Secondary battery

By using a combination of doped Si-based materials and graphite particles in the negative electrode active material of lithium-ion secondary batteries, the problems of increasing resistance and expansion and contraction caused by Si-based materials are solved, and efficient input and output characteristics and cycle characteristics are achieved.

CN118943462APending Publication Date: 2024-11-12PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410567619.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2024-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When using Si-based materials as the negative electrode active substances, the existing lithium-ion secondary batteries tend to reduce the input and output characteristics due to the increase in resistance, and expand and contract during charging and discharging, causing the conduction path to be disconnected, and the side reactions increase, resulting in a decrease in capacity.

Method used

The secondary battery containing Si-based materials and graphite particles as negative electrode active materials is used. By doping group VA and group VIA elements in Si, the weight ratio between graphite particles and Si-containing particles is adjusted to 9:1 to 4:6, and the weight ratio of graphite particles is improved. Input and output characteristics and suppress expansion and contraction.

Benefits of technology

A secondary battery that takes into account both input and output characteristics and cycle characteristics is realized, the capacity maintenance rate and resistance reduction effect of the battery are improved, and the expansion and contraction of the negative electrode are appropriately controlled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943462A_ABST
    Figure CN118943462A_ABST
Patent Text Reader

Abstract

The present invention provides a secondary battery which appropriately combines input / output characteristics and cycle characteristics. A secondary battery disclosed herein includes an electrode body having a positive electrode and a negative electrode. The negative electrode includes a negative electrode active material layer. The negative electrode active material layer contains graphite particles and Si-containing particles. The Si-containing particles are a complex of Si and C, and the Si is doped with an element M, and the element M is at least one of elements belonging to group VA and group VIA of the periodic table. The doping amount of the element M in the Si-containing particles is 0.1 at% to 5 at%. The weight ratio of the graphite particles to the Si-containing particles is 9: 1-4: 6.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a secondary battery. Background Art

[0002] Secondary batteries such as lithium-ion secondary batteries can be used as portable power sources for personal computers, mobile terminals, etc., and vehicle driving power sources for electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs). The negative electrode used in such a secondary battery generally has a structure in which a negative electrode active material layer containing a negative electrode active material is arranged on a negative electrode current collector.

[0003] In recent years, with the purpose of increasing the capacity of secondary batteries, the use of Si-based materials as negative electrode active materials has been studied (for example, Japanese Patent Application Publication No. 2022-507948, Japanese Patent Application Publication No. 2016-152213). Japanese Patent Application Publication No. 2022-507948 discloses a sulfur-doped silicon negative electrode material having an average width of 500nm to 3μm and an average diameter of 1μm to 5μm. In addition, Japanese Patent Application Publication No. 2016-152213 discloses a negative electrode active material particle containing silicon, oxygen, and boron, and the concentration of oxygen and boron is inclined.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application No. 2022-507948

[0007] Patent Document 2: Japanese Patent Application Publication No. 2016-152213 Summary of the invention

[0008] In the negative electrode with a high Si content, there is a possibility of a decrease in input-output characteristics and Li precipitation due to increased resistance. In addition, as disclosed in the Japanese Patent Application Publication No. 2022-507948, when only doped silicon is used as the negative electrode active material, the resistance is small and the input-output characteristics of the secondary battery are high. On the other hand, there is a tendency for expansion and contraction during charge and discharge to increase. Therefore, there is a tendency for the conductive path to be disconnected, and a decrease in capacity due to increased side reactions.

[0009] The present invention has been made in view of the above circumstances and provides a secondary battery including a negative electrode containing a Si-based material and graphite particles as a negative electrode active material, and which appropriately achieves both input-output characteristics and cycle characteristics.

[0010] The secondary battery disclosed herein is a secondary battery having an electrode body having a positive electrode and a negative electrode, wherein the negative electrode has a negative electrode collector and a negative electrode active material layer disposed on the negative electrode collector. The negative electrode active material layer contains graphite particles and Si-containing particles as negative electrode active materials. The Si-containing particles are a composite of Si and C, and the Si of the Si-containing particles is doped with an element M. The element M is at least one element belonging to the VA group and the VIA group of the periodic table. The doping amount of the element M in the Si-containing particles is 0.1 at% to 5 at%. The weight ratio of the graphite particles to the Si-containing particles is 9:1 to 4:6.

[0011] According to the above configuration, by doping the Si-containing particles containing Si and C with the element M, the input-output characteristics can be improved, and the expansion and contraction of Si accompanying charge and discharge can be appropriately suppressed. In addition, by containing the Si-containing particles and the graphite particles in the above weight ratio, the expansion and contraction of the negative electrode active material as a whole can be appropriately suppressed. Therefore, a secondary battery that takes into account both the input-output characteristics and the cycle characteristics can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a diagram schematically showing the internal structure of a secondary battery according to one embodiment.

[0013] Figure 2 It is a diagram schematically showing the structure of an electrode body according to one embodiment.

[0014] Figure 3 This is a diagram schematically showing a negative electrode according to one embodiment.

