Aluminum alloy brazing sheet
By using internal brazing and leather layers with high concentrations of Mg and Bi in aluminum alloy brazed sheets, the problem of poor brazing properties in inactive atmosphere is solved, and uniform damage and brazing properties of the oxide film are achieved. promote.
Patent Information
- Application Number
- CN202380028975.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-02-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing aluminum alloy brazing technology is difficult to achieve excellent brazing properties in an inactive atmosphere, especially when flux is not used, there are uneven growth of the oxide film, insufficient fill angle and reduced brazing properties. question.
The core material formed of pure aluminum or aluminum alloy is coated with an outer side of the inner brazing material and leather layer with a specified amount of Mg and Bi. By controlling the average concentration of Mg and Bi in the thickness direction, the internal brazing material and leather layer are ensured. The Mg concentration is greater than 0.50% and the Bi concentration is greater than 0.050% to achieve uniform damage to the oxide film and improve brazing properties.
In an inactive gas atmosphere without flux, excellent brazing properties of aluminum alloy brazed sheets are achieved, ensuring uniformity of fill angles and effectiveness of brazing process.
Smart Images

Figure BDA0005051522040000301 
Figure BDA0005051522040000311 
Figure HDA0005051522050000011
Abstract
Description
Technical Field
[0001] The present invention relates to an aluminum alloy brazing sheet for brazing in an inert gas atmosphere without using a flux. Background Art
[0002] In aluminum heat exchangers and mechanical parts, brazing technology that can simultaneously join multiple joints is widely used. Since aluminum is very easy to oxidize, it is quickly covered with a dense oxide film. Therefore, although it has excellent corrosion resistance, it is difficult to join. Therefore, in aluminum brazing, it is important to inhibit the growth and destroy the surface oxide film. Generally speaking, there are two methods: heating in a vacuum without using a flux and using a flux in a nitrogen furnace. Both methods have been put into practical use.
[0003] The method of heating in vacuum without flux is to use a brazing filler metal formed of an Al-Si-Mg alloy, prevent the growth of an oxide film caused by Al and Mg by heating in a vacuum, and when the brazing filler metal melts, the oxide film on the surface of the material is destroyed due to the evaporation of Mg, thereby achieving brazing. However, this method has the disadvantage of requiring expensive vacuum heating equipment. In addition, since the evaporated Mg will adhere to the furnace, there is also the problem of high maintenance costs for removing the attached Mg.
[0004] On the other hand, in the method of using flux in a nitrogen furnace, a brazing filler metal formed of an Al-Si alloy and a flux formed of an Al-KF alloy are used. Even in a nitrogen atmosphere where the oxygen concentration is higher than that of a vacuum, the molten flux can prevent the growth of an oxide film on the surface of the brazing filler metal and strongly destroy the oxide film, thereby achieving brazing. Although this method does not require expensive vacuum heating equipment, there are problems such as the cost of the flux and the cost of the process of applying the flux. In addition, if the flux is scattered into the working environment due to evaporation when applied to the heat exchanger or during the brazing process, there are concerns about safety, hygiene and environmental issues.
[0005] Therefore, there is an increasing demand for bonding in an inert gas atmosphere without using a flux.
[0006] To meet such a demand, for example, Patent Document 1 proposes brazing of a close-fitting portion by containing Mg and Bi in the brazing material and treating it with an inorganic acid. Materials containing Mg in the brazing material cannot be brazed because MgO is formed during the heat treatment process in the material manufacturing process, but brazing can be achieved by removing the MgO through an inorganic acid treatment.
[0007] In addition, Patent Document 2 proposes to achieve brazing by controlling the Mg in the brazing filler metal and diffusing the Mg contained in the core material during the brazing process. Since there is no Mg in the brazing filler metal, it is advantageous in that the formation of MgO during the material manufacturing process and the brazing temperature rise process can be prevented.
[0008] On the other hand, Patent Document 3 proposes that by coating an intermediate layer having a high Mg concentration between the brazing filler metal and the core material, the amount of Mg supplied to the brazing filler metal can be increased without adding Mg to the brazing filler metal, thereby effectively destroying the oxide film to a certain extent.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 8-354934
[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 2014-037576
[0013] Patent Document 3: WO2016 / 056306 Summary of the invention
[0014] Problem that the invention aims to solve
[0015] However, in Reference 1, since MgO also grows during the brazing temperature rise process, the material surface is covered with a thick oxide film. Therefore, there is a problem that sufficient fillet cannot be formed in practical joints with large gaps.
