Composite heat stabilizer for PVC (polyvinyl chloride) and PVC profile

Through the combination of modified hydrotalcite and metal organic framework, the problem of poor thermal decomposition catalysis and initial coloring performance of calcium and zinc thermal stabilizers in PVC is solved, and the efficient thermal stability and initial coloring performance of PVC are improved.

CN118930970AInactive Publication Date: 2024-11-12ANHUI HUAWEN PLASTIC TECH CO LTD

Patent Information

Application Number
CN202410969776.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing calcium and zinc thermal stabilizers have problems with poor thermal decomposition catalysis and initial coloring performance during PVC processing, and the synergistic effect of auxiliary thermal stabilizers needs to be further improved.

Method used

Modified hydrotalcite is used as an auxiliary stabilizer and combined with a metal organic framework. By coating the combination of hydrotalcite and metal organic framework with silica nanoparticles, the thermal stability and initial coloring performance of PVC are improved.

Benefits of technology

It significantly improves the long-term thermal stability and initial tinting properties of PVC, extends the thermal aging time, and maintains the balance between initial tinting and long-term thermal stability under appropriate proportions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930970A_ABST
    Figure CN118930970A_ABST
Patent Text Reader

Abstract

The invention discloses a composite heat stabilizer for PVC (polyvinyl chloride) and a PVC profile, the composite heat stabilizer comprises a main stabilizer and an auxiliary stabilizer, the main stabilizer is a mixture of calcium stearate and zinc stearate, the auxiliary stabilizer is modified hydrotalcite, and the modified hydrotalcite is hydrotalcite coated with silicon dioxide nanoparticles. The hydrotalcite is modified, so that when the hydrotalcite is used as an auxiliary stabilizer for calcium-zinc thermal stability, the long-term thermal stability of a PVC product can be improved; meanwhile, the metal organic framework is added on the basis of the modified hydrotalcite, so that the initial dyeing property of the PVC product is improved while the long-term thermal stability is maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a composite heat stabilizer for PVC and a PVC profile. Background Art

[0002] PVC is the abbreviation of polyvinyl chloride. The products made from it are called PVC plastics. Because of its self-extinguishing, flame retardant, wear-resistant, high strength, good electrical insulation and chemical stability, it is known as the four basic building materials together with steel, wood and cement. It is widely used in industry, agriculture, construction, chemical industry, electronics, machinery and daily life, and has become one of the pillars of national economic development.

[0003] During the processing of PVC, people found that PVC plastic can only be processed and formed at a temperature above 160°C, and it begins to thermally decompose at 120-130°C, releasing HCl gas. HCl gas catalyzes the degradation of PVC, affecting its service life. The additives added to prevent the degradation of plastics due to heat during processing and use are called heat stabilizers.

[0004] At present, the commonly used heat stabilizers include lead salt heat stabilizers, calcium zinc composite heat stabilizers, rare earth heat stabilizers, organic tin heat stabilizers, organic heat stabilizers, etc., and their stabilization mechanisms and performances are different. Calcium zinc heat stabilizers and organic heat stabilizers are novel, low-toxic, and high-efficiency heat stabilizers that have appeared in recent years and have attracted the attention of many professionals.

[0005] Generally speaking, calcium stearate alone as a PVC heat stabilizer has good long-term thermal stability, but the initial coloring is serious and leads to poor performance. Zinc stearate has excellent initial coloring performance when used alone, but the Lewis acid ZnCl2 produced will catalyze the degradation of PVC, causing "zinc burning" and reducing its later thermal stability. Therefore, calcium stearate and zinc stearate are usually mixed in a certain ratio to form a calcium-zinc composite heat stabilizer, so that calcium stearate and zinc stearate can work synergistically to obtain better thermal stability.

[0006] Although calcium zinc heat stabilizers can improve the thermal stability of PVC processing, further research is needed to meet the requirements of different processing techniques and different products. The addition of auxiliary heat stabilizers to form a composite heat stabilizer with calcium zinc heat stabilizers can improve PVC performance, which is also the main research and development direction of calcium zinc heat stabilizers.