[0015] Explanation of symbols

[0016] 20 Electrode body

[0017] 30 Battery housing

[0018] 36 Safety valve

[0019] 42 Positive terminal

[0020] 42a Positive electrode collector plate

[0021] 44 Negative terminal

[0022] 44a Negative collector plate

[0023] 50 positive electrode (positive electrode sheet)

[0024] 52 positive electrode collector

[0025] 52a Positive electrode current collector exposed portion

[0026] 54 Positive electrode active material layer

[0027] 60 Negative electrode (negative electrode sheet)

[0028] 62 negative electrode collector

[0029] 62a Negative electrode current collector exposed portion

[0030] 64 Negative electrode active material layer

[0031] 66 Graphite particles

[0032] 68 Containing Si particles

[0033] 68a Porous carbon materials

[0034] 68b Si nanoparticles

[0035] 68p fine hole

[0036] 70 Spacer

[0037] 100 Secondary batteries DETAILED DESCRIPTION

[0038] Hereinafter, the implementation of the technology disclosed herein will be described with reference to the accompanying drawings. It should be noted that matters other than those specifically mentioned in this specification and matters required for the implementation of the technology disclosed herein (for example, the general structure and manufacturing process of the secondary battery that does not characterize the technology disclosed herein, etc.) can be grasped as design matters of a person skilled in the art based on the prior art in this field. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in this field. It should be noted that each of the drawings is drawn schematically, and the dimensional relationship (length, width, thickness, etc.) does not necessarily reflect the actual dimensional relationship. In addition, in the drawings described below, the same symbols are marked for components and parts that play the same role, and repeated descriptions are omitted or simplified. In addition, in this specification, the expression "A~B" (A and B are arbitrary numerical values) indicating a range includes the meaning of above A and below B, as well as the meaning of "greater than A (exceeding A)" and "less than B (less than B)".

[0039] Figure 1 Schematic diagram of the internal structure of a secondary battery 100 according to one embodiment. Figure 1 As shown, the secondary battery 100 includes an electrode body 20 having a positive electrode 50 and a negative electrode 60, a non-aqueous electrolyte (not shown), and a battery case 30 that accommodates the electrode body 20 and the non-aqueous electrolyte. Figure 1The secondary battery 100 shown is a lithium ion secondary battery. The negative electrode 60 disclosed herein is preferably used as a negative electrode for a lithium ion secondary battery.

[0040] The battery case 30 is provided with a positive terminal 42, a negative terminal 44 and a thin safety valve 36 for external connection, and the thin safety valve 36 is set to release the internal pressure of the battery case 30 when the internal pressure rises to a predetermined level or above. In addition, the battery case 30 is provided with an injection port (not shown) for injecting a non-aqueous electrolyte. The positive terminal 42 is electrically connected to the positive electrode collector plate 42a. The negative terminal 44 is electrically connected to the negative electrode collector plate 44a. As the material of the battery case 30, for example, a metal material such as aluminum, which is lightweight and has good thermal conductivity, can be used.

[0041] Figure 2 2 is a diagram schematically showing the structure of the electrode body 20. Here, the electrode body 20 is a flat wound electrode body. Figure 2 As shown, the electrode body 20 has the following form: a long sheet of positive electrode 50 (hereinafter also referred to as "positive electrode sheet 50") and a long sheet of negative electrode 60 (hereinafter also referred to as "negative electrode sheet 60") overlap with two long strips of separators 70 and are wound along the long side direction. The positive electrode sheet 50 has a structure in which a positive electrode active material layer 54 is formed on one side or both sides (here both sides) of a long strip of positive electrode collector 52 along the length direction. The negative electrode sheet 60 has a structure in which a negative electrode active material layer 64 is formed on one side or both sides (here both sides) of a long strip of negative electrode collector 62 along the length direction. As Figure 1 and Figure 2 As shown, the positive electrode current collector exposed portion 52a (i.e., the portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode current collector exposed portion 62a (i.e., the portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends of the winding axial direction (i.e., the sheet width direction orthogonal to the above-mentioned long side direction) of the electrode body 20. The positive electrode current collector plate 42a and the negative electrode current collector plate 44a are joined to the positive electrode current collector exposed portion 52a and the negative electrode current collector exposed portion 62a, respectively.

[0042] As the positive electrode collector 52 constituting the positive electrode sheet 50, a known positive electrode collector used in a lithium-ion secondary battery can be used without particular limitation. For example, sheets or foils made of metals with good electrical conductivity (such as aluminum, nickel, titanium, stainless steel, etc.) can be cited. As the positive electrode collector 52, aluminum foil is preferred. The size of the positive electrode collector 52 is not special, as long as it is appropriately determined according to the battery design. When aluminum foil is used as the positive electrode collector 52, its thickness is not particularly limited, for example, 5μm to 35μm, preferably 7μm to 20μm.

[0043] The positive electrode active material layer 54 contains a positive electrode active material. As the positive electrode active material, a known positive electrode active material used in lithium ion secondary batteries can be used. Specifically, for example, as the positive electrode active material, a lithium composite oxide, a lithium transition metal phosphate compound (such as lithium iron phosphate (LiFePO4)) can be used. 4 ), lithium manganese phosphate (LiMnPO 4 )) etc. The crystal structure of the positive electrode active material is not particularly limited, and may be a layered structure, a spinel structure, an olivine structure, or the like.