[0016] In addition, in Reference 2, due to limitations such as formability, the amount of Mg that can be added to the core material is limited, so in order to diffuse the Mg in the core material into the oxide film, high-temperature and long-term brazing heating is required. Therefore, in a practical brazing atmosphere, high-temperature and long-term brazing promotes the oxidation of aluminum itself, and the oxide film grows thicker, so there is a problem of significantly reduced brazing properties.
[0017] In addition, Comparative Document 3 does not solve the problem of uneven destruction of the oxide film and does not reach a practical level.
[0018] Therefore, an object of the present invention is to provide an aluminum alloy brazing sheet having excellent brazing properties in brazing in an inert gas atmosphere without using a flux.
[0019] Solutions for solving problems
[0020] The inventors of the present invention have repeatedly conducted in-depth studies to solve the above-mentioned problems, and as a result, found that: an aluminum alloy brazing sheet in which a skin layer (skin material 1) having a Mg and Bi content below a specified amount is provided on the outside of a brazing material (internal brazing material 1) containing specified amounts of Mg and Bi, and in which the average Mg concentration and the average Bi concentration in the thickness direction of the internal brazing material 1 and the skin material 1 are set to a specified range, has excellent brazing properties in brazing in an inactive gas atmosphere without using a flux, thereby completing the present invention.
[0021] That is, the present invention (1) provides an aluminum alloy brazing sheet, characterized in that it has a core material formed of pure aluminum or an aluminum alloy, and an internal brazing filler metal 1 and a skin material 1 coated on at least one surface of the core material in the order of skin material 1 / internal brazing filler metal 1 / core material, and is used for brazing in an inert gas atmosphere without using a flux,
[0022] The internal brazing filler metal 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and inevitable impurities.
[0023] The skin material 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the remainder being aluminum and unavoidable impurities.
[0024] The average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.50 mass %, and the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.050 mass %.
[0025] In addition, the present invention (2) provides an aluminum alloy brazing sheet according to (1), characterized in that it further comprises a sacrificial anode material A coated on the other surface of the core material in the order of skin material 1 / internal brazing material 1 / core material / sacrificial anode material A,
[0026] The sacrificial anode material A is formed by an aluminum alloy containing any one or more of less than 5.00 mass% Si, less than 1.50 mass% Fe, less than 2.00 mass% Cu, less than 2.00 mass% Mn, less than 3.00 mass% Mg, less than 6.00 mass% Zn, less than 0.30 mass% Cr, less than 0.30 mass% Ti, and less than 0.30 mass% Zr, with the remainder being aluminum and unavoidable impurities.
[0027] In addition, the present invention (3) provides an aluminum alloy brazing sheet according to (1), characterized in that it further comprises an outer surface brazing filler metal coated on the other surface of the core material in the order of skin material 1 / internal brazing filler metal 1 / core material / outer surface brazing filler metal,
[0028] The outer surface brazing filler metal is formed by an aluminum alloy containing 6.00 to 13.00 mass % Si, and also containing any one or more of less than 1.00 mass % Fe, less than 2.00 mass % Cu, less than 2.00 mass % Mn, less than 4.50 mass % Mg, less than 6.00 mass % Zn, less than 0.50 mass % Bi, less than 0.30 mass % Cr, less than 0.30 mass % Ti, and less than 0.30 mass % Zr, with the balance being aluminum and unavoidable impurities.
[0029] In addition, the present invention (4) provides an aluminum alloy brazing sheet according to (2), characterized in that it also has an outer surface brazing filler metal coated on the surface of the sacrificial anode material A on the opposite side of the core material in the order of skin material 1 / internal brazing filler metal 1 / core material / sacrificial anode material A / outer surface brazing filler metal,
[0030] The outer surface brazing filler metal 1 is formed by an aluminum alloy containing 6.00 to 13.00 mass % Si, and also containing any one or more of less than 1.00 mass % Fe, less than 2.00 mass % Cu, less than 2.00 mass % Mn, less than 4.50 mass % Mg, less than 6.00 mass % Zn, less than 0.50 mass % Bi, less than 0.30 mass % Cr, less than 0.30 mass % Ti, and less than 0.30 mass % Zr, with the remainder being aluminum and unavoidable impurities.