[0007] Prior art 1:

[0008] It is disclosed that a hydrotalcite (LDHs) heat stabilizer has a unique layered structure, can effectively absorb hydrogen chloride gas generated by PVC degradation, and significantly improve the heat resistance of PVC. Therefore, it can be used as an auxiliary heat stabilizer in combination with a calcium-zinc composite heat stabilizer. However, since hydrotalcite is an inorganic functional material with active hydroxyl functional groups on the surface, it is easy for hydrogen bonds to form between its particles to produce soft agglomeration, resulting in poor surface structural stability. Therefore, it is usually necessary to modify the hydrotalcite.

[0009] Prior art 2:

[0010] Disclosed are a calcium-zinc MOFs composite thermal stabilizer, a preparation method and an application thereof, which comprises the following components by weight: 8 to 10 parts of a main stabilizer and 0.5 to 2 parts of an auxiliary stabilizer, wherein the main stabilizer is a mixture of calcium stearate and zinc stearate, and the auxiliary stabilizer is a metal organic framework material MOFs, wherein the specific surface area of ​​the metal organic framework material MOFs is 490 m2 / g to 6240 m2 / g.

[0011] The metal organic framework material MOFs with high specific surface area, porosity and excellent gas adsorption is used as an auxiliary component of the calcium zinc stabilizer to effectively improve the stability time of the calcium zinc heat stabilizer. At the same time, MOFs can be used as a carrier for the calcium zinc stabilizer and organic additives to reduce their migration and precipitation during the processing, thereby improving the stabilization effect on PVC. It can be widely used in the production of PVC drainage pipes.

[0012] Whether hydrotalcite is used as an auxiliary thermal stabilizer or metal organic framework material MOFs is used as an auxiliary thermal stabilizer, the core idea is to eliminate the negative impact of hydrogen chloride on the degradation catalysis of PVC processing as much as possible based on the adsorption and binding properties of the auxiliary thermal stabilizer. How to improve the synergistic effect of the auxiliary thermal stabilizer on the calcium zinc thermal stabilizer is still the direction that technicians in this field are committed to studying.

[0013] Prior art 1: Yuan Haokun, Application progress of organic modified hydrotalcite in PVC thermal stabilizer[J]. Chemical Engineering Design Communications, 2022, 48(8), 99;

[0014] Prior art 2: CN116178792A. Summary of the invention

[0015] In view of the above technical problems, this application proposes a composite heat stabilizer for PVC and a PVC profile, and the specific technical solutions are as follows:

[0016] One of the purposes of the present application is to provide a composite heat stabilizer for PVC, which comprises a main stabilizer and an auxiliary stabilizer, wherein the main stabilizer is a mixture of calcium stearate and zinc stearate, and the auxiliary stabilizer is a modified hydrotalcite, and the modified hydrotalcite is a hydrotalcite coated with silica nanoparticles.

[0017] Hydrotalcite is an inorganic functional material with active hydroxyl functional groups on its surface, which can easily form hydrogen bonds between its particles to produce soft agglomerations, resulting in poor surface structural stability, poor dispersibility and compatibility in PVC particles. By coating hydrotalcite with silica nanoparticles, the stability of hydrotalcite is improved, its specific surface area is increased, and hydrotalcite is better dispersed in different media.

[0018] The silica nanoparticles described in the present application refer to functionalized silica nanoparticles, including amino-functionalized silica nanoparticles, carboxyl-functionalized silica nanoparticles and phosphate-functionalized silica nanoparticles.

[0019] Taking amino-functionalized silica nanoparticles as an example, the modification method of the modified hydrotalcite is as follows:

[0020] Adding hydrotalcite powder into deionized water and dispersing by ultrasonication to obtain a hydrotalcite suspension;

[0021] Adding tetramethylsilane to anhydrous ethanol and adding aqueous ammonia to obtain a silicon dioxide precursor solution;

[0022] Slowly adding the prepared silica precursor solution into the hydrotalcite suspension while stirring;

[0023] The mixed solution is transferred into a sealed container and allowed to age at a constant temperature;

[0024] After aging, the product was centrifuged and then washed with a large amount of deionized water and ethanol. Finally, the washed product was dried in a vacuum drying oven.

[0025] As a preferred embodiment of the above technical solution, the mass ratio of the main stabilizer to the modified hydrotalcite is 8:(1-3).

[0026] As a preferred embodiment of the above technical solution, the mass ratio of the main stabilizer to the modified hydrotalcite is 4:1.

