Electrochemical device and electronic device

By coating the silicon-based material on the negative electrode sheet of the lithium-ion battery and setting up a polymer particle layer, the electrode fragment fracture and interface problems caused by silicon-based expansion are solved, and the energy density and reliability of the lithium-ion battery are improved.

CN118922957AActive Publication Date: 2024-11-08NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202380025303.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-07
Publication Date
2024-11-08
Estimated Expiration
2043-12-07

AI Technical Summary

Technical Problem

The ultra-high volume expansion of the silicon-based negative electrode material during charging and discharging of lithium-ion batteries leads to damage to the interface of solid electrolyte and fracture of corner poles, reducing the life and reliability of lithium-ion batteries.

Method used

By coating the first negative electrode active material layer containing silicon-based material on the negative electrode sheet and providing a polymer particle layer on the surface of the diaphragm, a corner area space is reserved to match the different silicon element content and polymer particle layer thickness to Overcome the problems of pole fragment fracture and circulating lithium excretion caused by expansion.

Benefits of technology

Effectively reserve corner space to buffer the pole plate extrusion and breakage, improve the energy density of lithium-ion batteries, optimize the cyclic lithium-ion problem, and extend the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922957A_ABST
    Figure CN118922957A_ABST
Patent Text Reader

Abstract

The invention discloses an electrochemical device and an electronic device. The electrochemical device comprises a positive pole piece, a negative pole piece and a diaphragm, the negative pole piece comprises a negative current collector, and a first negative active material layer containing a silicon-based material is arranged on the surface of the negative current collector; the diaphragm is arranged between the negative pole piece and the positive pole piece; and a polymer particle layer is arranged on the surface of the diaphragm adjacent to the first negative electrode active material layer. The diaphragm coated with the polymer particle layers with different thicknesses is matched according to different silicon contents in the negative electrode active material layer coated on the surface of the negative electrode current collector in the negative electrode plate, so that a corner space can be reserved to buffer extrusion and breakage of the electrode plate, the problems of breakage of the electrode plate and cyclic lithium precipitation caused by silicon-based expansion are solved, and meanwhile, the energy density is maximized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to electrochemical devices and electronic devices. Background Art

[0002] Since silicon has a reversible capacity of up to 4200mAh / g, silicon-based negative electrode materials are considered to be one of the effective strategies to improve the energy density of lithium-ion batteries. However, when lithium ions are embedded and extracted during the charge and discharge process, silicon particles will expand by more than 300%. The ultra-high volume expansion will bring a series of problems. First, the ultra-high volume expansion will damage the solid electrolyte interface (SEI) membrane, causing the electrolyte to penetrate into the negative electrode plate, triggering a series of unstable reactions, such as the decomposition of the electrolyte and the repeated formation of SEI, which will lead to the attenuation of the capacity and performance instability of the lithium-ion battery; secondly, the volume expansion of silicon may also cause the problem of corner pole piece fracture. The corner pole piece must remain stable during the charge and discharge cycle of the lithium-ion battery, and the volume expansion of silicon may cause stress concentration in the corner pole piece, eventually leading to fracture, thereby reducing the life and reliability of the lithium-ion battery. Summary of the invention

[0003] In view of the above-mentioned problems existing in the prior art, the present application proposes an electrochemical device and an electronic device, which configures and designs the silicon content of the negative electrode pole piece and the polymer particle layer on the surface of the diaphragm, and reserves space in the corner area to buffer the extrusion, aiming to solve the corner fracture and interface problems of the negative electrode pole piece caused by silicon-based expansion, while improving the energy density of lithium-ion batteries.

[0004] In a first aspect, the present application provides an electrochemical device comprising a positive electrode plate, a negative electrode plate and a separator; the negative electrode plate comprises a negative electrode collector, and a first negative electrode active material layer containing a silicon-based material is arranged on the surface of the negative electrode collector; the separator is arranged between the negative electrode plate and the positive electrode plate; a polymer particle layer is arranged on the surface of the separator adjacent to the first negative electrode active material layer.

[0005] Based on the mass of the first negative electrode active material layer, the mass percentage of silicon element is X; the thickness of the polymer particle layer is H, in some embodiments, 0<X<2%, 0<H<1μm. In some embodiments, 2%≤X<10%, 1μm≤H<2.8μm. In some embodiments, 10%≤X<25%, 2.8μm≤H<4μm. In some embodiments, 25%≤X≤30%, 4μm≤H≤5μm. The thickness of the polymer particle layer is the thickness of the straight area, and the thickness of the polymer particle layer in the corner area is greater than the thickness of the polymer particles in the straight area. This is because in the battery preparation process, after winding, formation and hot pressing, due to the influence of hot pressing, the polymer particle layer in the straight area is flattened, and the thickness of the polymer layer in the corner area does not change much. When the polymer particle layer after hot pressing satisfies this relationship, it must be ensured that the space reserved in the corner area is sufficient to withstand the stress generated by the expansion of the corner area. The diaphragm coated with polymer particle layers of different thicknesses is matched according to the different silicon contents in the negative electrode active material layer coated on the surface of one side of the negative electrode current collector in the negative electrode pole piece. This can reserve corner space to buffer the pole piece extrusion and fracture, overcome the pole piece fracture and cyclic lithium deposition problems caused by silicon-based expansion, and maximize energy density.

