Negative electrode active material for secondary battery, method for producing same, negative electrode for secondary battery, and secondary battery
By using negative electrode materials combined with silicon composite and carbon nanotubes in lithium-ion batteries, the capacity deterioration of silicon negative electrode materials caused by volume expansion and poor contact of conductive additives in lithium-ion batteries is solved, and higher cycles are achieved Stability and conductivity.
Patent Information
- Application Number
- CN202380027019.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-16
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-08
AI Technical Summary
When silicon is used as the negative electrode material in lithium-ion batteries, repeated charging and discharge leads to capacity deterioration, and the active substance particles are broken due to volume expansion and poor contact with conductive additives, which affects battery performance.
Active material particles containing silicon composites and self-assembled single molecular films are used, and carbon nanotubes are used as binders to form a combination of multi-layer carbon nanotubes and single-layer carbon nanotubes to enhance the bonding between active material particles. Force and conductivity suppress volume changes caused by charge and discharge.
It effectively suppresses capacity degradation caused by repeated charging and discharging, improves the cycle stability and conductivity of the battery, and extends the service life of the battery.
Smart Images

Figure CN118922959A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode active material for a secondary battery and a method for producing the same, a negative electrode for a secondary battery and a secondary battery.
[0002] This application claims priority based on Japanese Patent Application No. 2022-041246 filed in Japan on March 16, 2022, and the contents are incorporated herein by reference. Background Art
[0003] In order to increase the energy density of lithium-ion batteries, alloy materials such as silicon have attracted much attention as new materials to replace graphite, which is a conventional negative electrode material (e.g., non-patent documents 1 to 3). Compared with graphite, the specific capacity of silicon is nearly 4 times greater. On the other hand, the volume expansion when absorbing lithium ions is also large. Therefore, it is known that when silicon is used as a negative electrode material for secondary batteries, the active material particles may be broken with the charge and discharge cycle of the secondary battery, or the capacity may be degraded due to poor contact with the conductive additive. In addition, it is known that due to the formation of a film during the initial charging reaction, the activation reaction accompanied by the breakage of the active material, and the generation of non-capacitance accompanied by the generation of Li4SiO4, the lithium ions in the positive electrode decrease and the capacity deteriorates.
[0004] Prior art literature
[0005] Non-patent literature
[0006] Non-patent document 1: T. Hirose et al., Solid State Ionics 303 (2017) 154-160 Non-patent document 2: T. Hirose et al., Solid State Ionics 304 (2017) 1-6 Non-patent document 3: T. Hirose et al., Solid State Communications 269 (2018) 39-44 Summary of the invention
[0007] Technical issues to be solved
[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a secondary battery in which capacity degradation due to repeated charge and discharge is suppressed, a secondary battery negative electrode active material constituting the secondary battery, a method for producing the same, and a secondary battery negative electrode.
[0009] Means of solving the problem
[0010] In order to solve the above-mentioned problems, the present invention adopts the following means.
[0011] (1) According to one embodiment of the present invention, a negative electrode active material for a secondary battery comprises: active material particles comprising a silicon composite and a self-assembled monolayer covering the surface of the silicon composite and containing an amino group; and a binder comprising a carbon compound bonded to the self-assembled monolayer via the amino group, the carbon compound comprising a first carbon nanotube having a length of less than 1000 nm and a second carbon nanotube having a length of more than 2 μm.
[0012] (2) In the negative electrode active material for a secondary battery described in (1) above, the binder is preferably contained in a ratio of 1 wt % to 15 wt %.
[0013] (3) In the binder of the secondary battery negative electrode active material described in (1) or (2), the second carbon nanotubes are preferably contained in a ratio of 1 wt % to 15 wt %.
[0014] (4) In the negative electrode active material for a secondary battery according to any one of (1) to (3), it is preferred that the first carbon nanotubes are multi-walled carbon nanotubes, and the second carbon nanotubes are single-walled carbon nanotubes.
[0015] (5) A negative electrode for a secondary battery according to one embodiment of the present invention is a negative electrode for a secondary battery using the negative electrode active material for a secondary battery described in any one of (1) to (4) above, and comprises a current collector and the negative electrode active material for a secondary battery formed on one side of the current collector.
[0016] (6) In the secondary battery negative electrode described in (5) above, a carbon film may be further provided between one surface of the current collector and the secondary battery negative electrode active material.
[0017] (7) According to one embodiment of the present invention, a secondary battery preferably comprises a negative electrode for a secondary battery, a positive electrode for a secondary battery, and an electrolyte filling between the negative electrode for a secondary battery and the positive electrode for a secondary battery as described in (5) or (6) above, wherein the proportion of fluoroethylene carbonate contained in the electrolyte is less than 15 wt %.
[0018] (8) A method for producing a negative electrode active material for a secondary battery according to one aspect of the present invention is a method for producing a negative electrode active material for a secondary battery as described in any one of (1) to (4) above, comprising the following steps: forming a carbon compound body bonded with 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride molecules; forming a silicon complex bonded with amines; and mixing the carbon compound body and the silicon complex in a liquid to form an amide bond.
[0019] Effects of the Invention
[0020] According to the present invention, it is possible to provide a secondary battery in which capacity degradation due to repeated charge and discharge is suppressed, a secondary battery negative electrode active material constituting the secondary battery, a method for producing the same, and a secondary battery negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is an enlarged cross-sectional view of a negative electrode for a secondary battery according to a first embodiment of the present invention.
[0022] Figure 2 is Figure 1 An enlarged view of the bonding portion between active material particles and a binder in a negative electrode active material for a secondary battery.
[0023] Figure 3 is Figure 1 A diagram illustrating a process for producing active material particles in a method for producing a negative electrode for a secondary battery.
[0024] Figure 4 is Figure 1 A diagram illustrating a process for producing a binder in a method for producing a negative electrode for a secondary battery.
[0025] Figure 5A This is a schematic diagram of a negative electrode for a secondary battery when active material particles expand.
[0026] Figure 5B This is a schematic diagram of a negative electrode for a secondary battery when active material particles shrink.
[0027] Figure 6 It is an enlarged cross-sectional view of a negative electrode for a secondary battery according to a second embodiment of the present invention.
[0028] Figure 7 This is a SEM image of the surface of the negative electrode active material for a secondary battery of Example 1.
[0029] Figure 8 This is a SEM image of a cross section of the negative electrode active material for a secondary battery of Example 1.
[0030] Fig. 9 This is a graph showing the results of cycle tests of the discharge capacity of secondary batteries using the secondary battery negative electrode active materials of Example 1 and Comparative Examples 1 and 2.
[0031] Fig.10 This is a graph showing the results of cycle tests of the average operating voltage of the secondary batteries using the secondary battery negative electrode active materials of Example 1 and Comparative Example 1.