[0027] As a preferred embodiment of the above technical solution, the auxiliary stabilizer also includes a metal organic framework, and the mass ratio of the metal organic framework in the auxiliary stabilizer exceeds 30%.

[0028] The metal organic framework is a type of crystalline porous material with a periodic network structure formed by interconnecting inorganic metal centers (metal ions or metal clusters) and bridging organic ligands through self-assembly.

[0029] As a preferred embodiment of the above technical solution, the mass ratio of the metal organic framework in the auxiliary stabilizer is 30-70%.

[0030] As a preferred embodiment of the above technical solution, the mass ratio of the metal organic framework to the modified hydrotalcite in the auxiliary stabilizer is 2:1.

[0031] As a preferred embodiment of the above technical solution, the auxiliary stabilizer is treated in the following manner:

[0032] The powders of modified hydrotalcite and metal organic framework are added to ethanol and stirred to form a suspension, which is maintained while being heated and stirred. After the suspension is completed, the mixture is cooled to room temperature, and then the precipitate is separated by centrifugation. The precipitate is repeatedly washed with a large amount of deionized water and ethanol, and finally the precipitate is dried in a vacuum oven.

[0033] After the above treatment, nano-scale silica nanoparticles are deposited on the surface of the hydrotalcite modified by coating with silica nanoparticles. When some metal organic frameworks are matched, some nano-scale silica nanoparticles deposited on the main layer will be adsorbed by the pore structure of the metal organic framework to further form a composite structure. This composite structure helps to further improve the adsorption of HCl in the degradation process of PVC as a whole, and reduce the generation of ZnCl and reduce its catalytic effect.

[0034] Another object of the present invention is to provide a PVC profile, which comprises any one of the composite heat stabilizers described above, and indispensable PVC resin powder and some additives that can be selectively added depending on specific performance requirements.

[0035] The beneficial effects of the present invention are as follows: the present application modifies the hydrotalcite so that when it is used as an auxiliary stabilizer for calcium zinc thermal stability, the long-term thermal stability applied to PVC products can be improved; at the same time, a metal organic framework is added on the basis of the modified hydrotalcite, which improves the initial colorability of the PVC products while maintaining long-term thermal stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Shown are the test results of Examples 1 to 5 and Comparative Example 1;

[0037] Figure 2 Shown are the test results of Examples 6 to 8 and Comparative Examples 2 to 7;

[0038] Figure 3The test results of Examples 9 to 16 are shown. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments.

[0040] Description of all reagents in this application:

[0041] Calcium stearate, CAS No. 1592-23-0, was purchased from the market;

[0042] Zinc stearate, CAS No. 557-05-1, was purchased from the market;

[0043] Magnesium aluminum carbonate hydrotalcite, CAS No. 12539-23-0, was purchased from the market;

[0044] Tetramethylsilane, CAS No. 75-76-3, was purchased from the market;

[0045] Metal organic framework, CAS No. 1072413-89-8, was purchased from the market.

[0046] Example 1

[0047] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 1 part of an auxiliary stabilizer.

[0048] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0049] The auxiliary stabilizer is modified hydrotalcite, and the hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased from the market.

[0050] The method for modifying hydrotalcite is:

[0051] (1) Hydrotalcite pretreatment:

[0052] 100 g of hydrotalcite powder was added to 10 L of deionized water and ultrasonically dispersed for 30 minutes to ensure that the hydrotalcite was evenly dispersed;

[0053] (2) Preparation of silicon dioxide precursor:

[0054] 100 ml of tetramethylsilane (TEOS) as a silica source was added to 5 L of anhydrous ethanol, and 50 ml of 25% aqueous ammonia (NH3) was added as a catalyst;

[0055] (3) Mixing of hydrotalcite and silica precursor:

[0056] Slowly adding the prepared silica precursor solution into the hydrotalcite suspension while stirring;

[0057] (4) Aging process:

[0058] The mixed solution was transferred into a sealed container and aged in an oven at 60°C for 24 hours to promote the hydrolysis and gelation of silica;

[0059] (5) Post-processing:

[0060] After aging, the product was centrifuged at 10,000 rpm for 10 minutes, and then washed with a large amount of deionized water and ethanol to remove unreacted precursors and by-products; finally, the washed product was dried at 80°C overnight.