[0006] In some embodiments, 2% ≤ X < 5%, 1.5 μm ≤ H < 2.5 μm. In some embodiments, 5% ≤ X < 10%, 2.5 μm ≤ H < 2.8 μm. In some embodiments, 10% ≤ X < 15%, 2.8 μm ≤ H < 3.5 μm. In some embodiments, 15% ≤ X ≤ 20%, 3.5 μm ≤ H < 4 μm. When the silicon content in the negative active material layer coated on the surface of the negative current collector on one side of the negative electrode sheet and the thickness of the polymer particle layer on the matching diaphragm meet this rule, the problem of cyclic lithium deposition is further optimized and improved.

[0007] In some embodiments, the separator adjacent to the first negative electrode active material layer is provided with a polymer particle layer on its surface away from the first negative electrode active material layer.

[0008] In some embodiments, the separator adjacent to the first negative electrode active material layer is provided with an adhesive layer on a surface thereof facing the first negative electrode active material layer, and the thickness of the adhesive layer is preferably 0 to 1 μm.

[0009] In some embodiments, the bonding layer can be selected from at least one material of homopolymers or copolymers of methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, ethylene, styrene, chlorostyrene, fluorostyrene, methylstyrene, acrylic acid, methacrylic acid, methacrylonitrile, and maleic acid. In some embodiments, the bonding layer is preferably a polymer of acrylic acid, acrylate, styrene, isobutyl acrylate, or acrylonitrile.

[0010] In some embodiments, the first negative electrode active material layer includes a negative electrode active material, the negative electrode active material includes a silicon-based active material, and the silicon-based material is selected from at least one of silicon, silicon oxides, silicon carbon compounds, or silicon alloys. In some embodiments, the silicon-based active material is preferably silicon carbon particles.

[0011] In some embodiments, the negative electrode active material includes a carbon active material, and the carbon active material is selected from at least one of graphite or hard carbon. In some embodiments, the carbon active material is preferably graphite.

[0012] In some embodiments, based on the mass of the first negative electrode active material layer, the mass percentage content X of silicon preferably satisfies 2%≤X≤5%. When silicon satisfies this range, the expansion of silicon can be better controlled and the lithium precipitation problem can be improved.

[0013] In some embodiments, a second negative electrode active material layer is disposed on the other surface of the negative electrode current collector; the second negative electrode active material layer does not contain silicon. In this case, silicon is distributed in the active material layer on one surface of the negative electrode current collector.

[0014] In some embodiments, the second negative electrode active material layer does not contain silicon element, and no polymer particle layer exists on the surface of the separator adjacent to the second negative electrode active material layer.

[0015] In some embodiments, the second negative electrode active material layer does not contain silicon, and the separator adjacent to the second negative electrode active material layer includes a substrate, an inorganic coating coated on one side of the substrate, and an adhesive layer coated on the surface of the inorganic coating. In some embodiments, the adhesive layer is coated on the other side of the substrate of the separator.

[0016] In some embodiments, the bonding layer can be selected from at least one material of homopolymers or copolymers of methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, ethylene, styrene, chlorostyrene, fluorostyrene, methylstyrene, acrylic acid, methacrylic acid, methacrylonitrile, and maleic acid. In some embodiments, the bonding layer is preferably a polymer of acrylic acid, acrylate, styrene, isobutyl acrylate, or acrylonitrile.

[0017] In some embodiments, the thickness of the adhesive layer is preferably 0 to 1 μm.

[0018] In some embodiments, a second negative electrode active material layer is disposed on the other surface of the negative electrode current collector; the second negative electrode active material layer contains silicon. Based on the mass of the second negative electrode active material layer, the mass percentage of silicon is also X. At this time, silicon is evenly distributed in the active material layer on both sides of the negative electrode current collector.

[0019] In some embodiments, the second negative electrode active material layer includes silicon, and a polymer particle layer is disposed on one surface of the separator adjacent to the second negative electrode active material layer.

[0020] In some embodiments, the second negative electrode active material layer includes silicon, and the separator adjacent to the second negative electrode active material layer is provided with a polymer particle layer on a surface thereof away from the second negative electrode active material layer.

[0021] In some embodiments, the second negative electrode active material layer includes silicon element, and the separator adjacent to the second negative electrode active material layer does not have a polymer particle layer on a surface thereof facing the second negative electrode active material layer.

[0022] In some embodiments, the polymer particle layer is selected from at least one of homopolymers or copolymers of vinylidene fluoride, hexafluoropropylene, ethylene, propylene, vinyl chloride, allyl chloride, acrylic acid, acrylate, styrene, butadiene, and acrylonitrile. In some embodiments, the polymer particle layer is preferably polyvinylidene fluoride.

[0023] In some embodiments, the separator adjacent to the first negative active material layer includes a substrate and an inorganic coating layer disposed between the substrate and the polymer particle layer.

[0024] In some embodiments, a bonding layer is coated on the other surface of the substrate of the separator adjacent to the first negative electrode active material layer.

[0025] In some embodiments, the inorganic coating is selected from at least one material of boehmite, magnesium hydroxide, aluminum oxide, titanium dioxide, silicon dioxide, zirconium dioxide, tin dioxide, magnesium oxide, zinc oxide, barium sulfate, boron nitride, aluminum nitride, or silicon nitride.

[0026] In some embodiments, the inorganic coating is preferably boehmite. In some embodiments, the thickness of the inorganic coating is preferably 0.5 μm to 6 μm.

[0027] In some embodiments, the substrate is selected from at least one material selected from a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric, or a polypropylene-polyethylene-polypropylene porous composite film.