[0032] Fig.11 This is a graph showing the results of cycle tests of the discharge capacity of secondary batteries using the secondary battery negative electrode active materials of Examples 1 and 2.
[0033] Fig.12 This is a SEM image of the surface of the negative electrode active material for a secondary battery obtained in Example 3.
[0034] Fig.13 This is a SEM image of the surface of the negative electrode active material for a secondary battery obtained in Example 4.
[0035] Fig.14 This is a graph showing the cycle test results of the secondary batteries using the secondary battery negative electrode active materials of Examples 2 to 4, showing the discharge capacity depending on the content of the binder.
[0036] Fig.15 This is a graph showing the cycle test results of the secondary batteries using the secondary battery negative electrode active materials of Examples 5 to 7, showing the discharge capacity depending on the content of the binder.
[0037] Fig.16 This is a SEM image of a cross section of the secondary battery negative electrode obtained in Example 6.
[0038] Fig.17 This is a SEM image of a cross section of the secondary battery negative electrode obtained in Example 7.
[0039] Fig.18 This is a graph showing the results of cycle tests of the secondary batteries using the secondary battery negative electrode active materials of Examples 2 and 5, and the discharge capacity depending on whether or not FEC is added.
[0040] Fig.19 This is a graph showing the cycle test results of the secondary batteries using the secondary battery negative electrode active materials of Examples 3 and 6, and the discharge capacity depending on whether FEC is added or not.
[0041] Fig. 20 This is a graph showing the results of cycle tests of the secondary batteries using the secondary battery negative electrode active materials of Examples 4 and 7, with the discharge capacity depending on whether or not FEC was added under the condition of a discharge time of 5 hours (0.2 C).
[0042] Fig.21 This is a graph showing the results of a cycle test of the discharge capacity of a secondary battery using the secondary battery negative electrode active material of Example 7 under the condition that the discharge time was 0.5 hours (2C).
[0043] Fig.22A This is a graph showing the charge and discharge curves of the secondary batteries of Examples 2 and 3 when charge and discharge were repeated 10 times.
[0044] Fig. 22BThis is a graph showing the charge and discharge curves of the secondary batteries of Examples 2 and 3 when charge and discharge were repeated 30 times.
[0045] Fig. 22C This is a graph showing the charge and discharge curves of the secondary batteries of Examples 2 and 3 when charge and discharge were repeated 50 times.
[0046] Fig.23A This is a graph showing the dQ / dV curve of the secondary battery of Example 2 when charge and discharge were repeated 10 times, 30 times, and 50 times.
[0047] Fig. 23B This is a graph showing the dQ / dV curve of the secondary battery of Example 3 when charge and discharge were repeated 10 times, 30 times, and 50 times.
[0048] Fig.24 This is a graph showing dQ / dV curves of the secondary batteries of Examples 2 to 5 in which charge and discharge were repeated 50 times.
[0049] Fig.25A This is a graph showing average operating characteristics of the secondary batteries of Examples 2 to 5.
[0050] Fig.25B It is a graph showing the coulombic efficiency of the secondary batteries of Examples 2 to 5.
[0051] Fig.26 These are images of the cross section of the negative electrode constituting the secondary battery of Example 3 when it is expanded (left side) and when it is contracted (right side).
[0052] Fig. 27 These are images of the cross section of the negative electrode constituting the secondary battery of Example 5 when it is expanded (left side) and when it is contracted (right side).
[0053] Fig.28A This is an image of the surface of the composite electrode layer of Example 2.
[0054] Fig.28B This is an image of the surface of the composite electrode layer of Example 3.
[0055] Fig.28C This is an image of the surface of the composite electrode layer of Example 4.
[0056] Fig.28D This is an image of the surface of the composite electrode layer of Example 5.
[0057] Fig.29A This is an image of a cross section of the composite electrode layer of Example 2.
[0058] Fig.29B This is an image of a cross section of the composite electrode layer of Example 3.
[0059] Fig.29C This is an image of a cross section of the composite electrode layer of Example 4.
[0060] Fig.29D This is an image of a cross section of the composite electrode layer of Example 5.
[0061] Fig. 30A This is a graph showing the variation in the measurement results of the volume resistivity of the mixed electrode layers of Examples 2 to 5.
[0062] Fig. 30B This is a graph showing the variation in the measurement results of the interface resistance of the mixed electrode layers of Examples 2 to 5.
[0063] Fig. 30C This is a graph showing the variation in the measurement results of the surface resistance of the mixed electrode layers of Examples 2 to 5.
[0064] Fig.31 This is a graph showing the charge and discharge curves of the secondary battery of Example 9.
[0065] Description of Reference Numerals
[0066] 100 Negative electrode for secondary battery
[0067] 101 Current Collector
[0068] 101a One side of the current collector
[0069] 102 compound electrode layer
[0070] 103 Silicon compound
[0071] 104 Self-assembled monolayers
[0072] 105 Adhesive
[0073] 105A Long Carbon Material
[0074] 105B First Carbon Nanotube
[0075] 105C Second Carbon Nanotube
[0076] 106 Active substance particles
[0077] 106A Precursor of active material particles
[0078] 106B amino
[0079] 107EDC molecule
[0080] 108 carbon film DETAILED DESCRIPTION
[0081] Hereinafter, the negative electrode active material for secondary batteries and the method for manufacturing the negative electrode for secondary batteries and the secondary battery to which the embodiments of the present invention are applied are described in detail using the accompanying drawings. It should be noted that, with respect to the accompanying drawings used in the following description, in order to facilitate the understanding of the features, the features are sometimes enlarged for convenience, and the size ratios of the components are not necessarily the same as the actual ones. In addition, the materials, dimensions, etc. illustrated in the following description are examples, and the present invention is not limited to these, and can be appropriately changed for implementation without changing its purpose.
[0082] <First Embodiment>
[0083] (Negative electrode active material for secondary battery, negative electrode for secondary battery)
[0084] Figure 1 This is a cross-sectional view schematically showing a part of the structure of a secondary battery negative electrode 100 having a composite electrode layer 102 containing a negative electrode active material for a secondary battery according to the first embodiment of the present invention. The secondary battery negative electrode 100 is deposited (coated) with a composite electrode layer 102 in a film-forming manner on one side 101a of a current collector 101 composed of a conductive member such as a copper foil. The composite electrode layer 102 has a plurality of negative electrode active materials for secondary batteries (hereinafter referred to as active material particles 106), and a binder (binder) 105 filled in the gaps between the active material particles 106. The gaps between the active material particles 106 can be filled with a conductive auxiliary agent or the like depending on the application.
[0085] The active material particles 106 include the silicon composite 103 and the self-assembled monomolecular film 104 having amino groups and covering the surface of the silicon composite 103. The binder 105 is bonded to the self-assembled monomolecular film 104 via the amino groups.