[0061] Example 2

[0062] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 2 parts of an auxiliary stabilizer.

[0063] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0064] The auxiliary stabilizer is modified hydrotalcite, and the hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased from the market.

[0065] The method for modifying the hydrotalcite is the same as that in Example 1.

[0066] Example 3

[0067] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0068] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0069] The auxiliary stabilizer is modified hydrotalcite, and the hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased from the market.

[0070] The method for modifying the hydrotalcite is the same as that in Example 1.

[0071] Example 4

[0072] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 4 parts of an auxiliary stabilizer.

[0073] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0074] The auxiliary stabilizer is modified hydrotalcite, and the hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased from the market.

[0075] The method for modifying the hydrotalcite is the same as that in Example 1.

[0076] Example 5

[0077] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 5 parts of an auxiliary stabilizer.

[0078] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0079] The auxiliary stabilizer is modified hydrotalcite, and the hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased from the market.

[0080] The method for modifying the hydrotalcite is the same as that in Example 1.

[0081] Comparative Example 1

[0082] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 2 parts of an auxiliary stabilizer.

[0083] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0084] The auxiliary stabilizer is hydrotalcite, and the hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased from the market.

[0085] The composite heat stabilizers for PVC in Examples 1 to 5 and the composite heat stabilizer for PVC in Comparative Example 1 were used to prepare PVC test samples, and static heat aging tests and Congo red heat stabilization time were performed. The preparation method of the PVC test samples adopted the general means of the prior art, as follows:

[0086] 100g of PVC resin powder, 5g of calcium carbonate and 5g of composite heat stabilizer were added into a high-speed mixer respectively, mixed as experimental materials and heat-plasticized in advance, and the mixed materials were used for thermal stability test.

[0087] from Figure 1It can be seen that compared with the use of hydrotalcite as an auxiliary stabilizer, the modification of hydrotalcite has little effect on the discoloration time of Congo red, but can significantly increase the heat aging time, that is, the modified hydrotalcite can cooperate with the main stabilizer to improve the long-term thermal stability of PVC products, and with the increase of the addition amount of modified hydrotalcite, the heat aging time has an obvious trend of first increasing and then decreasing. The synergistic effect is best when the ratio of the main stabilizer to the auxiliary stabilizer is 4:1.

[0088] Example 6

[0089] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0090] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0091] The auxiliary stabilizers are modified hydrotalcite and metal organic frameworks (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 2:1, and the two are compounded in a blending manner.

[0092] The method for modifying the hydrotalcite is the same as that in Example 1.

[0093] Example 7

[0094] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 4 parts of an auxiliary stabilizer.

[0095] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0096] The auxiliary stabilizers are modified hydrotalcite and metal organic frameworks (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite and the metal organic framework is 1:1, and the two are compounded in a blending manner.

[0097] The method for modifying the hydrotalcite is the same as that in Example 1.

[0098] Example 8

[0099] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 5 parts of an auxiliary stabilizer.

[0100] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0101] The auxiliary stabilizers are modified hydrotalcite and metal organic frameworks (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 2:3, and the two are compounded in a blending manner.

[0102] The method for modifying the hydrotalcite is the same as that in Example 1.

[0103] Comparative Example 2

[0104] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 2 parts of an auxiliary stabilizer.

[0105] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0106] The auxiliary stabilizer is modified hydrotalcite, and the hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased from the market.

[0107] The method for modifying the hydrotalcite is the same as that in Example 1.

[0108] Comparative Example 3

[0109] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 1 part of an auxiliary stabilizer.

[0110] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0111] The auxiliary stabilizer is a metal organic framework, which uses terephthalic acid as a ligand and zirconium as a coordination metal and can be purchased from the market.

[0112] Comparative Example 4

[0113] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 2 parts of an auxiliary stabilizer.

[0114] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0115] The auxiliary stabilizer is a metal organic framework, which uses terephthalic acid as a ligand and zirconium as a coordination metal and can be purchased from the market.

[0116] Comparative Example 5

[0117] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0118] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0119] The auxiliary stabilizer is a metal organic framework, which uses terephthalic acid as a ligand and zirconium as a coordination metal and can be purchased from the market.

[0120] Comparative Example 6

[0121] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 4 parts of an auxiliary stabilizer.

