium stearate, barium stearate, magnesium stearate, strontium stearate, etc.

[0116] Examples of the nitrogen-containing basic compound include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, trimethylbenzylammonium hydroxide, trimethylamine, triethylamine, dimethylbenzylamine, triphenylamine, and dimethylaminopyridine.

[0117] As other transesterification catalysts, the catalysts listed as the transesterification catalysts in the above-mentioned method for producing polycarbonate can be used in the same manner.

[0118] When the thermoplastic resin of the present invention is polyester carbonate, after the polymerization reaction is completed, the catalyst may be removed or deactivated in order to maintain thermal stability and hydrolytic stability. Generally, a method of deactivating the catalyst by adding a known acidic substance may be appropriately implemented. As these substances, specifically, esters such as butyl benzoate, aromatic sulfonic acids such as p-toluenesulfonic acid, aromatic sulfonic acid esters such as butyl p-toluenesulfonate and hexyl p-toluenesulfonate, phosphoric acids such as phosphorous acid, phosphoric acid, and phosphonic acid, triphenyl phosphite, monophenyl phosphite, diphenyl phosphite, diethyl phosphite, di-n-propyl phosphite, di-n-butyl phosphite, di-n-hexyl phosphite, dioctyl phosphite, monooctyl phosphite, phosphate esters such as triphenyl phosphate, diphenyl phosphate, monophenyl phosphate, dibutyl phosphate, dioctyl phosphate, monooctyl phosphate, phosphonic acids such as diphenylphosphonic acid, dioctylphosphonic acid, dibutylphosphonic acid, phosphonic acid esters such as diethyl phenylphosphonate, phosphines such as triphenylphosphine and bis(diphenylphosphino)ethane, boric acid, boric acid such as phenylboric acid, tetrabutyl dodecylbenzenesulfonate, Aromatic sulfonates such as salts, organic halides such as stearyl chloride, benzoyl chloride, and p-toluenesulfonyl chloride, alkyl sulfates such as dimethyl sulfate, and organic halides such as benzyl chloride. These deactivators are used in a ratio of 0.01 to 50 mol, preferably 0.3 to 20 mol, relative to 1 mol of the catalyst. If the amount is less than 0.01 mol relative to 1 mol of the catalyst, the deactivation effect is insufficient, which is not preferred. In addition, if the amount is more than 50 mol relative to 1 mol of the catalyst, the heat resistance decreases and the molded body becomes easily colored, which is not preferred.

[0119] After the catalyst is deactivated, a step of devolatilizing and removing low boiling point compounds in the thermoplastic resin at a pressure of 13.3 to 133 Pa and a temperature of 200 to 320° C. may be provided.

[0120] <Thermoplastic resin composition>

[0121] The thermoplastic resin of the present invention can be appropriately added with additives such as a release agent, a heat stabilizer, a UV absorber, a bluing agent, an antistatic agent, a flame retardant, a plasticizer, a filler, an antioxidant, a light stabilizer, a polymer metal deactivator, a lubricant, a surfactant, and an antibacterial agent as needed, and used in the form of a resin composition. As specific release agents and heat stabilizers, release agents and heat stabilizers described in International Publication No. 2011 / 010741 can be preferably cited.

[0122] As particularly preferred release agents, stearic acid monoglyceride, stearic acid triglyceride, pentaerythritol tetrastearate, a mixture of stearic acid triglyceride and stearyl stearate can be preferably used. In addition, the amount of the above ester in the release agent is preferably 90% by weight or more, and more preferably 95% by weight or more, when the release agent is set to 100% by weight. In addition, as a release agent mixed in a thermoplastic resin, it is preferably in the range of 0.005 to 2.0 parts by weight, more preferably in the range of 0.01 to 0.6 parts by weight, and further preferably in the range of 0.02 to 0.5 parts by weight relative to 100 parts by weight of the thermoplastic resin.

[0123] Examples of the heat stabilizer include phosphorus-based heat stabilizers, sulfur-based heat stabilizers, and hindered phenol-based heat stabilizers.