[0086] The silicon composite 103 is composed of a silicon compound and at least one carbon material selected from graphite, non-graphitizable carbon (hard carbon) or soft carbon. The silicon composite 103 may further include one or both of Sn and Li. The silicon compound includes Si, SiO, SiO x (x is a real number).
[0087] From the viewpoint of increasing specific capacity, the silicon compound preferably accounts for 5% or more of the volume of the silicon composite 103. The average diameter of the silicon compound (the diameter obtained by averaging the particle diameters of the silicon compound measured in two or more directions) is preferably 10 nm to 15,000 nm.
[0088] As the silicon compound, for example, composite particles can be used in which nano silicon particles with a particle size of about 100 nm are dispersed in hollow soft carbon with a particle size of about 10 μm. In this case, the volume ratio of nano silicon to soft carbon is preferably 50:50. In addition, as the silicon compound, for example, silicon oxide (SiO2) with a particle size of about 10000 nm can also be used. x ) particles, silicon oxide (SiO x ) and other particles.
[0089] The self-assembled monolayer 104 is a film composed of molecules such as carbon, with amino groups (-NH2) formed on the surface. The thickness of the self-assembled monolayer 104 is preferably greater than 1 nm and less than 10 nm. In this embodiment, the case of using N-[3-(trimethoxysilyl)propyl]diethylenetriamine (DEADAPTS) as the self-assembled monolayer 104 is described as an example.
[0090] The binder 105 contains a long carbon material (structure) 105A containing carbon atoms as a main component. The long carbon material 105A contains two types of carbon nanotubes of different sizes and shapes in a state of being mixed with each other. Hereinafter, one of the two types of carbon nanotubes is referred to as a first carbon nanotube, and the other is referred to as a second carbon nanotube. The binder 105 may further contain a conductive material such as graphene, reduced graphene oxide, acetylene black, amorphous carbon, a conductive polymer, or a binder such as polyimide or carboxymethyl cellulose.
[0091] The proportion of the binder 105 contained in the composite electrode layer 102 can be freely selected according to the application, but is preferably set to 2 wt% or more from the viewpoint of improving the binding force and conductivity between the active material particles 106, and is preferably set to 6 wt% or less from the viewpoint of ensuring sufficient capacity characteristics. That is, for the same reason, the proportion of the active material particles 106 in the composite electrode layer 102 is preferably set to 94 wt% or more and 98 wt% or less.
[0092] The first carbon nanotube is mainly distributed in the form of a self-assembled monolayer 104 adhered to the surface of the active material particles, and functions as a low-elastic adhesive that can deform to follow the shape of the surface. Since the first carbon nanotube constitutes the skeleton of the adhesive and plays a role in maintaining its strength, it has a shape that is thicker and shorter than the second carbon nanotube. Therefore, the length of the length direction of the first carbon nanotube is less than 1000nm, preferably more than 300nm and less than 700nm. In addition, the diameter of the cross section perpendicular to the length direction of the first carbon nanotube is preferably more than 10nm and less than 40nm, more preferably more than 20nm and less than 30nm. As such a first carbon nanotube, for example, a multilayer carbon nanotube can be cited.
[0093] The second carbon nanotube functions as a low elastic binder in the same manner as the first carbon nanotube, but has a higher conductivity than the first carbon nanotube, has a slender and easily condensed shape, and more firmly binds the active material particles to each other. The second carbon nanotube is complexly entangled in the first carbon nanotube, binds the active material particles more firmly, and spreads over the entire surface of the active material particles, acting as a conductive path. Therefore, the second carbon nanotube has a shape that is slender and easily condensed than the first carbon nanotube, and has high conductivity. Therefore, the length of the second carbon nanotube in the longitudinal direction is more than 2μm, preferably more than 5μm and less than 10μm. The diameter of the cross section perpendicular to the length direction of the second carbon nanotube is preferably more than 1nm and less than 5nm, more preferably more than 2nm and less than 3nm. As such a second carbon nanotube, for example, a single-layer carbon nanotube can be cited.
[0094] In the long carbon material 105A, the second carbon nanotube is preferably contained in a ratio of 10wt% or more. When the ratio of the second carbon nanotube is less than 10wt%, the function of bonding the active material particles is weakened. In addition, when the ratio of the second carbon nanotube is too large, the ratio of the first carbon nanotube becomes small, and it is difficult to maintain the shape of the active material.
[0095] Figure 2 Yes Figure 1 FIG. 1 is an enlarged view of the bonding portion of the active material particles 106 and the binder 105. Figure 2 As shown, the composite electrode layer 102 has a portion where the self-assembled monolayer 104 of the organosilane compound and the long carbon material (carbon nanotube) 105A form a non-covalent bond. More specifically, in this portion, the positively charged functional group (-NH 3+ ) forms a non-covalent bond with the carboxyl group formed on the long carbon material 105A by an attractive force accompanied by electrostatic interaction.
[0096] The composite electrode layer 102 may also include an additional binder other than the above-mentioned binder 105 as a binder for further improving the bonding between the active material particles 106. Examples of the additional binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-propylene-diene copolymer (EPDM), styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), polyimide (PI), carboxymethyl cellulose (CMC), fluororubber, and the like.
[0097] The composite electrode layer 102 may include, for example, ketjen black, acetylene black, carbon black, graphite, carbon nanotubes, carbon fibers, graphene, amorphous carbon, conductive polymer polyaniline, polypyrrole, polythiophene, polyacetylene, polyacene, etc. as conductive additives.
[0098] The secondary battery according to this embodiment is composed of a secondary battery negative electrode 100 using the above-mentioned composite electrode layer 102, a secondary battery positive electrode made of a known material, and an electrolyte filling between the two electrodes. The electrolyte may also contain FEC (fluoroethylene carbonate) to reduce the elasticity of the active material particles 106 of the secondary battery negative electrode 100. However, since FEC is an expensive material and generates unnecessary gas, the content ratio of FEC in the electrolyte is preferably suppressed to less than 15wt%.
[0099] Furthermore, as described later as an example, the negative electrode active material for a secondary battery of the present embodiment contains the second carbon nanotubes as a binder, and thus even if the content ratio of FEC is suppressed to 0.1 wt % or less, it is possible to reduce the elasticity of the active material particles.
[0100] (Method for producing negative electrode active material for secondary battery)
[0101] The negative electrode active material for secondary battery according to this embodiment is obtained by separately preparing active material particles 106 and binder 105 and mixing them. Active material particles 106 are composed of silicon composite 103 and self-assembled monomolecular film 104 covering the surface thereof. Binder 105 is formed by combining EDC (1-ethyl-3-(3-dimethylaminopropyl) carbodiimide hydrochloride) molecules 107 with long carbon materials (carbon nanotubes) 105A. Figure 3 , 4 The procedure for producing the active material particles 106 and the binder 105 will be described.