[0044] As the lithium composite oxide, it is preferred to contain at least one of Ni, Co, and Mn as transition metal elements. As specific examples thereof, lithium nickel composite oxides, lithium cobalt composite oxides, lithium manganese composite oxides, lithium nickel manganese composite oxides, lithium nickel cobalt manganese composite oxides, lithium nickel cobalt manganese composite oxides, lithium nickel cobalt aluminum composite oxides, lithium iron nickel manganese composite oxides, etc. can be cited. These positive electrode active materials can be used alone or in combination of two or more. Among them, lithium nickel cobalt manganese composite oxides can be preferably used as the positive electrode active material.

[0045] It should be noted that in this specification, "lithium nickel cobalt manganese composite oxide" is a term that includes oxides containing one or more additional elements other than Li, Ni, Co, Mn, and O as constituent elements. Examples of the above-mentioned additional elements include transition metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn, typical metal elements, and the like. In addition, the additional elements may also be metalloid elements such as B, C, Si, and P, and non-metallic elements such as S, F, Cl, Br, and I. This is also the same for the above-mentioned lithium nickel composite oxides, lithium cobalt composite oxides, lithium manganese composite oxides, lithium nickel manganese composite oxides, lithium nickel cobalt aluminum composite oxides, and lithium iron nickel manganese composite oxides.

[0046] The positive electrode active material layer 54 may further include components other than the positive electrode active material, such as a conductive material, a binder, etc. As the conductive material, carbon black such as acetylene black (AB); carbon fibers such as vapor grown carbon fiber (VGCF) and carbon nanotubes (CNT); and other carbon materials (such as graphite, etc.) may be preferably used. As the binder, for example, polyvinylidene fluoride (PVdF) may be used.

[0047] Although not particularly limited, the content of the positive electrode active material in the positive electrode active material layer (i.e., the content of the positive electrode active material relative to the total weight of the positive electrode active material layer 54) is preferably 70 wt% or more, more preferably 80 wt% to 99 wt%, and can also be 85 wt% to 98 wt%. In addition, the content of the conductive material in the positive electrode active material layer is not particularly limited, but is preferably 0.5 wt% to 5 wt%, and more preferably 0.7 wt% to 5 wt%. In addition, the content of the binder in the positive electrode active material layer is not particularly limited, but is preferably 0.5 wt% to 5 wt%, and more preferably 0.7 wt% to 5 wt%.

[0048] The thickness per side of the positive electrode active material layer 54 is not particularly limited, and is, for example, 20 μm or more, preferably 50 μm or more. On the other hand, the thickness per side of the positive electrode active material layer 54 is, for example, 300 μm or less, preferably 200 μm or less.

[0049] As the separator 70, various microporous sheets similar to those in the past can be used, for example, microporous resin sheets made of resins such as polyethylene (PE) and polypropylene (PP). The microporous resin sheet can be a single-layer structure or a multi-layer structure of two or more layers (for example, a three-layer structure in which PP layers are stacked on both sides of a PE layer). In addition, the separator 70 can also have a heat-resistant layer (HRL).

[0050] The non-aqueous electrolyte may use the same material as in the past. For example, a non-aqueous electrolyte solution containing a supporting salt in an organic solvent (non-aqueous solvent) may be used. As the non-aqueous solvent, aprotic solvents such as carbonates, esters, and ethers may be used. Among them, carbonates may be appropriately used such as ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), etc. Alternatively, fluorinated solvents such as fluorinated carbonates such as monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC) may be preferably used. Such non-aqueous solvents may be used alone or in appropriate combinations of two or more. As the supporting salt, for example, LiPF may be preferably used. 6 , LiBF 4 、LiClO 4 The concentration of the supporting salt is not particularly limited, but is preferably about 0.7 mol / L to 1.3 mol / L. It should be noted that the non-aqueous electrolyte may also contain ingredients other than the non-aqueous solvent and supporting salt, such as various additives such as a gas generating agent, a film forming agent, a dispersant, and a thickening agent, as long as the effect of the present technology is not significantly impaired.

[0051] Next, the negative electrode 60 of the secondary battery disclosed here will be described. Figure 3 Schematically shows the negative electrode 60 of the secondary battery 100 disclosed herein. Figure 3 As shown, the negative electrode 60 includes a negative electrode collector 62 and a negative electrode active material layer 64 disposed on the negative electrode collector 62. The negative electrode collector 62 can use a conventionally known material without particular limitation. Examples include sheets or foils made of metals such as copper, nickel, titanium, and stainless steel. When copper foil is used as the negative electrode collector 62, its average thickness is not particularly limited, and is, for example, 5 μm to 30 μm, preferably 5 μm to 20 μm, and more preferably 5 μm to 15 μm.

[0052] The negative electrode active material layer 64 contains at least a negative electrode active material. The negative electrode active material layer 64 contains graphite particles 66 and Si-containing particles 68 as negative electrode active materials. The above-mentioned Si-containing particles 68 are doped with at least one element of the VA group and the VIA group of the periodic table. Moreover, in the negative electrode active material layer 64 disclosed here, the weight ratio of these graphite particles 66 to the Si-containing particles 68 is 9:1 to 4:6. According to the above-mentioned structure, a secondary battery 100 that takes into account both cycle characteristics and input-output characteristics can be achieved. It should be noted that in this specification, "doping" means adding elements of the VA group and the VIA group that are different from the Si-containing particles to the Si-containing particles as a small amount of additives.