[0031] In addition, the present invention (5) provides an aluminum alloy brazing sheet according to (2), characterized in that it also has an internal brazing filler metal 2 and a skin material 2 coated on the surface of the sacrificial anode material A on the opposite side of the core material in the order of skin material 1 / internal brazing filler metal 1 / core material / sacrificial anode material A / internal brazing filler metal 2 / skin material 2,
[0032] The internal brazing filler metal 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and unavoidable impurities.
[0033] The skin material 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the balance being aluminum and inevitable impurities.
[0034] In addition, the present invention (6) provides an aluminum alloy brazing sheet according to (1), characterized in that it further comprises an internal brazing filler metal 2 and a skin material 2 coated on the other surface of the core material in the order of skin material 1 / internal brazing filler metal 1 / core material / internal brazing filler metal 2 / skin material 2,
[0035] The internal brazing filler metal 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and unavoidable impurities.
[0036] The skin material 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the balance being aluminum and inevitable impurities.
[0037] In addition, the present invention (7) provides an aluminum alloy brazing sheet, characterized in that it has a core material formed of pure aluminum or an aluminum alloy, and a sacrificial anode material B1, an internal brazing material 1 and a skin material 1 coated on at least one surface of the core material in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material, and is used for brazing in an inert gas atmosphere without using a flux.
[0038] The internal brazing filler metal 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and 4.50 mass % or less of Mg, and 0.010 to 0.50 mass % or less of Bi, with the remainder being aluminum and unavoidable impurities.
[0039] The skin material 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the remainder being aluminum and unavoidable impurities.
[0040] The sacrificial anode material B1 contains any one or more of 5.00 mass % or less of Si, 1.50 mass % or less of Fe, 2.00 mass % or less of Cu, 2.00 mass % or less of Mn, 3.00 mass % or less of Mg, 6.00 mass % or less of Zn, 0.30 mass % or less of Cr, 0.30 mass % or less of Ti, and 0.30 mass % or less of Zr, and the balance is aluminum and unavoidable impurities.
[0041] The average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.50 mass %, and the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.050 mass %.
[0042] In addition, the present invention (8) provides an aluminum alloy brazing sheet according to (7), characterized in that it also has a sacrificial anode material B2 coated on the other surface of the core material in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / sacrificial anode material B2,
[0043] The sacrificial anode material B2 is an aluminum alloy containing any one or more of less than 5.00 mass% Si, less than 1.50 mass% Fe, less than 2.00 mass% Cu, less than 2.00 mass% Mn, less than 3.00 mass% Mg, less than 6.00 mass% Zn, less than 0.30 mass% Cr, less than 0.30 mass% Ti, and less than 0.30 mass% Zr, with the balance being aluminum and unavoidable impurities.
[0044] In addition, the present invention (9) provides an aluminum alloy brazing sheet according to (7), characterized in that it also has an outer surface brazing filler metal coated on the other surface of the core material in the order of skin material 1 / internal brazing filler metal 1 / sacrificial anode material B1 / core material / outer surface brazing filler metal,
[0045] The outer surface brazing filler metal is an aluminum alloy containing 6.00 to 13.00 mass % Si, and also containing any one or more of less than 1.00 mass % Fe, less than 2.00 mass % Cu, less than 2.00 mass % Mn, less than 4.50 mass % Mg, less than 6.00 mass % Zn, less than 0.50 mass % Bi, less than 0.30 mass % Cr, less than 0.30 mass % Ti, and less than 0.30 mass % Zr, with the balance being aluminum and unavoidable impurities.
[0046] In addition, the present invention (10) provides an aluminum alloy brazing sheet according to (8), characterized in that it also has an outer surface brazing filler metal coated on the surface of the sacrificial anode material 2 on the opposite side of the core material in the order of skin material 1 / internal brazing filler metal 1 / sacrificial anode material B1 / core material / sacrificial anode material B2 / outer surface brazing filler metal,
[0047] The outer surface brazing filler metal is an aluminum alloy containing 6.00 to 13.00 mass % Si, and also containing any one or more of less than 1.00 mass % Fe, less than 2.00 mass % Cu, less than 2.00 mass % Mn, less than 4.50 mass % Mg, less than 6.00 mass % Zn, less than 0.50 mass % Bi, less than 0.30 mass % Cr, less than 0.30 mass % Ti, and less than 0.30 mass % Zr, with the balance being aluminum and unavoidable impurities.