[0124] In addition, as particularly preferred phosphorus-based heat stabilizers, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite can be used. In addition, the content of the phosphorus-based heat stabilizer in the polycarbonate resin is preferably 0.001 to 0.2 parts by weight relative to 100 parts by weight of the thermoplastic resin.

[0125] In addition, a particularly preferred sulfur-based heat stabilizer is pentaerythritol-tetrakis(3-laurylthiopropionate). In addition, the content of the sulfur-based heat stabilizer in the thermoplastic resin is preferably 0.001 to 0.2 parts by weight relative to 100 parts by weight of the thermoplastic resin.

[0126] Preferred hindered phenol-based heat stabilizers include octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate].

[0127] The content of the hindered phenol-based heat stabilizer in the thermoplastic resin is preferably 0.001 to 0.3 parts by weight based on 100 parts by weight of the thermoplastic resin.

[0128] A phosphorus-based heat stabilizer and a hindered phenol-based heat stabilizer may be used in combination.

[0129] As the ultraviolet absorber, at least one ultraviolet absorber selected from the group consisting of benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, cyclic imidoester ultraviolet absorbers and cyanopropionate ultraviolet absorbers is preferred.

[0130] Among the benzotriazole-based ultraviolet absorbers, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole and 2,2′-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol] are more preferred.

[0131] Examples of the benzophenone-based ultraviolet absorber include 2-hydroxy-4-n-dodecyloxybenzophenone and 2-hydroxy-4-methoxy-2′-carboxybenzophenone.

[0132] Examples of the triazine-based ultraviolet absorber include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol and 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-[(octyl)oxy]-phenol.

[0133] As the cyclic urethane ultraviolet absorber, 2,2'-p-phenylenebis(3,1-benzo Oxazine-4-one).

[0134] Examples of the cyanopropionate-based ultraviolet absorber include 1,3-bis[(2′-cyano-3′,3′-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.

[0135] The amount of the ultraviolet absorber added is preferably 0.01 to 3.0 parts by weight based on 100 parts by weight of the thermoplastic resin. Within the above range, sufficient weather resistance can be imparted to the thermoplastic resin molded article depending on the intended use.

[0136] Examples of the antioxidant include triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,3,5-trimethyl-2,4,6-tris(3,5- tert-butyl-4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate), diethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane. The amount of the antioxidant to be added is preferably 0.50 parts by mass or less, more preferably 0.05 to 0.40 parts by mass, further preferably 0.05 to 0.20 parts by mass or 0.10 to 0.40 parts by mass, and particularly preferably 0.20 to 0.40 parts by mass, relative to 100 parts by mass of the thermoplastic resin composition.

[0137] <Optical components>

[0138] The optical component of the present invention comprises the above-mentioned thermoplastic resin. As such an optical component, as long as the above-mentioned thermoplastic resin is useful for optical purposes, it is not particularly limited, and can include optical disks, transparent conductive substrates, optical cards, sheets, films, optical fibers, lenses, prisms, optical films, base plates, optical filters, hard coatings, etc.

[0139] In addition, the optical component of the present invention can be composed of a resin composition comprising the above-mentioned thermoplastic resin, and the resin composition can be compounded with additives such as heat stabilizers, plasticizers, light stabilizers, polymer metal passivators, flame retardants, lubricants, antistatic agents, surfactants, antibacterial agents, ultraviolet absorbers, release agents, bluing agents, fillers, antioxidants, etc. as needed.

[0140] <Optical lens>

[0141] As the optical component of the present invention, an optical lens can be particularly mentioned. As such an optical lens, a photographing lens for a mobile phone, a smart phone, a tablet terminal, a personal computer, a digital camera, a video camera, a car camera, a surveillance camera, etc., and a sensor camera such as a TOF camera can be mentioned.