[0028] In some embodiments, the substrate is preferably a polyethylene (PE) porous polymer film. In some embodiments, the thickness of the substrate is preferably 3 μm to 6 μm.

[0029] In a second aspect, the present application provides an electronic device, which includes the electrochemical device of the first aspect.

[0030] Beneficial effects:

[0031] Based on the easy expansion property of silicon-based negative electrodes, the present application proposes a matching design scheme for silicon-based negative electrode plates and diaphragms. By matching the diaphragms coated with polymer particle layers of different thicknesses according to the different silicon contents in the negative electrode active material layer coated on the surface of one side of the negative electrode current collector in the negative electrode plate, corner space can be reserved to buffer the extrusion and fracture of the plate, thereby overcoming the problems of plate fracture and cyclic lithium deposition caused by silicon-based expansion, while maximizing energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The following will briefly describe the drawings necessary for describing the embodiments of the present application or the prior art to facilitate the description of the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, drawings of other embodiments can still be obtained based on the structures illustrated in these drawings.

[0033] Figure 1 This is a schematic diagram of the design of the negative electrode plate of Example 1 of the present application.

[0034] Figure 2 This is a schematic diagram of the design of a separator matching the first negative electrode active material layer of Example 1 of the present application.

[0035] Figure 3 This is a schematic diagram of the design of the battery of Example 1 of the present application.

[0036] Figure 4 This is a schematic diagram of the winding effect of the battery before compression in Example 1 of the present application.

[0037] Figure 5 This is a schematic diagram of the winding effect of the battery after compression in Example 1 of the present application.

[0038] Figure 6 This is a surface picture of the separator before compression matching the first negative electrode active material layer of Example 1 of the present application.

[0039] Figure 7 This is a side view of the compressed separator matching the first negative electrode active material layer of Example 1 of the present application.

[0040] Figure 8 This is a schematic diagram of the design of the negative electrode plate of Example 22 of the present application.

[0041] Fig. 9 This is a schematic diagram of the design of the battery of Example 22 of the present application.

[0042] Fig.10 This is a schematic diagram of the winding effect of the battery before compression in Example 22 of the present application.

[0043] Figure numbers: 1-silicon carbon particles, 2-graphite, 3-negative electrode current collector, 4-substrate, 5-polymer particles, 6-inorganic coating, 7-positive electrode plate, 8-first negative electrode active material layer, 9-second negative electrode active material layer, 10-negative electrode plate, 11-diaphragm. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical scheme and advantages of the present application clearer, the technical scheme of the present application will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of the present application. The embodiments of the present application should not be interpreted as limiting the present application.

[0045] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0046] In the description herein, unless otherwise specified, “above” and “below” include the number.

[0047] Unless otherwise specified, the terms used in this application have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values ​​of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).

[0048] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0049] In the detailed description and claims, a list of items connected by the terms "one of," "one of," "one of," or other similar terms may mean any of the listed items. For example, if items A and B are listed, then the phrase "one of A and B" means only A; or only B. In another example, if items A, B, and C are listed, then the phrase "one of A, B, and C" means only A; or only B; or only C.

[0050] In the description of this article, it should also be noted that the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.

[0051] In the first aspect, the present application provides an electrochemical device, including a positive electrode sheet, a negative electrode sheet and a separator; the negative electrode sheet includes a negative electrode current collector, and a first negative electrode active material layer containing a silicon-based material is arranged on the surface of the negative electrode current collector; the separator is arranged between the negative electrode sheet and the positive electrode sheet; a polymer particle layer is arranged on the surface of the separator adjacent to the first negative electrode active material layer. Based on the mass of the first negative electrode active material layer, the mass percentage of silicon element is X; the thickness of the polymer particle layer is H, in some embodiments, 0<X<2%, 0<H<1μm. In some embodiments, 2%≤X<10%, 1μm≤H<2.8μm. In some embodiments, 10%≤X<25%, 2.8μm≤H<4μm. In some embodiments, 25%≤X≤30%, 4μm≤H≤5μm.

[0052] The present application provides a diaphragm coated with polymer particle layers of different thicknesses according to the different silicon contents in the negative electrode active material layer coated on the surface of the negative electrode current collector in the negative electrode plate, which can reserve corner space to buffer the extrusion and fracture of the plate, overcome the problems of plate fracture and lithium deposition in the cyclic corners caused by silicon-based expansion, and maximize energy density.

[0053] In some embodiments, 2% ≤ X < 5%, 1.5 μm ≤ H < 2.5 μm. In some embodiments, 5% ≤ X < 10%, 2.5 μm ≤ H < 2.8 μm. In some embodiments, 10% ≤ X < 15%, 2.8 μm ≤ H < 3.5 μm. In some embodiments, 15% ≤ X ≤ 20%, 3.5 μm ≤ H < 4 μm. When the silicon content in the negative electrode active material layer coated on the surface of one side of the negative electrode current collector in the negative electrode sheet and the thickness of the polymer particle layer on the matching diaphragm meet this rule, the problem of lithium deposition in the cycle corner is further improved.

[0054] In some embodiments, the separator adjacent to the first negative electrode active material layer is provided with a polymer particle layer on its surface away from the first negative electrode active material layer.

[0055] In some embodiments, the separator adjacent to the first negative electrode active material layer is provided with an adhesive layer on its surface facing the first negative electrode active material layer. Since the polymer particle layer has a weaker adhesiveness and the adhesive layer has a stronger adhesiveness, in order to avoid the separation between the pole piece and the separator caused by the large expansion of the first negative electrode active material layer, it is preferred to place the side of the separator with the adhesive layer close to the side of the first negative electrode active material layer to ensure good adhesion between the first negative electrode active layer and the separator.