[0053] Although it is not intended to limit the technology disclosed herein, the reasons why the above effects can be obtained are presumed to be as follows. By doping Si with element M, a metal phase transition (insulator to metal transition) occurs, and the conductivity is improved. As a result, the input and output characteristics of the secondary battery can be improved. On the other hand, the expansion and contraction of the negative electrode accompanying charging and discharging tends to increase, the conductive path is disconnected, the side reactions increase, and the cycle characteristics (such as capacity retention rate) of the secondary battery may decrease. Therefore, in the secondary battery 100 disclosed herein, by making the Si doped with element M into Si-containing particles 68 containing Si and C, the expansion and contraction of Si accompanying charging and discharging can be suppressed. Furthermore, in the secondary battery 100 disclosed herein, by including graphite particles 66 and Si-containing particles 68 in a prescribed ratio, the expansion and contraction of the negative electrode as a whole can be more appropriately controlled. According to the above-mentioned structure, a secondary battery 100 that appropriately takes into account both input and output characteristics and cycle characteristics can be realized.

[0054] As the graphite particles 66, for example, artificial graphite, natural graphite, etc. can be used. The graphite particles 66 can have a non-carbon coating layer on their surface. Although not particularly limited, the graphite particles 66 can be roughly spherical. It should be noted that in this specification, "roughly spherical" is a term that includes spherical, rugby-shaped, etc., for example, it refers to a shape with an average aspect ratio (the ratio of the length in the major axis direction to the length in the minor axis direction in the smallest rectangle circumscribed by the particle) of, for example, 1 to 2 (preferably 1 to 1.5).

[0055] The average particle size (D 50 The average particle size of the graphite particles is not particularly limited, and is preferably 5 μm to 30 μm, and more preferably 10 μm to 25 μm. If it is in the above range, the expansion and contraction of the negative electrode as a whole can be appropriately suppressed. It should be noted that in this specification, the "average particle size of the graphite particles" refers to the particle size (D) equivalent to 50% of the cumulative volume from the microparticle side in the particle size distribution measured by the particle size distribution measurement based on the laser diffraction and light scattering method. 50 particle size).

[0056] The Si-containing particles 68 are not particularly limited as long as they are particles containing Si and C. As long as the Si-containing particles 68 contain Si and C, they may also contain components other than Si and C. As the Si-containing particles 68, it is preferred to use a Si-C complex. The Si-C complex can be formed by, for example, supporting Si metal, Si oxide, etc. in a carbon material (graphite, porous carbon material, etc.). The Si-containing particles 68 are preferably, for example, Figure 3 The structure shown includes a porous carbon material 68a and Si nanoparticles 68b. The porous carbon material 68a includes pores 68p, and the Si nanoparticles 68b are arranged in the pores 68p of the porous carbon material 68a.

[0057] Although not particularly limited, when the total weight of the Si-containing particles 68 is set to 100wt%, the Si content of the Si-containing particles 68 is preferably 30wt% or more, more preferably 40wt% or more, and further preferably 50wt% or more. Thus, a high capacity of the secondary battery 100 can be achieved. In addition, the resistance reduction effect brought about by the doping element M can be more appropriately exerted. The upper limit of the Si content in the Si-containing particles 68 is not particularly limited, and is preferably 75wt% or less, and can also be 70wt% or less. Thus, the input-output characteristics and the cycle characteristics can be appropriately taken into account. It should be noted that the Si content in the Si-containing particles can be confirmed using an inductively coupled plasma optical emission spectrometry (ICP-OES) device.

[0058] Although not particularly limited, the average particle size (D 50The particle size) is preferably 0.5 μm to 20 μm, and more preferably 1 μm to 15 μm. It should be noted that in this specification, the "average particle size of Si-containing particles" refers to the particle size (D) corresponding to 50% of the cumulative volume from the microparticle side in the particle size distribution measured by the particle size distribution measurement based on the laser diffraction / light scattering method. 50 particle size).

[0059] The Si-containing particle 68 preferably has a plurality of pores (voids) 68p therein. The Si-containing particle 68 has the pores 68p, so that the expansion and contraction accompanying charge and discharge can be appropriately suppressed. Although not particularly limited, the Si-containing particle 68 preferably has a plurality of pores 68p with a small average pore diameter. Since the pores 68p are small, there is a tendency for the pores 68p to remain even when pressing is performed when the negative electrode 60 is manufactured. Therefore, the expansion and contraction of the Si-containing particle 68 accompanying charge and discharge can be more appropriately alleviated, and the cycle characteristics can be improved.

[0060] The porosity of the Si-containing particles 68 is preferably, for example, 5 vol% or more. The upper limit of the porosity is not particularly limited, and may be, for example, 60 vol% or less. It should be noted that the "porosity" can be calculated based on the formula: porosity (%) = (1-bulk density of Si-containing particles / true density of Si-containing particles) × 100.

[0061] Although not particularly limited, the oxygen content in the Si-containing particles 68 may be, for example, 7 wt % or less when the total Si-containing particles are 100 wt %. The oxygen content can be measured by an oxygen analyzer.