[0048] In addition, the present invention (11) provides an aluminum alloy brazing sheet according to (8), characterized in that it also has an internal brazing filler metal 2 and a skin material 2 coated on the surface of the sacrificial anode material 2 on the opposite side of the core material in the order of skin material 1 / internal brazing filler metal 1 / sacrificial anode material B1 / core material / sacrificial anode material B2 / internal brazing filler metal 2 / skin material 2,
[0049] The internal brazing filler metal 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and unavoidable impurities.
[0050] The skin material 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the balance being aluminum and inevitable impurities.
[0051] In addition, the present invention (12) provides an aluminum alloy brazing sheet according to (7), characterized in that it also has an internal brazing filler metal 2 and a skin material 2 coated on the other surface of the core material in the order of skin material 1 / internal brazing filler metal 1 / sacrificial anode material B1 / core material / internal brazing filler metal 2 / skin material 2,
[0052] The internal brazing filler metal 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and unavoidable impurities.
[0053] The skin material 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the balance being aluminum and inevitable impurities.
[0054] In addition, the present invention (13) provides an aluminum alloy hard brazing sheet according to any one of (1) to (12), characterized in that the core material is formed by the following aluminum alloy, which contains any one or more of 1.50 mass% Si, 1.50 mass% Fe, 2.00 mass% Cu, 2.00 mass% Mn, 3.00 mass% Mg, 3.00 mass% Zn, 0.50 mass% Bi, 0.30 mass% Cr, 0.30 mass% Ti, and 0.30 mass% Zr, and the balance is aluminum and unavoidable impurities.
[0055] In addition, the present invention (14) provides an aluminum alloy hard brazing sheet according to any one of (1) to (13), characterized in that the internal brazing material 1 or the internal brazing material 2 also contains any one or more of 1.00 mass% of Fe, 2.00 mass% of Cu, 2.00 mass% of Mn, 6.00 mass% of Zn, 0.30 mass% of Cr, 0.30 mass% of Ti, and 0.30 mass% of Zr.
[0056] In addition, the present invention (15) provides an aluminum alloy hard brazing sheet according to any one of (1) to (14), characterized in that the skin material 1 or the skin material 2 also contains any one or more of 1.00 mass% of Fe, 2.00 mass% of Cu, 2.00 mass% of Mn, 6.00 mass% of Zn, 0.30 mass% of Cr, 0.30 mass% of Ti, and 0.30 mass% of Zr.
[0057] In addition, the present invention (16) provides the aluminum alloy brazing sheet according to any one of (1) to (15), characterized in that the thickness of the skin material 1 or the skin material 2 is 5.0 μm or more.
[0058] In addition, the present invention (17) provides the aluminum alloy brazing sheet according to any one of (1) to (16), characterized in that the thickness of the internal brazing filler metal 1 or the internal brazing filler metal 2 is 15.0 μm or more.
[0059] Effects of the Invention
[0060] According to the present invention, it is possible to provide an aluminum alloy brazing sheet having excellent brazing properties in brazing in an inert gas atmosphere without using a flux. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 It is a figure which shows the test product of the opening overlap test.
[0062] Figure 2 Schematic diagram of an X-ray CT image obtained by X-ray CT of a fillet shape. DETAILED DESCRIPTION
[0063] The aluminum alloy brazing sheet of the first embodiment of the present invention is characterized in that it has a core material formed of pure aluminum or an aluminum alloy, and an internal brazing filler metal 1 and a skin material 1 coated on at least one surface of the core material in the order of skin material 1 / internal brazing filler metal 1 / core material, and is used for brazing in an inert gas atmosphere without using a flux.
[0064] The internal brazing filler metal 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and inevitable impurities.
[0065] The skin material 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the remainder being aluminum and unavoidable impurities.
[0066] The average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.50 mass %, and the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.050 mass %.
[0067] In addition, the aluminum alloy brazing sheet of the second embodiment of the present invention is characterized in that it has a core material formed of pure aluminum or an aluminum alloy, and a sacrificial anode material B1, an internal brazing material 1, and a skin material 1 coated on at least one surface of the core material in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material, and is used for brazing in an inert gas atmosphere without using a flux.
[0068] The internal brazing filler metal 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and 4.50 mass % or less of Mg, and 0.010 to 0.50 mass % or less of Bi, with the remainder being aluminum and unavoidable impurities.
[0069] The skin material 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the remainder being aluminum and unavoidable impurities.