[0056] In some embodiments, the first negative electrode active material layer includes a negative electrode active material, the negative electrode active material includes a silicon-based active material, and the silicon-based material is selected from at least one of silicon, silicon oxides, silicon carbon compounds, or silicon alloys. In some embodiments, the silicon-based active material is preferably silicon carbon particles.

[0057] In some embodiments, the negative electrode active material includes a carbon active material, and the carbon active material is selected from at least one of graphite or hard carbon. In some embodiments, the carbon active material is preferably graphite.

[0058] In some embodiments, based on the mass of the first negative electrode active material layer, the mass percentage X of silicon preferably satisfies 2%≤X<5%. When the silicon element satisfies this range, the expansion of silicon can be better controlled and the lithium precipitation problem can be improved.

[0059] In some embodiments, a second negative electrode active material layer is disposed on the other surface of the negative electrode current collector; the second negative electrode active material layer does not contain silicon. In this case, silicon is distributed in the active material layer on one surface of the negative electrode current collector.

[0060] In some embodiments, when the second negative electrode active material layer does not include silicon element, there is no polymer particle layer on the surface of the separator adjacent to the second negative electrode active material layer.

[0061] In some embodiments, the second negative electrode active material layer does not contain silicon, and the separator adjacent to the second negative electrode active material layer includes a substrate, an inorganic coating coated on one side of the substrate, and an adhesive layer coated on the surface of the inorganic coating. In some embodiments, the adhesive layer is coated on the other side of the substrate of the separator.

[0062] In some embodiments, the bonding layer can be selected from at least one material of homopolymers or copolymers of methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, ethylene, styrene, chlorostyrene, fluorostyrene, methylstyrene, acrylic acid, methacrylic acid, methacrylonitrile, and maleic acid. In some embodiments, the bonding layer is preferably a polymer of acrylic acid, acrylate, styrene, isobutyl acrylate, or acrylonitrile.

[0063] In some embodiments, the thickness of the adhesive layer is preferably 0 to 1 μm. In some embodiments, a second negative electrode active material layer is provided on the other surface of the negative electrode current collector; the second negative electrode active material layer contains silicon. Based on the mass of the second negative electrode active material layer, the mass percentage of silicon is also X. At this time, silicon is evenly distributed in the active material layer on both sides of the negative electrode current collector.

[0064] In some embodiments, the second negative electrode active material layer includes silicon, and a polymer particle layer is disposed on one surface of the separator adjacent to the second negative electrode active material layer.

[0065] In some embodiments, the second negative electrode active material layer includes silicon, and a polymer particle layer is disposed on a surface of the separator adjacent to the second negative electrode active material layer away from the second negative electrode active material layer.

[0066] In some embodiments, the second negative electrode active material layer includes silicon element, and the separator adjacent to the second negative electrode active material layer does not have a polymer particle layer on a surface thereof facing the second negative electrode active material layer.

[0067] In some embodiments, the polymer particle layer is selected from at least one of homopolymers or copolymers of vinylidene fluoride, hexafluoropropylene, ethylene, propylene, vinyl chloride, allyl chloride, acrylic acid, acrylate, styrene, butadiene, and acrylonitrile. In some embodiments, the polymer particle layer is preferably polyvinylidene fluoride.

[0068] In some embodiments, the separator adjacent to the first negative electrode active material layer includes a substrate and an inorganic coating, and the inorganic coating is disposed between the substrate and the polymer particle layer. The present application has no particular restrictions on the inorganic coating, for example, the inorganic coating can be selected from at least one material of boehmite, magnesium hydroxide, aluminum oxide, titanium dioxide, silicon dioxide, zirconium dioxide, tin dioxide, magnesium oxide, zinc oxide, barium sulfate, boron nitride, aluminum nitride or silicon nitride.

[0069] In some embodiments, a bonding layer is coated on the other surface of the substrate of the separator adjacent to the first negative electrode active material layer.

[0070] In some embodiments, the inorganic coating is preferably boehmite. In some embodiments, the thickness of the inorganic coating is preferably 0.5 μm to 6 μm.

[0071] In some embodiments, the substrate is selected from at least one material selected from a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric, or a polypropylene-polyethylene-polypropylene porous composite film.

[0072] In some embodiments, the substrate is preferably a polyethylene (PE) porous polymer film. In some embodiments, the thickness of the substrate is preferably 3 μm to 6 μm.

[0073] In some embodiments, the negative electrode current collector may be copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or a combination thereof.

[0074] In some embodiments, the first negative electrode active material layer further includes a conductive agent and a binder. The binder includes, but is not limited to: at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinyl ether or styrene-butadiene rubber. In some embodiments, the conductive agent can use any conductive material as long as it does not cause chemical changes. In some embodiments, the conductive agent includes at least one of conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, carbon fiber or graphene.

[0075] In some embodiments, the positive electrode sheet includes a positive active material layer and a positive current collector.