[0142] When the optical lens of the present invention is manufactured by injection molding, it is preferably molded under the conditions of a barrel temperature of 230 to 350°C and a mold temperature of 70 to 180°C. It is further preferred to mold under the conditions of a barrel temperature of 250 to 300°C and a mold temperature of 80 to 170°C. When the barrel temperature is higher than 350°C, the thermoplastic resin decomposes and colors, and when it is lower than 230°C, the melt viscosity is high and it tends to become difficult to mold. In addition, when the mold temperature is higher than 180°C, the molded sheet formed by the thermoplastic resin tends to become difficult to remove from the mold. On the other hand, when the mold temperature is less than 70°C, the resin in the mold dries up prematurely during molding, making the shape of the molded sheet difficult to control, or it tends to become difficult to fully transfer the shaping provided by the mold.

[0143] The optical lens of the present invention may be in the form of an aspherical lens as required. Since an aspherical lens can substantially reduce the spherical aberration by one lens, it is not necessary to remove the spherical aberration by combining multiple spherical lenses, and it is possible to achieve lightweighting and reduction in molding costs. Therefore, an aspherical lens is particularly useful as a camera lens among optical lenses.

[0144] In addition, the thermoplastic resin of the present invention is particularly useful as a material for thin-walled, small and complex-shaped optical lenses due to its high molding fluidity. As a specific lens size, the thickness of the center portion is 0.05 to 3.0 mm, more preferably 0.05 to 2.0 mm, and further preferably 0.1 to 2.0 mm. In addition, the diameter is 1.0 mm to 20.0 mm, more preferably 1.0 to 10.0 mm, and further preferably 3.0 to 10.0 mm. In addition, as its shape, it is preferably a concave-convex lens with one convex side and one concave side.

[0145] The thermoplastic resin lens of the present invention can be molded by any method such as mold molding, cutting, grinding, laser processing, electrical discharge machining, etching, etc. Among them, mold molding is more preferred from the viewpoint of production cost.

[0146] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited thereto.

[0147] Example

[0148] Evaluation was performed by the following method.

[0149] <Thermoplastic resin composition>

[0150] Measured by using JNM-ECZ400S manufactured by JEOL 1 H NMR, and calculate the copolymerization ratio of each thermoplastic resin.

[0151] <Refractive Index>

[0152] A 3 mm thick test piece of each thermoplastic resin was prepared and polished, and then the refractive index nd (587.56 nm) was measured using a Carnew precision refractometer KPR-2000 manufactured by Shimadzu Corporation.

[0153] <Abbe number>

[0154] The Abbe number (νd) was calculated using the following formula from the refractive index at a temperature of 20° C. and wavelengths of 486.13 nm, 587.56 nm, and 656.27 nm.

[0155] νd=(nd-1) / (nF-nC)

[0156] nd: refractive index at a wavelength of 587.56nm,

[0157] nF: refractive index at a wavelength of 486.13nm,

[0158] nC: refractive index at a wavelength of 656.27nm.

[0159] <Absolute value of orientation birefringence>

[0160] The thermoplastic resin was dissolved in dichloromethane, cast on a glass dish, and dried thoroughly to prepare a cast film with a thickness of 100 μm. The film was stretched 2 times at Tg+10°C, and the phase difference (Re) of 589 nm was measured using a polarization ellipsometer M-220 manufactured by JASCO Corporation. The absolute value of the oriented birefringence (|Δn|) was calculated using the following formula.

[0161] |Δn|=|Re / d|

[0162] Δn: Orientation birefringence

[0163] Re: Phase difference (nm)

[0164] d: thickness (nm)

[0165] <Glass transition temperature (Tg)>

[0166] The obtained thermoplastic resin was measured at a temperature increase rate of 20° C. / min using Discovery DSC25Auto manufactured by TA Instruments Japan Co., Ltd. The sample was measured in an amount of 5 to 10 mg.