[0102] Figure 3 Schematically illustrates the steps of producing the active material particles 106. The active material particles 106 can be synthesized, for example, by a dry method. The synthesis of the active material particles 106 by the dry method can be performed by the following procedure.
[0103] First, an amount corresponding to the intended use, for example, about 2 to 10 g, is weighed and an ultraviolet irradiation unit such as a tabletop optical surface treatment device (LP16-110, SEN Special Light Source Co., Ltd.) is used to irradiate the carbon-coated silicon oxide powder (SiO x @C: Osaka Titanium Technology Co., Ltd., etc.) irradiated with ultraviolet light. As the carbon-coated silicon oxide powder, it is preferred to use a powder with an average particle size of 0.1 to 10 μm, and if it is a mass-produced product, it is about 1 to 10 μm. The ultraviolet irradiation time is preferably set to 3 to 10 minutes, for example, about five minutes. The carbon-coated silicon oxide powder may also contain Li.
[0104] Through this treatment, hydroxyl groups (—OH) are formed on the carbon coating and the exposed silicon oxide surface, and the precursor 106A of active material particles is produced in the petri dish.
[0105] Next, N-[3-(trimethoxysilyl)propyl]diethylenetriamine (DAEAPTS: C 10 H 27 N3O3Si, SIGMA-ALDRICH) is stored in a screw-cap bottle. The storage volume is preferably set to 25 to 100 μL, for example, about 50 μL.
[0106] [Chemical formula 1]
[0107]
[0108] Next, the above-mentioned culture dish and screw bottle are placed in a sealed SUS container, and maintained at a predetermined temperature and time using a thermostatic bath (DRA430DA, Advantech) or the like. The holding temperature is preferably set to 80 to 150° C., for example, to about 120° C. The holding time is preferably set to 10 to 20 hours, for example, to about 15 hours.
[0109] This treatment generates a precursor 106A having hydroxyl groups formed on the surface of the active material, and produces active material particles 106 having amino groups (—NH 2 ) 106B formed on the hydroxyl groups on the surface via silicon in the petri dish.
[0110] Figure 4 1 is a diagram schematically illustrating the steps of producing the binder 105. First, a mixed solution of water and long carbon material (carbon nanotube) 105A is produced in a predetermined container, and carboxyl groups (-COOH) are formed on the surface of the long carbon material 105A in the mixed solution.
[0111] Next, a solution of EDC molecules 107 is added to the container, and in the mixed solution, the carbon nanotubes 105A and the EDC molecules 107 are bonded via carboxyl groups, thereby producing a binder 105 composed of an active ester compound.
[0112] Next, the prepared active material particles 106 and the binder 105 are mixed in a predetermined container. Figure 2 As shown, the amino groups in the active material particles 106 and the EDC molecules in the binder 105 form amide bonds, and the composite electrode layer 102 can be produced in the mixed solution. In the produced composite electrode layer 102, a plurality of granular silicon composites 103 containing nano-silicon are stacked (deposited) on one side 101a of the collector via a self-assembled monomolecular film 104 covering the surface, in a state of forming non-covalent bonds with the carbon nanotubes 105A by the attraction accompanied by electrostatic interaction. In step 1, when a carbon-coated silicon oxide powder containing lithium is used, the lithium is contained in the silicon composite 103 in the state of Li4SiO.
[0113] (Method for producing negative electrode for secondary battery)
[0114] The mixed solution of the composite electrode layer 102 obtained in the above-mentioned order is dropped onto the current collector, and after being pressed by a pressing member, it is vacuum dried to remove unnecessary liquid in the mixed solution. Figure 1 A negative electrode 100 for a secondary battery is shown.
[0115] Figure 5A , Figure 5B Schematic diagrams showing the structures of the first carbon nanotube 105B and the second carbon nanotube 105C when the active material particles 106 are expanded and contracted, respectively.
[0116] The plurality of first carbon nanotubes 105B form covalent bonds with the amino groups on the surface of the active material particles 106. The second carbon nanotubes 105C bundle the plurality of first carbon nanotubes 105B and bond to each of the first carbon nanotubes 105B at the plurality of locations. Since the bonding is weak, the first carbon nanotubes 105B are reassembled according to the external force applied to the first carbon nanotubes 105B, resulting in sliding of the bonding locations.
[0117] When the active material particles 106 expand, Figure 5A As shown, the plurality of first carbon nanotubes 105B approach each other. Accordingly, the bonding sites of the plurality of first carbon nanotubes 105B and the second carbon nanotubes 105C slide and approach each other.
[0118] When the active material particles 106 shrink, as Figure 5B As shown, the plurality of first carbon nanotubes 105B move away from each other. Accordingly, the bonding sites between the plurality of first carbon nanotubes 105B and the second carbon nanotubes 105C slide and move away from each other.
[0119] By sliding the bonded portion in this way, the load acting on the bonded portion can be eliminated when the active material particles 106 expand or contract, thereby avoiding the problem of disconnection of the bond and obstruction of conduction between the active material particles 106. In addition, since the second carbon nanotubes 105C have excellent elasticity, even if an external force exceeding the sliding limit of the bonded portion is applied, the second carbon nanotubes 105C will stretch and contract to alleviate the external force, thereby helping to maintain the bond.
[0120] As described above, the negative electrode active material for the secondary battery of the present embodiment includes a second elongated carbon nanotube having a length of more than 2 μm as a low elastic binder for bonding the active material particles 106. The second carbon nanotube has high cohesion, entangles the first carbon nanotube, and adheres to the surface of the active material particle 106 and is distributed. Therefore, the second carbon nanotube can deform as the volume of the active material particle 106 changes, and the active material particles 106 are entangled with each other and firmly bonded. Therefore, the problem of reduced conductivity caused by adhesive peeling due to the volume change of the active material particles during charging and discharging can be avoided. Moreover, the second carbon nanotube has high electronic conductivity and functions as a solid conductive path that continuously follows the volume change, so that charging and discharging in a state of low resistance in the negative electrode can be achieved, and the capacity can be maintained at a high state.
[0121] When using silicon oxide as an active material, part of the lithium forms a compound with silicon oxide and is consumed during the reaction process during charging, so part of the power after charging is lost. However, when lithium is pre-incorporated into the silicon compound, the lithium can make up for the part consumed during charging, and the reduction in the total amount of lithium that contributes to conduction can be suppressed, so that the power for discharge can be maintained.
[0122] The composite electrode layer 102 having the above structure contains a conductive material containing two carbon nanotubes of different lengths at a very high ratio without containing an insulating binder such as PVDF or SBR, so that the resistance becomes low. In addition, since the weight ratio of the active material particles 106 in the composite electrode layer 102 is high, a lithium-ion secondary battery with a high capacity per unit weight, that is, a lithium-ion secondary battery with a high energy density can be obtained by having the composite electrode layer 102. Moreover, since the composite electrode layer 102 has high adhesion to the collector 101, a lithium-ion secondary battery that can withstand even a large current, that is, a lithium-ion secondary battery with a high output density can be obtained by having the composite electrode layer 102.