[0076] In some embodiments, the positive electrode active material layer includes a positive electrode active material. In some embodiments, the positive electrode active material includes at least one of a nickel-cobalt ternary material and a phosphate-based material. In some embodiments, the nickel-cobalt ternary material includes LiNi x Co y M (1-x-y) At least one of the O2 materials, M includes at least one of manganese, aluminum, magnesium, chromium, calcium, zirconium, molybdenum, silver or niobium, 0.5≤x≤1, 0≤y≤0.5, x+y≤1. In some embodiments, the phosphate-based material includes LiMn k B (1-k)PO4, 0≤k≤1, B element includes at least one of iron, cobalt, magnesium, calcium, zinc, chromium or lead. In some preferred embodiments, the positive active material is selected from nickel-cobalt ternary materials. In some embodiments, the positive active material may have a coating on the surface, or may be mixed with another compound having a coating. In some embodiments, the coating may include at least one coating element compound selected from an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. The compound used for the coating may be amorphous or crystalline. The coating elements contained in the coating may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or a mixture thereof. The coating may be applied by any method as long as the method does not adversely affect the performance of the positive active material. For example, the method may include any coating method well known to those of ordinary skill in the art, such as spraying, dipping, and the like.

[0077] In some embodiments, the positive electrode active material layer further includes a conductive agent and a binder. In some embodiments, the binder includes, but is not limited to: polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, styrene butadiene rubber or acrylic (ester) styrene butadiene rubber, etc. In some embodiments, the conductive agent includes, but is not limited to: carbon-based materials, metal-based materials, conductive polymers and mixtures thereof. In some embodiments, the carbon-based material is selected from graphite, carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, graphene or any combination thereof. In some embodiments, the metal-based material is selected from metal powder, metal fiber, copper, nickel, aluminum or silver. In some embodiments, the conductive polymer is a polyphenylene derivative.

[0078] In some embodiments, the positive electrode plate further includes a positive current collector, which may be a metal foil or a composite current collector. For example, aluminum foil may be used. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer substrate.

[0079] In some embodiments, the electrochemical device further includes an electrolyte comprising a lithium salt and a non-aqueous solvent.

[0080] In some embodiments, the lithium salt is selected from one or more of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB and lithium difluoroborate. For example, the lithium salt can be selected from LiPF6.

[0081] In some embodiments, the non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents, or a combination thereof.

[0082] The carbonate compound may be a linear carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof.

[0083] Examples of the above-mentioned linear carbonate compounds are dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) and combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate and combinations thereof.

[0084] Examples of the above carboxylic acid ester compounds are methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid lactone, valerolactone, mevalonolactone, caprolactone and combinations thereof.

[0085] Examples of the above ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, and combinations thereof.

[0086] Examples of the above other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate and phosphoric acid esters and combinations thereof.

[0087] According to some embodiments of the present application, the electrochemical device of the present application includes, but is not limited to: all kinds of primary batteries or secondary batteries. In some embodiments, the electrochemical device is a lithium secondary battery. In some embodiments, the lithium secondary battery includes, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0088] In a second aspect, the electronic device of the present application may be any device using the electrochemical device of the first aspect of the present application.

[0089] In some embodiments, the electronic device includes, but is not limited to: laptop computers, pen-type computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries or lithium-ion capacitors, etc.

[0090] Examples and Comparative Examples

[0091] Hereinafter, the present application will be described in more detail with reference to Examples and Comparative Examples, but the present application is not limited to these Examples unless departing from the gist of the present application.

[0092] Preparation of lithium-ion batteries

[0093] Example 1

[0094] (1) Preparation of negative electrode sheet

[0095] Copper foil is used as the negative electrode current collector, 87.84wt% artificial graphite, 9.76wt% silicon carbon, 0.5wt% carboxymethyl cellulose (CMC), 1.7wt% polyacrylic acid (PAA) and 0.2% carbon nanotubes are fully stirred and mixed in an appropriate amount of deionized water to form a first negative electrode slurry. The first negative electrode slurry is evenly coated on one side of the copper foil (i.e., side A), 97.6wt% artificial graphite, 1.3wt% carboxymethyl cellulose (CMC) and 1.1wt% styrene-butadiene rubber (SBR) are fully stirred in an appropriate amount of deionized water to form a second negative electrode slurry, and the second negative electrode slurry is evenly coated on the other side of the copper foil (i.e., side B, the opposite side of side A), and then dried and cold pressed, and then cut into pieces and welded to the pole ears to prepare the negative electrode sheet. The active material layer on the negative electrode current collector A is the first negative electrode active material layer, in which the mass percentage of silicon element is 4.3%; the active material layer on the negative electrode current collector B is the second negative electrode active material layer, in which the mass percentage of silicon element is 0 (a silicon element percentage of no more than 0.5% can be considered to contain no silicon element).

[0096] (2) Preparation of positive electrode sheet

[0097] Aluminum foil is used as the positive electrode current collector. 97.8wt% lithium cobalt oxide (LCO), 0.8wt% polyvinylidene fluoride (PVDF) and 1.4wt% conductive carbon black are fully stirred and mixed in an appropriate amount of N-methylpyrrolidone solvent to form a uniform positive electrode slurry. The positive electrode slurry is evenly coated on the surface of both sides of the aluminum foil, and then dried and cold pressed, and then cut into pieces and welded to the pole ears to prepare the positive electrode sheet.

[0098] (3) Preparation of electrolyte

[0099] In a dry argon environment, LiPF6 was added to a solvent mixed with propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio of 1:1:1) and mixed evenly to obtain an electrolyte, wherein the concentration of LiPF6 was 1.15 mol / L.