[0167] <Example 1>

[0168] 197.33 g (0.45 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter, sometimes abbreviated to BPEF), 7.61 g (0.03 mol) of 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (hereinafter, sometimes abbreviated to SPG), 7.76 g (0.03 mol) of 4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol (hereinafter, sometimes abbreviated to BisTMC), 109.25 g (0.51 mol) of diphenyl carbonate, 62.5 μL of a sodium hydrogen carbonate aqueous solution having a concentration of 40 mmol / L (sodium hydrogen carbonate 2.5 μmol) as a catalyst, and 54.7 μL of a tetramethylammonium hydroxide aqueous solution having a concentration of 274 mmol / L (tetramethylammonium hydroxide 15 μmol) were heated to 180° C. in a nitrogen atmosphere to be melted. Then, the reduced pressure was adjusted to 20 kPa over 10 minutes. The temperature was raised to 250°C at a rate of 60°C / hr. After the outflow of phenol reached 70%, the pressure inside the reactor was reduced to below 133 Pa over 1 hour. The mixture was stirred for a total of 3.5 hours, and the resin was removed after the reaction was completed. 1 The copolymerization ratio of the obtained polycarbonate resin was measured by H NMR, and the refractive index, Abbe number, absolute value of orientation birefringence, and Tg of the polycarbonate resin were evaluated.

[0169] <Examples 2 to 5>

[0170] A polycarbonate resin was produced in the same manner as in Example 1 except that the monomer ratio was changed so that the copolymerization ratio of BPEF, SPG, and BisTMC became the ratio described in Table 1.

[0171] <Comparative Examples 1 to 4>

[0172] A polycarbonate resin was produced in the same manner as in Example 1 except that the monomer ratio was changed so that the copolymerization ratio of BPEF, SPG, and BisTMC became the ratio described in Table 1.

[0173] <Results>

[0174] The configurations of the respective Examples and Comparative Examples and the evaluation results thereof are summarized in Table 1 below.

[0175] Table 1

[0176]

[0177] BPEF: 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene

[0178] SPG: 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane

[0179] BisTMC: 4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol

[0180] Examples 1 to 5 can satisfy all of the requirements of a refractive index of about 1.600 to 1.660, an Abbe number, low birefringence, and heat resistance.

[0181] In both Comparative Examples 1 and 2, polycarbonate resins composed of BPEF, SPG, and BisTMC were exemplified. However, since the proportion of BPEF was small, the refractive index and birefringence were insufficient compared with those of the Examples.

[0182] In Comparative Example 3, a polycarbonate resin composed of BPEF and BisTMC was exemplified. However, since it did not contain SPG, its Tg was higher than that of the examples and it was not suitable for use as a molding material.

[0183] In Comparative Example 4, a polycarbonate resin composed of BPEF and SPG was exemplified. However, since BisTMC was not contained, Tg was lower than that of the examples and heat resistance was insufficient.

[0184] Industrial Applicability

[0185] The thermoplastic resin of the present invention can be used for optical materials, such as optical lenses, prisms, optical disks, transparent conductive substrates, optical cards, sheets, films, optical fibers, optical films, optical filters, hard coatings and other optical parts, and is particularly useful in optical lenses.

Claims

1. A thermoplastic resin comprising repeating units represented by formula (1), formula (2) and formula (3), wherein the repeating unit represented by formula (1) accounts for 60 mol% or more, and has a refractive index greater than 1.600 and less than 1.660, In formula (1), R 1 ~R 4 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, In formula (3), n is in the range of 1 to 8, R 5 and R 6 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and R 7 It represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.

2. The thermoplastic resin according to claim 1, in, The repeating unit of the formula (1) is 60 mol% to 80 mol%.

3. The thermoplastic resin according to claim 1 or 2, in, R of the formula (1) 1 ~R 4 A hydrogen atom.

4. The thermoplastic resin according to any one of claims 1 to 3, in, The repeating unit of the formula (3) is a repeating unit derived from 4,4'-(3,3,5-trimethylcyclohexylidene)bisphenol.

5. The thermoplastic resin according to any one of claims 1 to 4, in, The glass transition temperature is 130-160°C.

6. The thermoplastic resin according to any one of claims 1 to 5, in, The absolute value of the orientation birefringence is 3.0×10 -3 the following.

7. The thermoplastic resin according to any one of claims 1 to 5, in, The absolute value of the orientation birefringence is 1.0×10 -3 the following.

8. The thermoplastic resin according to any one of claims 1 to 7, in, The Abbe number is 24.0~29.