[0123] In the conductive binder 105, the first carbon nanotubes 105B are mainly connected to the adjacent active material particles 106. Thus, an electron conduction path is formed between the adjacent active material particles 106, and a three-dimensional mesh network structure is formed on the current collector 101. Due to the action of the first carbon nanotubes 105B, the active material particles 106 are not dropped from the composite electrode layer 102 and are retained on the current collector 101.
[0124] One of the reasons for the deterioration of lithium-ion secondary batteries during long-term use is that the active material particles 106 physically deviate from the conductive path in the electrode. When the composite electrode layer 102 is peeled off from the current collector 101, a large amount of active material particles 106 are separated from the conductive path, which is fatal. Therefore, the composite electrode layer 102 usually contains a binder for binding the active material particles 106.
[0125] On the other hand, in the present invention, the first carbon nanotubes 105B play the role of forming the above-mentioned mesh network structure, which can inhibit the active material particles 106 from detaching from the conductive path in the electrode. Therefore, it is possible to exhibit high adhesion between the active material particles 106 or sufficient adhesion of the active material particles 106 to the collector 101 without including a binder in the composite electrode layer 102.
[0126] The second carbon nanotubes 105C in the conductive binder 105 connect not only the adjacent active material particles 106 but also other active material particles 106 located around them, thus forming low-resistance and continuous electron conduction paths between more active material particles 106, compared with the case where the carbon nanotubes contained in the conductive binder 105 are only the first carbon nanotubes 105B. The electrical conductivity is greatly improved by the action of the second carbon nanotubes 105C.
[0127] In this way, the first carbon nanotubes 105B play a role in forming a mesh network structure, and the active material particles 106 are mechanically connected to each other, and the active material particles 106 can exhibit sufficient adhesion to the collector 101. In addition, the second carbon nanotubes 105C play a role in forming a low-resistance and continuous electron conduction path, and compared with the case where only the first carbon nanotubes 105B are formed, the active material particles 106 are electrically connected, and the electrical conductivity in the composite electrode layer 102 is greatly improved. In addition, by making the first carbon nanotubes 105B bear the bonding between the active material particles 106, it is not necessary to include a binder in the composite electrode layer 102, so the active material particles 106 can be included at a very high ratio relative to the composite electrode layer 102.
[0128] In addition, highly crystalline carbon materials are described as materials composed of graphene sheets composed only of carbon, but the ends or defects of the graphene sheets are usually terminated with hydrogen but are highly active and easily replaced by functional groups due to the surrounding environment. For example, in the case of carbon nanotubes formed into a cylindrical shape by dispersing graphene sheets in water, if the carbon nanotubes are cut, the ends are modified by hydroxyl groups from water due to the activity of the cut surface. Therefore, the more necked carbon nanotubes are, the more active surfaces are generated in water, so hydrophilic groups are easily adsorbed.
[0129] In this way, the hydrophilic groups on the fibrous carbon nanotubes form hydrogen bonds with the hydrophilic groups on other carbon nanotubes or the hydrophilic groups on the surface of the collector 101, thereby forming a network in which multiple carbon nanotubes are fixed to the collector 101, which can prevent the active material particles 106 from falling off from the composite electrode layer 102.
[0130] <Second Embodiment>
[0131] Figure 6 This is a cross-sectional view schematically showing a part of the structure of a secondary battery negative electrode 200 having a secondary battery negative electrode active material according to a second embodiment of the present invention. The secondary battery negative electrode 200 also has a carbon film 108 between one side 101a of the collector and the composite electrode layer 102. The thickness of the carbon film 108 is preferably greater than 0.5 μm and less than 2 μm. The other structures are the same as those of the secondary battery negative electrode 100 of the first embodiment, and at least have the same effect as the secondary battery negative electrode 100. In addition, the parts corresponding to the secondary battery negative electrode 100 are represented by the same figure marks.
[0132] In the secondary battery negative electrode 200 of the present embodiment, the carbon film 108 is provided between the composite electrode layer 102 and the current collector 101, so that the long carbon material 105A (particularly the second carbon nanotube) in the composite electrode layer 102 is firmly bonded to the current collector 101 via the carbon film 108. Therefore, it is possible to suppress the composite electrode layer 102 from peeling off from the current collector 101 due to the volume change caused by charging and discharging.
[0133] [Example]
[0134] The effects of the present invention will be more apparent through the following examples. The present invention is not limited to the following examples, and can be implemented by making appropriate changes within the scope of the gist thereof.
[0135] (Example 1)
[0136] The secondary battery according to the above embodiment is manufactured in the following order (steps 1 to 6).
[0137] [Process 1]
[0138] First, a tabletop optical surface treatment device (LP16-110, SEN Special Light Source Co., Ltd.) was used to weigh about 5 g of carbon-coated silicon oxide powder (SiO x @C: Osaka Titanium Technology Co., Ltd., etc.) was irradiated with ultraviolet rays. As carbon-coated silicon oxide powder, a material with an average particle size of 5 μm was used. The ultraviolet irradiation time was set to 5 minutes.
[0139] Next, 50 μL of N-[3-(trimethoxysilyl)propyl]diethylenetriamine (DAEAPTS: C 10 H 27 N3O3Si, SIGMA-ALDRICH) was stored in a screw-cap bottle.
[0140] Next, the above-mentioned Petri dish and screw bottle were placed in a SUS sealed container and maintained at 120° C. for 15 hours using a thermostatic bath (DRA430DA, Advantech), thereby producing active material particles in the Petri dish.
[0141] [Process 2]
[0142] In addition, the carbon nanotubes were mixed with water (H2O) contained in another container at room temperature to reach 2 wt % to prepare a mixed solution containing a binder having carboxyl groups (-COOH) formed on the surface. As carbon nanotubes, the first carbon nanotubes and the second carbon nanotubes were contained at a weight ratio of 9:1.
[0143] As the first carbon nanotube, a multilayer carbon nanotube (MWCNT) with a length of about 200 to 700 nm, a diameter of about 20 to 30 nm, and about 10 to 15 layers is used. As the second carbon nanotube, a single-walled carbon nanotube (SWCNT) with a length of about 5 to 10 μm and a diameter of about 2 to 3 nm is used.
[0144] [Process 3]
[0145] Next, the active material particles prepared in step 1 and the mixed solution prepared in step 2 were mixed at room temperature to prepare a mixed solution of active material particles, a binder and water. The weight ratio of the active material particles to the binder in the mixed solution was adjusted to 98:2.