[0100] (4) Preparation of diaphragm

[0101] The diaphragm (first diaphragm) matched by the first negative electrode active material layer includes a substrate, an inorganic coating coated on the surface of one side of the substrate, and a polymer particle layer coated on the surface of the inorganic coating. Among them, the substrate is a 4.5μm thick polyethylene (PE) porous polymer film, the inorganic coating is a 2μm thick boehmite, and the polymer particle layer is a 2μm thick polyvinylidene fluoride. An adhesive layer is coated on the other side of the substrate of the first diaphragm, and the adhesive layer is acrylic acid or an acrylate polymer. The diaphragm (second diaphragm) matched by the second negative electrode active material layer includes a substrate, an inorganic coating coated on the surface of one side of the substrate, and an adhesive layer coated on the surface of the inorganic coating. An adhesive layer is coated on the other side of the substrate of the second diaphragm. Among them, the substrate is a 4.5μm thick polyethylene (PE) porous polymer film, the inorganic coating is a 2μm thick boehmite, and the adhesive layer is an acrylic acid or an acrylate polymer.

[0102] (5) Preparation of lithium-ion batteries

[0103] The positive electrode sheet and the negative electrode sheet are wound after being stripped, and the positive electrode sheet and the negative electrode sheet are separated by a diaphragm, wherein the first negative electrode active material layer matches the diaphragm coated with a polymer particle layer on one side, and the polymer particle layer on the diaphragm is placed toward one side of the positive electrode sheet, and the second negative electrode active material layer matches the diaphragm without a polymer particle layer. Stack them in order so that the diaphragm plays an isolating role, and wind them to obtain a bare cell. The bare cell is hot pressed, top and side sealed, sprayed with code, vacuum dried, injected with electrolyte, and placed at high temperature for pressure formation and capacity measurement to obtain a finished lithium-ion battery.

[0104] Example 2-19

[0105] The preparation method of the lithium ion battery provided in Examples 2-19 can refer to Example 1, except that:

[0106] Adjust the mass percentage of silicon element in the active material layer on the surface of the negative electrode collector A (the first negative electrode active material layer) and the thickness of the polymer particle layer of the matching diaphragm (the first diaphragm), and adaptively adjust the mass percentage data of artificial graphite, carboxymethyl cellulose, styrene-butadiene rubber and conductive carbon black in the first negative electrode active material layer. For specific data, please see Table 1 below.

[0107] Embodiment 20

[0108] The preparation method of the lithium ion battery provided in this embodiment can refer to Example 1, except that:

[0109] The silicon-based material in the active material layer on the surface of the negative electrode collector A (the first negative electrode active material layer) is a silicon-oxygen material. The mass percentage of the silicon element and the thickness of the polymer particle layer of the matching diaphragm (the first diaphragm) are adjusted, and the mass percentage data of the artificial graphite, carboxymethyl cellulose, styrene-butadiene rubber and conductive carbon black in the first negative electrode active material layer are adaptively adjusted. For specific data, please see Table 1 below.

[0110] Embodiment 21

[0111] The preparation method of the lithium ion battery provided in this embodiment can refer to Example 1, except that:

[0112] The silicon-based material in the active material layer on the surface of the negative electrode collector A (the first negative electrode active material layer) is a silicon material. The mass percentage of the silicon element and the thickness of the polymer particle layer of the matching diaphragm (the first diaphragm) are adjusted, and the mass percentage data of the artificial graphite, carboxymethyl cellulose, styrene-butadiene rubber and conductive carbon black in the first negative electrode active material layer are adaptively adjusted. For specific data, please see Table 1 below.

[0113] Comparative Examples 1-6

[0114] The preparation method of the lithium ion battery provided in Comparative Examples 1-6 can refer to Examples 1-19, except that:

[0115] Adjust the mass percentage of silicon element in the active material layer on the surface of the negative electrode collector A (the first negative electrode active material layer) and the thickness of the polymer particle layer of the matching diaphragm (the first diaphragm), and adaptively adjust the mass percentage data of artificial graphite, carboxymethyl cellulose, styrene-butadiene rubber and conductive carbon black in the first negative electrode active material layer. For specific data, please see Table 1 below.

[0116] Embodiment 22

[0117] The preparation method of the lithium ion battery provided in this embodiment can refer to Example 1, except that:

[0118] (1) Preparation of negative electrode sheet

[0119] Copper foil is used as a negative electrode current collector, 92.2wt% artificial graphite, 5.6wt% silicon carbon, 0.5wt% carboxymethyl cellulose (CMC), 1.5wt% polyacrylic acid (PAA) and 0.2% conductive carbon nanotubes are fully mixed in an appropriate amount of deionized water to form a negative electrode slurry, the negative electrode slurry is evenly coated on both sides of the copper foil (i.e., side A and side B), and then dried and cold pressed, and then cut into pieces and welded to the pole ears to prepare a negative electrode sheet, the active material layer on the negative electrode current collector A side is a first negative electrode active material layer, wherein the mass percentage of silicon element is 2.5%, and the active material layer on the negative electrode current collector B side is a second negative electrode active material layer, wherein the mass percentage of silicon element is 2.5%.

[0120] (4) Preparation of diaphragm

[0121] The separator (first separator) matched with the first negative electrode active material layer and the separator (second separator) matched with the second negative electrode active material layer both include a substrate, an inorganic coating coated on one side of the substrate, and a polymer particle layer coated on the surface of the inorganic coating. The substrate is a 4.5 μm thick polyethylene (PE) porous polymer film, the inorganic coating is a 1.8 μm thick boehmite, and the polymer particle layer is a 1.8 μm thick polyvinylidene fluoride.