[0062] The Si nanoparticles 68b contained in the Si-containing particles 68 are particles containing Si of nanometer size (i.e., less than 1 μm). The Si nanoparticles 68b may be present in the pores 68p of the porous carbon material 68a. By the presence of the Si nanoparticles 68b in the pores 68p of the porous carbon material 68a, the expansion and contraction of the Si nanoparticles 68b is suppressed, and the expansion and contraction of the Si-containing particles themselves can also be appropriately suppressed. Thus, high capacity can be achieved and cycle characteristics can be improved.

[0063] Although not particularly limited, the Si nanoparticle 68b is preferably less than 100nm, and more preferably less than 50nm. As a result, the amount of expansion and contraction of each Si nanoparticle 68b during charge and discharge can be reduced, and it is difficult to break even if it expands and contracts repeatedly. In addition, although not particularly limited, the average particle size of the Si nanoparticle 68b can be, for example, more than 5nm. It should be noted that in this specification, the "average particle size of Si nanoparticles" can be calculated as follows. First, for the negative electrode active material layer, a sample for scanning transmission electron microscopy (STEM) observation is prepared by FIB (focused ion beam) processing. Then, the sample is elementally analyzed by EDX element mapping, and a BF image (bright field image) and a HAADF image (high-angle scattering annular dark field image) are obtained. Based on the contrast and shape obtained from the BF image and the HAADF image, the diameter of the Si nanoparticle can be calculated. The arithmetic average of the diameters of at least 10 Si nanoparticles is used as the "average particle size of Si nanoparticles" here.

[0064] As described above, the Si-containing particles 68 are doped with at least one element M in the VA group and the VIA group of the periodic table. That is, the Si-containing particles 68 contain at least one element M in the VA group and the VIA group of the periodic table. Specific examples of the above-mentioned element M include sulfur (S), phosphorus (P), nitrogen (N), arsenic (As), antimony (Sb), bismuth (Bi), selenium (Se), tellurium (Te), and polonium (Po). Among them, S and P can be preferably used as the element M. It should be noted that the Si-containing particles 68 can be doped with one of the above-mentioned elements alone, or with a combination of two or more.

[0065] The doping amount (i.e., content) of element M in the Si-containing particles 68 is preferably greater than 0.1 at%, more preferably greater than 0.5 at%, and further preferably greater than 1 at%. Thus, the resistance reduction effect brought about by the doping element M can be properly exerted, and the input-output characteristics can be improved. On the other hand, when the doping amount is too much, the resistance reduction effect tends to decrease. The doping amount of element M is preferably less than 5 at%, more preferably less than 4 at%, and further preferably less than 3 at%. It should be noted that, with respect to the doping amount, "at%" refers to the atomic composition percentage (atomic percent, atomic percent). The doping of element M in the Si-containing particles and its doping amount can be confirmed using an inductively coupled plasma optical emission spectrometry (ICP-OES) device.

[0066] In the Si-containing particles 68, the element M may be contained only on the surface of the Si nanoparticles 68b, or may be uniformly diffused inside the Si nanoparticles 68b. Preferably, in the Si-containing particles 68, the element M is uniformly diffused inside the Si nanoparticles 68b. Thus, the resistance reduction effect can be more appropriately improved. Although not particularly limited, it is preferred that the element M does not form a compound with Si and / or C in the Si-containing particles 68.

[0067] The Si-containing particles 68 of the present embodiment can be appropriately manufactured by the following method. It should be noted that the following description will be given by taking as an example the case where the Si-containing particles 68 are doped with sulfur (S) as the element M. However, the Si-containing particles 68 of the present embodiment are not limited to particles manufactured by the following manufacturing method.

[0068] A suitable method for producing the Si-containing particles 68 of the present embodiment may include at least a step of mixing a SiO—C composite (porous carbon material—SiO), a sulfate compound, and a metal reducing agent (mixing step), and a step of heating the mixture (heating step).

[0069] In the mixing step, the SiO-C complex, the sulfate compound, and the metal reducing agent are mixed to prepare a mixture. The mixing method in the mixing step is not particularly limited, and for example, mixing can be performed using a mortar. In addition, the sulfate compound used in the mixing step is not particularly limited, and examples thereof include magnesium sulfate, barium sulfate, sodium sulfate, and the like. The metal reducing agent is not particularly limited, and may be Mg, Al, and the like.

[0070] Next, in a heating process, the mixture prepared as above is heated to perform a reduction reaction. In the heating process, sulfur (S) is selectively reduced, and S is doped into the SiO-C composite. The heating process is preferably carried out in an inert atmosphere (for example, an argon atmosphere, a nitrogen atmosphere, etc.) at a heating temperature of 200°C to 500°C. In addition, the heating time is not particularly limited, and for example, it can be about 0.1 to 10 hours. It should be noted that the method for manufacturing Si-containing particles 68 of the present embodiment may also include the following steps: after the heating process (after the reduction reaction is completed), the reactants are dispersed in a solvent (for example, water, etc.) to remove sulfate compounds and the like.