[0146] [Process 4]
[0147] Next, the mixed solution prepared in step 3 was dropped onto a current collector (copper foil) made of copper, and doctor blade coating was performed using a pressing member.
[0148] [Process 5]
[0149] Next, water contained in the applied mixed solution was removed by vacuum drying at 80° C., thereby obtaining a secondary battery negative electrode having a secondary battery negative electrode active material formed on a current collector.
[0150] [Step 6]
[0151] A secondary battery (coin cell) was manufactured, which was composed of the obtained negative electrode for secondary battery, a counter electrode containing lithium metal, and an electrolyte (LiPF6) filled between the two electrodes. Here, FEC (fluoroethylene carbonate) was not included in the additive of the electrolyte.
[0152] (Example 2)
[0153] In step 4, a secondary battery was manufactured in the same manner as in the first example, except that the current collector on which the mixed solution was dropped was replaced with a current collector having a carbon film (thickness 1 μm) formed on the surface of the copper foil.
[0154] (Example 3)
[0155] A secondary battery was manufactured in the same manner as in Example 2 except that the weight ratio of the active material particles to the binder in the mixed solution prepared in step 3 was adjusted to 97:3.
[0156] (Example 4)
[0157] A secondary battery was manufactured in the same manner as in Example 2 except that the weight ratio of the active material particles to the binder in the mixed solution prepared in step 3 was adjusted to 95:5.
[0158] (Example 5)
[0159] A secondary battery was manufactured in the same manner as in Example 2 except that the weight ratio of the active material particles to the binder in the mixed solution was adjusted to 90:10 with respect to the mixed solution prepared in step 3.
[0160] (Example 6)
[0161] A secondary battery was produced in the same manner as in Example 2, except that 5 wt % of FEC was included in the additive of the electrolytic solution in step 6.
[0162] (Example 7)
[0163] A secondary battery was produced in the same manner as in Example 4, except that 5 wt % of FEC was included in the additive of the electrolytic solution in step 6.
[0164] (Example 8)
[0165] A secondary battery was produced in the same manner as in Example 5, except that 5 wt % of FEC was included in the additive of the electrolytic solution in step 6.
[0166] (Example 9)
[0167] A secondary battery was produced in the same manner as in Example 1, except that Li-containing carbon-coated silicon oxide powder was used in step 1.
[0168] (Comparative Example 1)
[0169] As the carbon nanotubes mixed with water in step 2, only the first carbon nanotubes (MWCNT) were used, and the second carbon nanotubes (SWCNT) were not used. In addition, the weight ratio of the active material particles and the MWCNT in the mixed solution was adjusted to 90:10 with respect to the mixed solution prepared in step 3. Except for this, a secondary battery was manufactured in the same manner as in Example 1.
[0170] (Comparative Example 2)
[0171] As the carbon nanotubes mixed with water in step 2, the first carbon nanotubes (MWCNT), styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) were used, and the second carbon nanotubes (SWCNT) were not used. In addition, the weight ratio of active material particles, MWCNT, and SBR / CMC in the mixed solution was adjusted to 90:4:3:3 with respect to the mixed solution prepared in step 3. In addition, a secondary battery was manufactured in the same manner as in Example 1.
[0172] Figure 7 , 8 These are SEM images of the surface and cross section of the negative electrode active material for a secondary battery obtained in Example 1. Figure 7 It can be seen that the long carbon material 105A including a plurality of first carbon nanotubes and second carbon nanotubes is distributed on the surface of the active material particle 106 in a state of being intricately entangled with each other. Figure 8 It can be seen that the plurality of second carbon nanotubes 105C are aggregated to connect adjacent active material particles 106 to each other.
[0173] A discharge capacity cycle test was performed on the secondary batteries (coin batteries) obtained in Example 1 and Comparative Examples 1 and 2. The discharge time was set to 5 hours (0.2 C). Fig. 9 The graph shows the test results. The horizontal axis of the graph shows the number of cycles (the number of times charge and discharge are repeated). The vertical axis (left and right) of the graph shows the discharge capacity (mAh / g) and the coulomb efficiency (%).
[0174] The discharge capacity of Comparative Examples 1 and 2 deteriorated rapidly with repeated charge and discharge, and became about 30% of the initial capacity after 20 cycles. In contrast, the discharge capacity of Example 1 hardly deteriorated after 20 cycles, and remained at more than 35% of the initial capacity even after 50 cycles.
[0175] The secondary batteries obtained in Example 1 and Comparative Example 1 were subjected to a cycle test of average operating voltage. Fig.10 The horizontal axis of the graph represents the number of cycles, and the vertical axis of the graph represents the average operating voltage (V).
[0176] The average operating voltage of Comparative Example 1 deteriorated rapidly with repeated charge and discharge, and became about 10% of the initial value after 50 cycles. In contrast, the average operating voltage of Example 1 deteriorated slowly, and was able to maintain about 50% of the initial value even after 50 cycles.
[0177] from Fig. 9 , 10 The test results show that in Example 1, the adhesive covering the active material particles contains elongated single-layer carbon nanotubes, and compared with Comparative Examples 1 and 2, the peeling of the adhesive and conductive additive accompanying the volume expansion of the active material particles and the breakage of the active material particles are reduced.
[0178] The secondary batteries obtained in Examples 1 and 2 were subjected to cycle tests of discharge capacity and coulombic efficiency. Fig.11 This is a graph showing the test results when the discharge time is set to 5 hours (0.2C). The horizontal axis of the graph represents the number of cycles. The vertical axis (left and right) of the graph represents the discharge capacity (mAh / g) and the coulomb efficiency (%).
[0179] from Fig.11 The test results show that in any of Examples 1 and 2, the changes in discharge capacity and coulomb efficiency are small, and high capacity can be maintained even with repeated charge and discharge. From these results, it can be seen that the peeling of the binder and conductive additive accompanying the volume expansion of the active material particles, the crushing of the active material particles, etc. are suppressed by the single-layer carbon nanotubes, and have nothing to do with the structure of the collector. It can be seen that the initial discharge capacity of Examples 1 and 2 is different, but the degree of degradation is the same.
[0180] Fig.12 , 13 These are SEM images of cross sections of the negative electrode active materials for secondary batteries obtained in Examples 4 and 5, respectively. Figure 8 When compared with the active material particles 106 of Example 1, it can be seen that more second carbon nanotubes 105C are aggregated between the active material particles 106 of Example 4, and more second carbon nanotubes 105C are aggregated between the active material particles 106 of Example 5. Therefore, it can be considered that the higher the content ratio of the binder 105 and the higher the content ratio of the second carbon nanotubes 105C, the stronger the connection between adjacent active material particles 106.
[0181] Cycle tests of discharge capacity and coulombic efficiency were performed on the secondary batteries obtained in Examples 2, 4, and 5. The discharge time was set to 5 hours (0.2 C). Fig.14The graph shows the test results. The horizontal axis of the graph shows the number of cycles. The vertical axis (left and right) of the graph shows the discharge capacity (mAh / g) and the coulombic efficiency (%).