[0122] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0123] The auxiliary stabilizer is a metal organic framework, which uses terephthalic acid as a ligand and zirconium as a coordination metal and can be purchased from the market.

[0124] Comparative Example 7

[0125] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 5 parts of an auxiliary stabilizer.

[0126] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0127] The auxiliary stabilizer is a metal organic framework, which uses terephthalic acid as a ligand and zirconium as a coordination metal and can be purchased from the market.

[0128] The composite heat stabilizers for PVC in Examples 6 to 8 and the composite heat stabilizers for PVC in Comparative Examples 2 to 7 were used to prepare PVC test samples, and static heat aging tests and Congo red heat stabilization time were performed. The preparation method of the PVC test samples adopts the general means of the prior art, as follows:

[0129] 100g of PVC resin powder, 5g of calcium carbonate and 5g of composite heat stabilizer were added into a high-speed mixer respectively, mixed as experimental materials and heat-plasticized in advance, and the mixed materials were used for thermal stability test.

[0130] from Figure 2 It can be seen from the results of Examples 6 to 8 and Comparative Example 2 that, compared with the use of modified hydrotalcite as a single component as an auxiliary stabilizer, the addition of a metal organic framework and a modified hydrotalcite as an auxiliary stabilizer can increase the time for Congo red to change color, and as the proportion of the metal organic framework in the auxiliary stabilizer increases, the effect of extending the time for Congo red to change color is also better, indicating that the metal organic framework and the modified hydrotalcite as an auxiliary stabilizer can synergistically improve the initial colorability of PVC products, and as the content of the metal organic framework is relatively increased, the improvement effect on the initial colorability of PVC products is also better; however, the newly added metal organic framework will reduce the heat aging time in the PVC product system, indicating that as the content of the metal organic framework is relatively increased, the long-term thermal stability of the PVC products will be affected, and this effect is positively correlated with the content of the metal organic framework in the auxiliary stabilizer.

[0131] In combination with Examples 6 to 8 and Comparative Examples 3 to 7, the use of a single metal organic framework as an auxiliary stabilizer can increase the time for Congo red to change color, and as the proportion of the metal organic framework in the auxiliary stabilizer increases, the effect of extending the time for Congo red to change color is also better, further illustrating that the metal organic framework as an auxiliary stabilizer can improve the initial colorability of PVC products, but even if the proportion of the metal organic framework component in Comparative Example 7 reaches 5, the effect of improving the initial colorability of PVC products is not significantly better than that of Example 6; in addition, when the metal organic framework is used as an auxiliary stabilizer in Comparative Examples 3 to 7, the heat aging time is also maintained at a medium level, which has certain advantages over the use of a single hydrotalcite as an auxiliary stabilizer, but does not have a significant advantage over the metal organic framework and modified hydrotalcite compound as an auxiliary stabilizer in Example 6.

[0132] In summary, the use of a single component of a metal organic framework as an auxiliary stabilizer helps to improve the initial colorability of PVC products, and the addition of a metal organic framework and a modified hydrotalcite as an auxiliary stabilizer can not only provide a better improvement in the initial colorability of PVC products, but also maintain the effect of the modified hydrotalcite on the long-term thermal stability of PVC products within a certain range. The effect is best when the mass ratio of the metal organic framework to the modified hydrotalcite is 1:2. As the content of the metal organic framework increases, it will have a greater impact on the long-term thermal stability of PVC products.

[0133] Example 9

[0134] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 2.1 parts of an auxiliary stabilizer.

[0135] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0136] The auxiliary stabilizers are modified hydrotalcite and metal organic frameworks (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 2:0.1, and the two are compounded by blending.

[0137] The method for modifying the hydrotalcite is the same as that in Example 1.

[0138] Example 10

[0139] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 2.5 parts of an auxiliary stabilizer.

[0140] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0141] The auxiliary stabilizers are modified hydrotalcite and metal organic frameworks (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 2:0.5, and the two are compounded by blending.

[0142] The method for modifying the hydrotalcite is the same as that in Example 1.

[0143] Embodiment 11

[0144] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0145] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0146] The auxiliary stabilizers are modified hydrotalcite and metal organic frameworks (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 2:1, and the two are compounded in a blending manner.

[0147] The method for modifying the hydrotalcite is the same as that in Example 1.