[0071] Although not particularly limited, the weight ratio of the graphite particles 66 to the Si-containing particles 68 is preferably adjusted to 9:1 to 4:6, more preferably 9:1 to 5:5, and may also be adjusted to 7:3 to 5:5. By adjusting the weight ratio of the graphite particles 66 to the Si-containing particles 68 to the above range, the expansion and contraction of the entire negative electrode can be appropriately suppressed. Thus, the improvement of the cycle characteristics and the improvement of the input-output characteristics of the secondary battery 100 can be appropriately taken into account.

[0072] Unless the effect of the present technology is significantly impaired, the negative electrode active material layer 64 may further include Si-containing particles (second Si-containing particles) other than Si-containing particles containing Si and C. Examples of the second Si-containing particles include SiOx and particles in which Si nanoparticles not doped with other elements are dispersed in porous particles.

[0073] The negative electrode active material layer 64 preferably includes a conductive material in addition to the above-mentioned negative electrode active material (graphite particles 66 and Si-containing particles 68). As a conductive material, carbon nanotubes such as single-layer carbon nanotubes (SWCNT), double-layer carbon nanotubes (DWCNT), multi-layer carbon nanotubes (MWCNT), carbon black such as acetylene black (AB), carbon fiber, etc. can be used. Among them, carbon nanotubes are preferred, and single-layer carbon nanotubes are more preferred. By using carbon nanotubes as conductive materials, the conductive path can be further appropriately maintained, and the cycle characteristics of the secondary battery 100 can be more appropriately improved.

[0074] The content of the negative electrode active material in the negative electrode active material layer (i.e., the content of the negative electrode active material relative to the total weight of the negative electrode active material layer 64) is not particularly limited, and is preferably 80 wt% or more, more preferably 90 wt% to 99 wt%, and may also be 95 wt% to 99 wt%. In addition, the content of the conductive material in the negative electrode active material layer is not particularly limited, and is preferably 0.01 wt% to 1 wt%, and more preferably 0.05 wt% to 0.5 wt%.

[0075] The negative electrode active material layer 64 may further include a binder in addition to the above-mentioned negative electrode active material. As the binder, a conventionally known binder can be used. Examples of the binder include carboxymethyl cellulose (CMC), polyacrylic acid (PAA), styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), and the like. Among them, CMC, PAA, and SBR can be preferably used. In addition, although not particularly limited, it is more preferred to use CMC, PAA, and SBR in combination. The content of the binder in the negative electrode active material layer is not particularly limited, but is preferably 1wt% to 10wt%, and more preferably 1.5wt% to 7wt%.

[0076] The thickness per side of the negative electrode active material layer 64 is not particularly limited, and is, for example, 20 μm or more, preferably 50 μm or more. On the other hand, the thickness per side of the negative electrode active material layer 64 is, for example, 300 μm or less, preferably 200 μm or less.

[0077] The negative electrode active material layer 64 can be formed by dispersing the graphite particles 66 and Si-containing particles 68 as the negative electrode active material and materials used as needed (e.g., conductive materials, binders) in an appropriate solvent (e.g., water) to prepare a paste (or slurry) composition, applying the composition on the surface of the negative electrode collector 62 and drying it. Then, pressing is performed as needed, thereby adjusting the thickness and density of the negative electrode active material layer 64.

[0078] The above describes the structure of the negative electrode 60 and the structure of the secondary battery 100 according to one embodiment. The negative electrode 60 can be applied to a non-aqueous electrolyte secondary battery. The conductivity of the negative electrode 60 is improved by doping the element M in Si. In addition, the negative electrode 60 can appropriately suppress the disconnection of the conductive path caused by expansion and contraction due to repeated charge and discharge. Therefore, a secondary battery 100 that appropriately takes into account input-output characteristics and cycle characteristics can be realized. The secondary battery 100 can be used in various applications, for example, it can be appropriately used as a power source (driving power source) for a motor mounted on a vehicle such as a car or a truck. The type of vehicle is not particularly limited, and examples thereof include plug-in hybrid electric vehicles (PHEV; Plug-in Hybrid Electric Vehicle), hybrid electric vehicles (HEV; Hybrid Electric Vehicle), electric vehicles (BEV; Battery Electric Vehicle), etc. The secondary battery 100 can also be applied to the construction of a battery pack.

[0079] In the secondary battery 100 described above, a wound electrode body is exemplified as the electrode body 20 , but the present invention is not limited thereto. For example, an electrode body in which a plurality of substantially rectangular positive electrodes and a plurality of substantially rectangular negative electrodes are alternately stacked with separators interposed therebetween, i.e., a stacked electrode body, may also be used.

[0080] Hereinafter, test examples of the present invention will be described, but the present invention is not intended to be limited to the contents shown in the following test examples.

[0081] <Example 1>

[0082] First, as negative electrode active materials, Si-containing particles (Si-C composite, Si content: 50 wt %, doping amount: 3 at %) and graphite particles (D 50Particle size: 15 μm). In addition, single-walled carbon nanotubes (SWCNT) were prepared as a conductive material. Then, carboxymethyl cellulose (CMC), polyacrylic acid (PAA) and styrene-butadiene rubber (SBR) were prepared as a binder. These were kneaded with water as a solvent in a weight ratio of graphite particles: Si-containing particles: SWCNT: CMC: PAA: SBR = 70:30:0.1:1:1:1.5 to prepare a slurry for forming a negative electrode active material layer.