[0122] (5) Preparation of lithium-ion batteries

[0123] The positive and negative pole pieces are wound after being stripped, and the positive and negative pole pieces are separated by a diaphragm, wherein the polymer particle layer on the diaphragm is placed toward one side of the positive pole piece. Stack them in order so that the diaphragm plays an isolating role, and then wind them to obtain a bare cell. The bare cell is hot pressed, top and side sealed, sprayed with code, vacuum dried, injected with electrolyte, and placed at high temperature for pressure formation and capacity measurement to obtain a finished lithium-ion battery.

[0124] Embodiment 23-33

[0125] The preparation methods of the lithium ion batteries provided in Examples 23-33 can refer to Example 22, except that:

[0126] Adjust the mass percentage of silicon element in the active material layer on the surface of the negative electrode collector A (the first negative electrode active material layer) and the thickness of the polymer particle layer of the matching diaphragm (the first diaphragm), and adaptively adjust the mass percentage data of artificial graphite, carboxymethyl cellulose, styrene-butadiene rubber and conductive carbon black in the first negative electrode active material layer and the thickness of the inorganic coating of the first diaphragm and the second diaphragm. For specific data, please see Table 2 below.

[0127] Comparative Examples 7-12

[0128] The preparation methods of the lithium ion batteries provided in Comparative Examples 7-12 can refer to Example 22, except that:

[0129] Adjust the mass percentage of silicon element in the active material layer on the surface of the negative electrode collector A (the first negative electrode active material layer) and the thickness of the polymer particle layer of the matching diaphragm (the first diaphragm), and adaptively adjust the mass percentage data of artificial graphite, carboxymethyl cellulose, styrene-butadiene rubber and conductive carbon black in the first negative electrode active material layer and the thickness of the inorganic coating of the first diaphragm and the second diaphragm. For specific data, please see Table 2 below.

[0130] Test Method

[0131] 1. Silicon element test

[0132] The silicon content in the present invention refers to the mass percentage of silicon based on the mass of the negative electrode active material layer containing silicon. The test method is to take the negative electrode sheet in the finished battery cell, use SEM / EDS to identify the active material layer containing silicon, take the material of the active material layer to test ICP, and obtain the mass percentage of silicon.

[0133] 2. Diaphragm polymer particle layer thickness test

[0134] In the cell plane area, determine the position of the separator between the silicon-containing negative electrode active material layer and the positive electrode plate, ion cutting to obtain a 6×6 mm sample, and then use SEM / EDS scanning to obtain a side view of the separator, such as Figure 7 As shown in the figure, by combining SEM and EDS, the membrane substrate PP / PE, inorganic coating and polymer particle layer can be distinguished. The thickness of the polymer particle layer was measured, and 10 sets of data were taken in the flat area and the protrusion, and the average thickness was calculated as the thickness of the polymer particle layer (the flat area here is roughly flat relative to the protrusion).

[0135] 3.25℃ cycle 1000 cycles corner lithium deposition area ratio test

[0136] CCD imaging technology is used to obtain images of the electrode surface. By processing and detecting the images, the corner lithium deposition area can be identified, and the proportion of the corner lithium deposition area to the total area can be calculated.

[0137] Test Results

[0138] Table 1

[0139]

[0140]

[0141] By comparing the data of Examples 1-21 and Comparative Examples 1-6 in Table 1, it can be seen that in the negative electrode plate of the present application, the silicon element is concentrated in the active material layer on the surface of one side of the negative electrode current collector. The present application provides a separator coated with polymer particle layers of different thicknesses according to different matching of the silicon content in the negative electrode active material layer coated on the surface of one side of the negative electrode current collector in the negative electrode plate. When the matching relationship between the mass percentage content X of the silicon element and the thickness H of the polymer particle layer meets the conditions defined in the present application, the electrochemical device can reserve corner space to buffer the extrusion and fracture of the electrode plate, overcome the problems of electrode plate fracture and cyclic lithium precipitation caused by silicon-based expansion, and maximize the energy density. By comparing the data of Examples 5-6, 7-8, 9-11, 12-13, and 14-15, it can be seen that the mass percentage X of the silicon element and the thickness H of the polymer particle layer further meet the conditions of 2%≤X<5% and 1.5μm≤H<2.5μm, 5%≤X<10% and 2.5μm≤H<2.8μm, 10%≤X<15% and 2.8μm≤H<3.5μm, 15%≤X≤20% and 3.5μm≤H<4μm as defined in this application, the problem of cyclic lithium deposition of the electrochemical device is further optimized and improved. It can be seen from the data shown in Examples 1-6 that when the thickness H of the polymer particle layer is lower than the conditions defined in this application, the problems caused by silicon-based expansion cannot be effectively overcome, especially the electrochemical device will have pole piece extrusion and fracture at the corners, accompanied by serious cyclic lithium deposition problems; when the thickness H of the polymer particle layer is higher than the conditions defined in this application, the energy density of the electrochemical device will be seriously reduced.