[0182] In any of Examples 2, 4, and 5, the capacity degradation accompanying repeated charge and discharge can be suppressed. Compared with the capacitance value of Example 2, it can be seen that the capacitance value of Example 4 is maintained at a higher value, and the capacitance value of Example 5 is maintained at an even higher value. It can be considered that the higher the content ratio of the binder 105, and further the higher the content ratio of the second carbon nanotube 105C, the stronger the connection between adjacent active material particles 106.
[0183] Cycle tests of discharge capacity and coulombic efficiency were performed on the secondary batteries obtained in Examples 6 to 8. The discharge time was set to 5 hours (0.2 C). Fig.15 The graph shows the test results. The horizontal axis of the graph shows the number of cycles. The vertical axis (left and right) of the graph shows the discharge capacity (mAh / g) and the coulombic efficiency (%).
[0184] In any of Examples 6 to 8, the capacity degradation accompanying repeated charge and discharge can be suppressed. Compared with the capacitance value of Example 6, it can be seen that the capacitance value of Example 7 is maintained at a higher value, and the capacitance value of Example 8 is maintained at an even higher value. It can be considered that the higher the content ratio of the binder 105, and further the higher the content ratio of the second carbon nanotube 105C, the stronger the connection between adjacent active material particles 106.
[0185] Fig.16 , 17 This is an SEM image of a cross section of the negative electrode for secondary batteries of Examples 7 and 8 after the cycle test. Even after the cycle test, a large number of second carbon nanotubes 105C are condensed between the carbon film 108 and the active material particles 106, firmly bonding the carbon film 108 and the active material particles 106. In the second carbon nanotubes 105C that contribute to the bonding, one end is bonded to the amino group in the active material particles 106 through a condensation reaction with EDC. On the other hand, the other end penetrates into the carbon film 108 and is firmly bonded by intermolecular forces. Since the composite electrode layer 102 is firmly bonded to the collector 101 via the carbon film 108, it is possible to avoid the problem of peeling off from the collector 101 due to the volume expansion of the active material particles during charging and discharging.
[0186] Cycle tests of discharge capacity and coulombic efficiency were conducted on the secondary batteries of Examples 2 and 6. The discharge time was set to 5 hours (0.2C). Fig.18 The graph shows the test results. The horizontal axis of the graph shows the number of cycles. The vertical axis (left and right) of the graph shows the discharge capacity (mAh / g) and the coulombic efficiency (%).
[0187] Cycle tests of discharge capacity and coulombic efficiency were conducted on the secondary batteries of Examples 4 and 7. The discharge time was set to 5 hours (0.2C). Fig.19 The graph shows the test results. The horizontal axis of the graph shows the number of cycles. The vertical axis (left and right) of the graph shows the discharge capacity (mAh / g) and the coulombic efficiency (%).
[0188] Cycle tests of discharge capacity and coulombic efficiency were conducted on the secondary batteries of Examples 5 and 8. The discharge time was set to 5 hours (0.2C). Fig. 20 The graph shows the test results. The horizontal axis of the graph shows the number of cycles. The vertical axis (left and right) of the graph shows the discharge capacity (mAh / g) and the coulombic efficiency (%).
[0189] Compared with the capacity characteristics of the secondary battery of Example 6, the capacity characteristics of the secondary battery of Example 2 are lower. In contrast, the secondary batteries of Examples 4 and 7 show the same capacity characteristics, and the secondary batteries of Examples 5 and 8 show the same capacity characteristics. From these results, it can be seen that if the secondary battery contains a large amount of binder (carbon nanotubes), even if the electrolyte does not contain FEC, the effect of reducing the elasticity of the active material particles can be obtained, and the peeling of the binder and the like accompanying the volume expansion of the active material particles, the crushing of the active material particles, etc. can be fully suppressed.
[0190] The secondary battery of Example 8 was subjected to a cycle test of discharge capacity and coulombic efficiency by setting the discharge time to 0.5 hours (2C). Fig.21 The graph shows the test results. The horizontal axis of the graph shows the number of cycles. The vertical axis (left and right) of the graph shows the discharge capacity (mAh / g) and the coulombic efficiency (%).
[0191] from Fig. 20 , 21 It can be seen from the comparison that the change of discharge capacity and coulomb efficiency caused by the increase or decrease of discharge rate is small, and high capacity can be maintained even if charge and discharge are repeated at any discharge rate. It can be considered that no matter at which discharge rate, the peeling of the binder and the crushing of the active material particles can be fully suppressed due to the volume expansion of the active material particles.
[0192] Three samples of the secondary batteries of Examples 2 and 3 were prepared, and the charge-discharge cycle tests were repeated 10, 30, and 50 times, respectively. Each sample after the cycle test was placed on a constant current potentiostat, and Li was inserted and removed from the negative electrode in the range of 0V to 1.2V. Fig.22A , 22B22C are graphs showing the results of the samples of Examples 2 and 3 when the number of charge and discharge times (number of cycles) was set to 10, 30, and 50, respectively.
[0193] When the number of cycles is 10, the capacities of Examples 2 and 3 are almost the same, but when the number of cycles increases to 30, the capacity of Example 2 becomes lower than that of Example 3. When the number of cycles increases to 50, the capacity of Example 2 becomes further lower than that of Example 3, and the difference between them increases. From these results, it can be seen that the smaller the proportion of carbon nanotubes contained in the composite electrode layer, the lower the capacity, and the greater the reduction as the number of cycles increases.
[0194] dQ / dV was calculated for the sample of Example 2 in which the number of cycles was 10, 30, and 50, and for the sample of Example 3 in which the number of charge and discharge was 10, 30, and 50. Fig.23A , 23B It is a graph showing the respective calculation results.
[0195] The height of the peak of the dQ / dV curve is related to the connection state of the carbon nanotubes and the active material particles. In the sample of Example 2, as the number of cycles increases, the peak value becomes lower, so it can be considered that as the charge and discharge, the contact points between the carbon nanotubes and the active material particles decrease, and the utilization efficiency of the active material decreases. In contrast, in the sample of Example 3, since the decrease in the peak value caused by the number of cycles is small, it can be considered that even after the cycle test, the utilization efficiency of the active material can be roughly maintained. From these results, it can be seen that the greater the proportion of carbon nanotubes contained in the composite electrode layer, the less susceptible it is to the influence of the cycle test, and the easier it is to maintain the utilization efficiency as a negative electrode.
[0196] In Examples 2 and 3, the peak positions were aligned regardless of the number of cycles, and it was found that abnormal degradation such as decomposition of the electrolyte solution and rupture of the active material did not occur due to the cycle test.