[0083] Specifically, the mixing and kneading of the slurry for forming the negative electrode active material layer is carried out as follows. First, Si-containing particles, paste SWCNT (solid content 2%) and a dispersion medium are added, and a disperser is used to disperse and mix them at 3000 rpm to prepare a paste. Next, a stirring granulator is used to dry-mix the graphite particles, CMC and PAA. Then, the paste prepared above, the mixed powder obtained by dry mixing and the dispersion medium are thickened and kneaded. The solid content during thickening and kneading is 65%. SBR and a solvent (water) are further added to the mixture after thickening and kneading and mixed. Thus, a slurry for forming a negative electrode active material layer is prepared. The slurry is applied to both sides of a copper foil (thickness 10 μm) into a strip shape. Then, the slurry on the copper foil is dried, pressed to a specified thickness, and processed into a specified size to prepare a negative electrode sheet.

[0084] Next, prepare lithium nickel cobalt manganese composite oxide (NCM) as a positive electrode active material, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder. These are mixed with N-methylpyrrolidone (NMP) as a solvent in a weight ratio of NCM:AB:PVDF=100:1:1 to prepare a slurry for forming a positive electrode active material layer. The slurry is applied to both sides of an aluminum foil (thickness 15μm) in a strip shape. Then, the slurry on the aluminum foil is dried, pressed to a specified thickness, and processed into a specified size to make a positive electrode sheet.

[0085] The negative electrode sheet and the positive electrode sheet prepared as above are stacked with a separator between them to produce a stacked electrode body. Wires for current collection are respectively installed on the positive electrode sheet and the negative electrode sheet, and the stacked electrode body is inserted into an outer casing composed of an aluminum laminate sheet. A non-aqueous electrolyte is injected into the interior of the outer casing, and the opening of the outer casing is sealed to produce the test battery of Example 1. It should be noted that as a separator, a porous polyolefin sheet having a three-layer structure of PP / PE / PP is used. In addition, as a non-aqueous electrolyte, LiPF as a supporting salt is used in a mixed solvent obtained by mixing ethylene carbonate (EC), fluorinated ethylene carbonate (FEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of EC:FEC:EMC:DMC=15:5:40:40. 6The electrolyte solution is dissolved at a concentration of 1 mol / L.

[0086] <Example 2>

[0087] An evaluation cell of Example 2 was prepared in the same manner as in Example 1 except that Si-containing particles doped with phosphorus (P) (Si—C composite, Si content: 50 wt %, doping amount: 3 at %) were prepared as Si-containing particles.

[0088] <Example 3>

[0089] An evaluation battery of Example 3 was prepared in the same manner as in Example 1 except that the blending ratio of each material was changed so as to have a weight ratio of graphite particles: Si-containing particles: SWCNT: CMC: PAA: SBR = 90:10:0.1:1:1:1.5.

[0090] <Example 4>

[0091] An evaluation battery of Example 4 was prepared in the same manner as in Example 1 except that the mixing ratio of each material was changed so as to have a weight ratio of graphite particles: Si-containing particles: SWCNT: CMC: PAA: SBR = 50:50:0.1:1:1:1.5.

[0092] <Example 5>

[0093] An evaluation battery of Example 5 was prepared in the same manner as in Example 1 except that Si-containing particles having a Si content of 25 wt % were prepared.

[0094] <Example 6>

[0095] An evaluation battery of Example 6 was prepared in the same manner as in Example 1 except that Si-containing particles having a Si content of 75 wt % were prepared.

[0096] <Example 7>

[0097] An evaluation cell of Example 7 was prepared in the same manner as in Example 1 except that undoped Si-containing particles were prepared as Si-containing particles.

[0098] <Example 8>

[0099] An evaluation battery of Example 8 was prepared in the same manner as in Example 1 except that undoped Si-containing particles were prepared and the blending ratio of each material was changed so that the weight ratio of graphite particles: Si-containing particles: SWCNT: CMC: PAA: SBR = 50:50:0.1:1:1:1.5.

[0100] <Example 9>

[0101] An evaluation cell of Example 9 was prepared in the same manner as in Example 1 except that Si-containing particles in which the S doping amount was 6 at % were prepared.

[0102] <Example 10>

[0103] An evaluation cell of Example 10 was prepared in the same manner as in Example 1 except that Si-containing particles in which the P doping amount was 6 at % were prepared.

[0104] <Example 11>

[0105] An evaluation battery of Example 11 was prepared in the same manner as in Example 1 except that the blending ratio of each material was changed so as to have a weight ratio of graphite particles: Si-containing particles: SWCNT: CMC: PAA: SBR = 30:70:0.1:1:1:1.5.

[0106] <Evaluation of Cycle Capacity Retention Rate>

[0107] Under 25°C environment, CCCV charging (rate 0.4C until 4.2V, then 0.1C cutoff) was performed, and then CC discharge (rate 0.4C, 2.5V cutoff) was performed, which was set as 1 cycle, and the capacity at this time was set as the initial capacity. A cycle test was performed by repeating 200 cycles of charge and discharge. The discharge capacity (initial capacity) of the first cycle and the discharge capacity of the 200th cycle were measured, and the cycle capacity maintenance rate was calculated by the following formula (1). The higher the cycle capacity maintenance rate, the higher the cycle characteristics of the secondary battery. The results are shown in Table 1.