[0148] Example 12

[0149] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0150] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0151] The auxiliary stabilizers are modified hydrotalcite and metal organic framework (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 1.5:1.5, and the two are compounded by blending.

[0152] The method for modifying the hydrotalcite is the same as that in Example 1.

[0153] Embodiment 13

[0154] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0155] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0156] The auxiliary stabilizers are modified hydrotalcite and metal organic frameworks (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 1:2, and the two are compounded in a blending manner.

[0157] The method for modifying the hydrotalcite is the same as that in Example 1.

[0158] Embodiment 14

[0159] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0160] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0161] The auxiliary stabilizers are modified hydrotalcite and metal organic framework (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 0.5:2.5, and the two are compounded in a blending manner.

[0162] The method for modifying the hydrotalcite is the same as that in Example 1.

[0163] Embodiment 15

[0164] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0165] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0166] The auxiliary stabilizers are modified hydrotalcite and metal organic framework (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 0.3:2.7, and the two are compounded by blending.

[0167] The method for modifying the hydrotalcite is the same as that in Example 1.

[0168] Example 16

[0169] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0170] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0171] The auxiliary stabilizers are modified hydrotalcite and metal organic frameworks (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 0.1:2.9, and the two are compounded by blending.

[0172] The method for modifying the hydrotalcite is the same as that in Example 1.

[0173] The PVC in Examples 9 to 16 was used to prepare PVC test samples with a composite heat stabilizer, and a static heat aging test and Congo red heat stabilization time were performed. The preparation method of the PVC test samples was a common method of the prior art, as follows:

[0174] 100g of PVC resin powder, 5g of calcium carbonate and 5g of composite heat stabilizer were added into a high-speed mixer respectively, mixed as experimental materials and heat-plasticized in advance, and the mixed materials were used for thermal stability test.

[0175] from Figure 3 It can be seen from the results of Examples 9 to 11 that, in the composite component of the metal organic framework and modified hydrotalcite, when the component of the modified hydrotalcite is kept unchanged and the metal organic framework is further reduced, it is found that the effect on the thermal aging time is not obvious. However, when the content of the metal organic framework is too low, the discoloration time of Congo red is reduced, indicating that the content of the metal organic framework must reach a certain proportion when compounded with the modified hydrotalcite to increase the thermal aging time and synergistically increase the discoloration time of Congo red.

[0176] In Examples 11 to 16, the total content of the metal organic framework and the modified hydrotalcite was kept unchanged, and the proportion of the components was changed. It was found that as the content of the metal organic framework increased above 30%, the time for Congo red discoloration and the improvement of the heat aging time showed the same positive correlation trend. When the content of the metal organic framework exceeded about 70%, the time for Congo red discoloration and the improvement of the heat aging time were negatively correlated with the content of the metal organic framework. When the mass ratio of the metal organic framework to the modified hydrotalcite was 2:1, the improvement effect on the time for Congo red discoloration and the improvement of the heat aging time was most obvious, that is, under this condition, the initial coloring and long-term thermal stability of PVC products were better improved.

[0177] Embodiment 17

[0178] A composite heat stabilizer for PVC comprises the following components by weight: 8 parts of a main stabilizer and 3 parts of an auxiliary stabilizer.

[0179] The main stabilizer is a mixture of calcium stearate and zinc stearate, and the mass ratio of the two is usually set to 3:1 according to the prior art.

[0180] The auxiliary stabilizers are modified hydrotalcite and metal organic framework (MOFs). The hydrotalcite is magnesium aluminum carbonate hydrotalcite prepared by constant pH co-precipitation method, and the magnesium aluminum carbonate hydrotalcite can also be purchased commercially. The metal organic framework uses terephthalic acid as a ligand and zirconium as a coordination metal, and can be purchased commercially. In addition, the mass ratio of the modified hydrotalcite to the metal organic framework is 1:2.

[0181] Auxiliary stabilizers are treated as follows:

[0182] The powders of modified hydrotalcite and metal organic framework were added to ethanol and stirred to form a suspension. The suspension was heated and stirred at 60°C for 10 hours. After the suspension was completed, the mixture was cooled to room temperature and the precipitate was separated by centrifugation. The precipitate was repeatedly washed with a large amount of deionized water and ethanol and finally dried in a vacuum oven at 130°C for 8 hours.