[0197] For the samples of Examples 2 to 5 whose charge and discharge times were set to 50, dQ / dV was calculated. Fig.24 It is a graph showing the calculation results.
[0198] The peak values become higher in the order of Examples 2, 3, and 4. On the other hand, the peak values of Examples 4 and 5 are of the same height. From these results, it can be seen that within the range where the proportion of carbon nanotubes contained in the composite electrode layer is 5% or less, the greater the proportion, the more contact points between the carbon nanotubes and the active material particles. It can also be seen that when the proportion of carbon nanotubes contained in the composite electrode layer is 5%, the state where the carbon nanotubes and the active material particles have the most contact points is reached, and this state does not change even if the proportion is greater than 5%.
[0199] The samples of Examples 2, 3, 4, and 5 were subjected to a cycle test, and the changes in the average operating voltage and coulombic efficiency when charged as secondary batteries were measured according to the number of cycles. Fig.25A , 25B These are graphs showing the measurement results of the average operating voltage and the coulombic efficiency, respectively.
[0200] In the range where the proportion of carbon nanotubes contained in the composite electrode layer is less than 5%, the smaller the proportion and the more cycles, the more the average operating voltage and coulomb efficiency tend to decrease. In addition, in the range where the proportion is more than 5%, the decreasing trend of the average operating voltage and coulomb efficiency caused by the number of cycles is slowed down regardless of the proportion. From these results, it can be seen that carbon nanotubes also have the function of improving the conductivity of secondary batteries, and by increasing the proportion of carbon nanotubes, the conductivity can be further improved.
[0201] The cross sections of the negative electrodes of the samples of Examples 3 and 5 were observed during charge and discharge. Fig.26 , 27 The images (FE-SEM images) of the negative electrode cross sections of Examples 3 and 5 are respectively, the left side is the image during charge, and the right side is the image during discharge.
[0202] The thickness of the composite electrode layer of Example 3 was 28.9 μm during charge and 26.3 μm during discharge, and the thickness reduction rate during discharge relative to the thickness during charge was 9%. The thickness of the composite electrode layer of Example 5 was 32.9 μm during charge and 23.6 μm during discharge, and the thickness reduction rate during discharge relative to the thickness during charge was 28.3%. The change in thickness is due to the volume change of the active material particles in the expanded state and the compressed state.
[0203] In Examples 3 and 5, the thickness during discharge was smaller than that during charge, and thus it was possible to confirm the ability of the carbon nanotubes to follow the volume change of the active material particles.
[0204] In addition, the thickness during expansion and the thickness shrinkage rate during contraction in Example 5 are much greater than those in Example 3. It can be seen that the greater the proportion of carbon nanotubes contained in the composite electrode layer, the higher the followability of the carbon nanotubes.
[0205] Fig.28A , 28B28C and 28D are images (FE-SEM images) of the surface of the composite electrode layer in Examples 2 to 5, respectively. In the active material particles of Example 2, where the proportion of carbon nanotubes is 2%, parts not covered by carbon nanotubes can be seen, while in the active material particles of Example 5, where the proportion of carbon nanotubes is 10%, almost the entire surface is covered by carbon nanotubes. From the comparison of Examples 2 to 5, it can be seen that the greater the proportion of carbon nanotubes contained in the composite electrode layer, the higher the coverage of the active material particles by carbon nanotubes.
[0206] Fig.29A , 29B , 29C, and 29D are images (FE-SEM images) of the cross-section of the composite electrode layer in Examples 2 to 5, respectively. The area surrounded by the thick line indicates the area where the carbon nanotubes are distributed in bundles. The carbon nanotubes are distributed here in a manner that penetrates from the front to the inside. From the comparison of Examples 2 to 5, it can be seen that the greater the proportion of carbon nanotubes contained in the composite electrode layer, the greater the area and number density of the area where the carbon nanotubes are distributed.
[0207] The volume resistivity, interface resistance, and surface resistance were measured at 16 locations of the mixed electrode layers of Examples 2 to 5. Fig. 30A , 30B , 30C are graphs showing the deviations of the measurement results of volume resistivity, interface resistance, and surface resistance, respectively. According to the comparison of Examples 2 to 5 in each figure, the larger the proportion of carbon nanotubes contained in the composite electrode layer, the smaller the deviation of resistance tends to be. In order to form a uniform electron conduction network, it is preferred that the deviation is within 20% of the average value.
[0208] The sample of Example 9 was placed in a constant current potentiostat, and Li was inserted and removed from the negative electrode in the range of 0V to 2.5V. Fig.31 is a graph showing the results. Fig.31 It can be seen that the charge capacity and the discharge capacity are approximately equal. This is believed to be because, by pre-incorporating lithium into the silicon compound body, the lithium can make up for the reduction of lithium consumed during charging, thereby suppressing the reduction of the total amount of lithium that contributes to conduction and maintaining the amount of electricity for discharge.
Claims
1. A negative electrode active material for a secondary battery, characterized in that: have: Active material particles comprising a silicon composite and a self-assembled monomolecular film covering a surface of the silicon composite and containing an amino group; and A binder is bonded to the self-assembled monolayer via the amino group, The binder includes first carbon nanotubes having a length of 1000 nm or less and second carbon nanotubes having a length of 2 μm or more.
2. The negative electrode active material for secondary battery according to claim 1, characterized in that: The binder is included in a ratio of 1 wt % or more and 15 wt % or less.
3. The negative electrode active material for secondary battery according to claim 1 or 2, characterized in that: The second carbon nanotubes are contained in the binder at a ratio of 1 wt % to 15 wt % both inclusive.
4. The negative electrode active material for secondary battery according to claim 1 or 2, characterized in that: The first carbon nanotubes are multi-layer carbon nanotubes, and the second carbon nanotubes are single-layer carbon nanotubes.
5. A negative electrode for a secondary battery, which is a negative electrode for a secondary battery using the negative electrode active material for a secondary battery according to claim 1 or 2, characterized in that: have: a current collector; and The negative electrode active material for a secondary battery is formed on one surface side of the current collector.
6. The negative electrode for a secondary battery according to claim 5, characterized in that: A carbon film is further provided between one side of the current collector and the secondary battery negative electrode active material.
7. A secondary battery, characterized in that: have: The negative electrode for a secondary battery according to claim 5; A positive electrode for a secondary battery; and filling an electrolyte solution between the negative electrode for the secondary battery and the positive electrode for the secondary battery, The proportion of fluoroethylene carbonate contained in the electrolyte is 15 wt % or less.
8. A method for producing a negative electrode active material for a secondary battery, the method for producing a negative electrode active material for a secondary battery according to claim 1 or 2, characterized in that: It has the following processes: forming an adhesive bonded with 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride molecules; forming an amine-bound silicon complex; and The adhesive and the silicon composite are mixed in a liquid so that an amide bond is formed.