[0142] Table 2

[0143]

[0144]

[0145] By comparing the data of Examples 22-33 and Comparative Examples 7-12 in Table 2, it can be seen that in the negative electrode sheet of the present application, silicon is evenly distributed in the active material layer on both sides of the negative electrode current collector. The present application is a separator coated with polymer particle layers of different thicknesses according to the different matching of the silicon content in the negative electrode active material layer coated on the single side surface of the negative electrode current collector in the negative electrode sheet. When the matching relationship between the mass percentage content X of the silicon element and the thickness H of the polymer particle layer meets the conditions defined in the present application, the electrochemical device can reserve corner space to buffer the extrusion and fracture of the electrode sheet, overcome the problems of electrode sheet fracture and cyclic lithium precipitation caused by silicon-based expansion, and maximize the energy density at the same time. By comparing the data of Examples 22-23, 24-25, 26-27, 28-29, 30-31, and 32-33, it can be seen that when the mass percentage X of the silicon element and the thickness H of the polymer particle layer further meet one of the conditions specified in the present application of 2%≤X<5% and 1.5μm≤H<2.5μm, 5%≤X<10% and 2.5μm≤H<2.8μm, 10%≤X<15% and 2.8μm≤H<3.5μm, 15%≤X≤20% and 3.5μm≤H<4μm, the problem of cyclic lithium deposition in the electrochemical device is further optimized and improved. It can be seen from the data shown in Comparative Examples 7-12 that when the thickness H of the polymer particle layer is lower than the conditions specified in the present application, the problems caused by silicon-based expansion cannot be effectively overcome, especially the electrode extrusion and breakage will occur at the corners of the electrochemical device, accompanied by serious cyclic lithium deposition problems; when the thickness H of the polymer particle layer is higher than the conditions specified in the present application, the energy density of the electrochemical device will be seriously reduced.

[0146] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. An electrochemical device, comprising a positive electrode sheet, a negative electrode sheet and a separator; the negative electrode sheet comprises a negative electrode current collector, and a first negative electrode active material layer containing a silicon-based material is disposed on the surface of the negative electrode current collector; The separator is arranged between the negative electrode sheet and the positive electrode sheet; A polymer particle layer is provided on a surface of the separator adjacent to the first negative electrode active material layer; Based on the mass of the first negative electrode active material layer, the mass percentage of the silicon element is X; the thickness of the polymer particle layer is H, and the electrochemical device satisfies one of the following conditions: 0<X<2%, 0<H<1μm; 2%≤X<10%, 1μm≤H<2.8μm; 10%≤X<25%, 2.8μm≤H<4μm; 25%≤X≤30%, 4μm≤H≤5μm.

2. The electrochemical device according to claim 1, wherein: The electrochemical device satisfies one of the following conditions: 2%≤X<5%, 1.5μm≤H<2.5μm; 5%≤X<10%, 2.5μm≤H<2.8μm; 10%≤X<15%, 2.8μm≤H<3.5μm; 15%≤X≤20%, 3.5μm≤H<4μm.

3. The electrochemical device according to claim 1, wherein The separator adjacent to the first negative electrode active material layer is provided with a polymer particle layer on a surface thereof remote from the first negative electrode active material layer.

4. The electrochemical device according to claim 1, wherein The first negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-based active material and a carbon active material; The silicon-based material is selected from at least one of silicon, silicon-oxygen compounds, silicon-carbon compounds or silicon alloys; and / or The carbon active material is selected from at least one of graphite and hard carbon.

5. The electrochemical device according to claim 4, wherein: The silicon-based active material is silicon-carbon particles, and the carbon active material is graphite.

6. The electrochemical device according to claim 1, wherein Based on the mass of the first negative electrode active material layer, the mass percentage X of the silicon element satisfies 2%≤X≤5%.

7. The electrochemical device according to any one of claims 1 to 5, wherein: A second negative electrode active material layer is disposed on the other surface of the negative electrode current collector; The second negative electrode active material layer does not contain silicon; Alternatively, the second negative electrode active material layer contains silicon.

8. The electrochemical device according to claim 7, wherein: The second negative electrode active material layer does not contain silicon element, and no polymer particle layer exists on the surface of the separator adjacent to the second negative electrode active material layer.

9. The electrochemical device according to claim 1, wherein: The polymer particle layer is selected from at least one of homopolymers or copolymers of vinylidene fluoride, hexafluoropropylene, ethylene, propylene, vinyl chloride, allyl chloride, acrylic acid, acrylic ester, styrene, butadiene, and acrylonitrile.

10. The electrochemical device according to claim 1, wherein The separator adjacent to the first negative electrode active material layer comprises a substrate and an inorganic coating, wherein the inorganic coating is disposed between the substrate and the polymer particle layer; the inorganic coating is selected from at least one material of boehmite, magnesium hydroxide, aluminum oxide, titanium dioxide, silicon dioxide, zirconium dioxide, tin dioxide, magnesium oxide, zinc oxide, barium sulfate, boron nitride, aluminum nitride or silicon nitride; The substrate is at least one material selected from a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film.

11. The electrochemical device according to claim 1, wherein The separator adjacent to the first negative electrode active material layer is provided with an adhesive layer on a surface thereof facing the first negative electrode active material layer.

12. The electrochemical device according to claim 11, wherein The adhesive layer is a polymer formed by at least one of acrylic acid, acrylic acid ester, styrene, isobutyl acrylate or acrylonitrile.

13. An electronic device comprising the electrochemical device according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Electrochemical device and electronic device

    CN112768784A

  • Negative pole piece, electrochemical device comprising negative pole piece and electronic device

    CN114530576A

  • Polymer lithium ion battery

    CN202737038U

  • Secondary battery

    JP2010176901A

  • Electrochemical apparatus and electronic apparatus

    US20220190442A1

Cited By

  • Negative pole piece, electrochemical device and preparation method of negative pole piece

    CN120497280A

  • Battery, electric device, and box body

    WO2026123904A1