[0108] Cycle capacity retention rate (%) = ((discharge capacity at the 200th cycle) / (discharge capacity at the 1st cycle)) × 100 Formula (1)

[0109] <Evaluation of IV resistance>

[0110] Under a 25°C environment, the initial capacity of each evaluation battery is set to its respective SOC 100%, and each evaluation battery is charged to an SOC of 50% in a constant temperature chamber at 25°C. Next, in a constant temperature chamber at 25°C, charge for 10 seconds at current values ​​of 0.1C, 0.2C, 0.5C, 1C, and 2C, and measure the battery voltage after charging at each current value. Plot each current value and each battery voltage to find the IV characteristics during charging, and find the IV resistance (mΩ) during discharge based on the slope of the obtained straight line. The results are shown in Table 1. It should be noted that the smaller the IV resistance value, the higher the input-output characteristics.

[0111] [Table 1]

[0112]

[0113] As shown in Table 1, it can be seen that in the evaluation batteries of Examples 1 to 6, the capacity retention rate is 76% or more, and the IV resistance is 103 mΩ or less. According to these results, by including graphite particles and Si-containing particles as negative electrode active materials, the Si-containing particles contain Si and C, and the Si of the Si-containing particles is doped with at least one element belonging to the VA group and the VIA group of the periodic table, and the weight ratio of the graphite particles to the Si-containing particles is 9:1 to 4:6, it is possible to realize a secondary battery that takes into account both excellent cycle characteristics and input-output characteristics.

[0114] In addition, as shown in Table 1, it can be seen that in Examples 1 to 4 and 6 where the Si content in the Si-containing particles is 30wt% to 75wt%, the capacity retention rate is greater than 76% and the IV resistance is less than 100mΩ, which more appropriately takes into account the input-output characteristics and cycle characteristics of the secondary battery.

[0115] Several embodiments of the present invention have been described above, but the above embodiment is only an example. The present invention can also be implemented in various other ways. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology recorded in the scope of the request includes the technology obtained by variously deforming and changing the above-mentioned exemplified embodiments. For example, part of the above-mentioned embodiment can be replaced by other deformation modes, and other deformation modes can be added to the above-mentioned embodiment. In addition, if it is not stated that the technical feature is a necessary feature, it can also be appropriately deleted.

[0116] In summary, as specific aspects of the technology disclosed herein, the following items can be cited.

[0117] Item 1: A secondary battery having an electrode body having a positive electrode and a negative electrode, the negative electrode having a negative electrode collector and a negative electrode active material layer arranged on the negative electrode collector, the negative electrode active material layer comprising graphite particles and Si-containing particles as negative electrode active materials, the Si-containing particles being a composite of Si and C, the Si of the Si-containing particles being doped with an element M, the element being at least one element belonging to Group VA and Group VIA of the periodic table, the doping amount of the element M in the Si-containing particles being 0.1 at% to 5 at%, and the weight ratio of the graphite particles to the Si-containing particles being 9:1 to 4:6.

[0118] Item 2: The secondary battery according to Item 1, wherein the Si content of the Si-containing particles is 30 wt % to 75 wt % when the total weight of the Si-containing particles is 100 wt %.

[0119] Item 3: The secondary battery according to Item 1 or 2, wherein the Si-containing particles include a porous carbon material and Si nanoparticles, the porous carbon material includes pores, and the Si nanoparticles are arranged in the pores of the porous carbon material.

[0120] Item 4: The secondary battery according to any one of Items 1 to 3, wherein the average particle size D of the graphite particles is 50 It is 10μm~25μm.

[0121] Item 5: The secondary battery according to any one of Items 1 to 4, wherein the negative electrode active material layer further comprises a conductive material, and when the total weight of the negative electrode active material layer is 100 wt %, the content of the conductive material is 0.01 wt % to 1 wt %.

Claims

1. A secondary battery comprising an electrode body having a positive electrode and a negative electrode, The negative electrode comprises a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer contains graphite particles and Si-containing particles as negative electrode active materials, The Si-containing particles are a composite of Si and C. The Si of the Si-containing particles is doped with an element M. The element M is at least one element belonging to Group VA and Group VIA of the periodic table, The doping amount of the element M in the Si-containing particles is 0.1 at% to 5 at%, The weight ratio of the graphite particles to the Si-containing particles is 9:1 to 4:

6.

2. The secondary battery according to claim 1, wherein When the total weight of the Si-containing particles is set to 100 wt %, the Si content of the Si-containing particles is 30 wt % to 75 wt %.

3. The secondary battery according to claim 1 or 2, wherein: The Si-containing particles include a porous carbon material and Si nanoparticles. The porous carbon material includes pores. The Si nanoparticles are arranged in the pores of the porous carbon material.

4. The secondary battery according to claim 1 or 2, wherein: The average particle size D of the graphite particles 50 It is 10μm~25μm.

5. The secondary battery according to claim 1 or 2, wherein: The negative electrode active material layer further comprises a conductive material, When the total weight of the negative electrode active material layer is 100 wt %, the content of the conductive material is 0.01 wt % to 1 wt %.