[0183] Compared with Example 13, Example 17 changes the treatment method of the auxiliary stabilizer, and accordingly further increases the Congo red discoloration time and heat aging time by 30%.

[0184] The performance test experiments of all the above embodiments and comparative examples adopt the following methods.

[0185] Thermal stability test:

[0186] (1) Static thermal aging test: Take part of the plasticized experimental material and place it on tin foil, and place it in an oven at 180°C for aging test. Take samples every 10 minutes, observe the color change of the powder and take photos to record until the sample completely changes color.

[0187] (2) Congo red thermal stability time: According to GB / T 2917.1-2002, place the plasticized test material in a test tube (about 50 mm in height), fix the Congo red test paper about 25 mm above the test material, seal the tube, place the test tube in an oil bath at 180°C, start timing, and stop timing when the Congo red test paper changes color. Record the time.

[0188] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them.

Claims

1. A composite heat stabilizer for PVC, characterized in that: The invention comprises a main stabilizer and an auxiliary stabilizer, wherein the main stabilizer is a mixture of calcium stearate and zinc stearate, and the auxiliary stabilizer is modified hydrotalcite, which is hydrotalcite coated with silicon dioxide nanoparticles.

2. The composite heat stabilizer for PVC according to claim 1, characterized in that: The mass ratio of the main stabilizer to the modified hydrotalcite is 8:(1-3).

3. The composite heat stabilizer for PVC according to claim 2, characterized in that: The mass ratio of the main stabilizer to the modified hydrotalcite is 4:

1.

4. The composite heat stabilizer for PVC according to claim 2, characterized in that: The modification method of modified hydrotalcite is: Adding hydrotalcite powder into deionized water and dispersing by ultrasonication to obtain a hydrotalcite suspension; Adding tetramethylsilane to anhydrous ethanol and adding aqueous ammonia to obtain a silicon dioxide precursor solution; Slowly adding the prepared silica precursor solution into the hydrotalcite suspension while stirring; The mixed solution is transferred into a sealed container and allowed to age at a constant temperature; After aging, the product was centrifuged and then washed with a large amount of deionized water and ethanol. Finally, the washed product was dried in a vacuum drying oven.

5. The composite heat stabilizer for PVC according to claim 1, characterized in that: The auxiliary stabilizer also includes a metal organic framework, and the mass ratio of the metal organic framework in the auxiliary stabilizer exceeds 30%.

6. The composite heat stabilizer for PVC according to claim 5, characterized in that: The mass ratio of the metal organic framework in the auxiliary stabilizer is 30-70%.

7. The composite heat stabilizer for PVC according to claim 5, characterized in that: The mass ratio of the metal organic framework to the modified hydrotalcite in the auxiliary stabilizer is 2:

1.

8. The composite heat stabilizer for PVC according to claim 5, characterized in that: The auxiliary stabilizer is treated in the following manner: The powders of modified hydrotalcite and metal organic framework are added to ethanol and stirred to form a suspension, which is maintained while being heated and stirred. After the suspension is completed, the mixture is cooled to room temperature, and then the precipitate is separated by centrifugation. The precipitate is repeatedly washed with a large amount of deionized water and ethanol, and finally the precipitate is dried in a vacuum oven. 9.PVC profile, characterized in that: The PVC profile comprises the composite heat stabilizer as claimed in any one of claims 1 to 8, PVC resin powder and additives.

Citation Information

Patent Citations

  • Metal organic frame material-based composite heat stabilizer for PVC (polyvinyl chloride) and application of metal organic frame material-based composite heat stabilizer

    CN104387702A

  • Method for preparing nano silicon dioxide core-shell particle intercalation-modified ternary zinc-magnesium-aluminum hydrotalcite thermal stabilizer

    CN107245166A

  • Transparent powder calcium-zinc composite heat stabilizer for PVC and preparation method thereof

    CN112940348A

  • Method for preparing layered hydrotalcite-like PVC heat stabilizer from vermiculite

    CN115028939A

  • Silicic acid coated hydrotalcite particle powder, stabilizers for chlorine-containing resins made by using the powder, and chlorine-containing resin compositions

    EP2058280A1

Cited By

  • Non-migration type PVC transparent film for toys and preparation method of non-migration type PVC transparent film

    CN121405994A