[0070] The sacrificial anode material B1 contains any one or more of 5.00 mass % or less of Si, 1.50 mass % or less of Fe, 2.00 mass % or less of Cu, 2.00 mass % or less of Mn, 3.00 mass % or less of Mg, 6.00 mass % or less of Zn, 0.30 mass % or less of Cr, 0.30 mass % or less of Ti, and 0.30 mass % or less of Zr, and the balance is aluminum and unavoidable impurities.
[0071] The average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.50 mass %, and the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.050 mass %.
[0072] The aluminum alloy brazing sheet of the first embodiment of the present invention and the aluminum alloy brazing sheet of the second embodiment of the present invention are brazing sheets that are formed into the shape of a component part of a heat exchanger in the manufacture of an aluminum alloy heat exchanger and brazed by brazing heating in an inactive gas atmosphere without using a flux, that is, aluminum alloy brazing sheets for manufacturing aluminum alloy heat exchangers, and are aluminum alloy brazing sheets for manufacturing aluminum alloy heat exchangers by brazing in an inactive gas atmosphere without using a flux.
[0073] The aluminum alloy brazing sheet of the first embodiment of the present invention has an internal brazing filler metal 1 and a skin material 1 stacked and coated in the order of skin material 1 / internal brazing filler metal 1 / core material on at least one surface of the core material. That is, the aluminum alloy brazing sheet of the first embodiment of the present invention has at least a skin material 1 as the outermost layer on one surface side of the core material, and an internal brazing filler metal 1 on an inner side of the skin material 1. In addition, the aluminum alloy brazing sheet of the first embodiment of the present invention may not be coated with anything on the other surface of the core material, that is, the surface on the opposite side to the side coated with the internal brazing filler metal 1 and the skin material 1, or may be coated with one or more coating materials. As examples of the form of the aluminum alloy hard soldering sheet of the first mode of the present invention, there can be listed a three-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / core material, a four-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / core material / sacrificial anode material A, a four-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / core material / outer surface brazing material, a five-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / core material / sacrificial anode material A / outer surface brazing material, a five-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / core material / internal brazing material 2 / skin material 2, and a six-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / core material / sacrificial anode material A / internal brazing material 2 / skin material 2. It should be noted that, in the case where the aluminum alloy hard brazing sheet of the first mode of the present invention has internal brazing material 2 and skin material 2 in addition to internal brazing material 1 and skin material 1, the internal brazing material 1 and the internal brazing material 2 can have the same chemical composition or different chemical compositions, and the skin material 1 and the skin material 2 can have the same chemical composition or different chemical compositions.
[0074] The aluminum alloy brazing sheet of the second embodiment of the present invention has a sacrificial anode material B1, an internal brazing filler metal 1, and a skin material 1 stacked and coated in the order of skin material 1 / internal brazing filler metal 1 / sacrificial anode material B1 / core material on at least one surface of the core material. That is, the aluminum alloy brazing sheet of the second embodiment of the present invention has at least a skin material 1 as the outermost layer on one surface side of the core material, an internal brazing filler metal 1 on one inner side of the skin material 1, and a sacrificial anode material B1 on one inner side of the internal brazing filler metal 1. In addition, the aluminum alloy brazing sheet of the second embodiment of the present invention may not be coated with anything on the other surface of the core material, that is, the surface on the opposite side to the side coated with the sacrificial anode material B1, the internal brazing filler metal 1, and the skin material 1, or may be coated with one or more coating materials. As examples of the form of the aluminum alloy hard soldering sheet of the second mode of the present invention, there can be listed a 4-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material, a 5-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / sacrificial anode material B2, a 5-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / outer surface brazing material, a 6-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / sacrificial anode material B2 / outer surface brazing material, a 6-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / internal brazing material 2 / skin material 2, and a 7-layer material stacked and coated in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / sacrificial anode material B2 / internal brazing material 2 / skin material 2. It should be noted that, when the aluminum alloy brazing sheet of the second embodiment of the present invention has a sacrificial anode material B2 in addition to the sacrificial anode material B1, the sacrificial anode material B1 and the sacrificial anode material B2 may have the same chemical composition or different chemical compositions. In addition, when the aluminum alloy brazing sheet of the second embodiment of the present invention has an internal brazing material 2 and a skin material 2 in addition to the internal brazing material 1 and the skin material 1, the internal brazing material 1 and the internal brazing material 2 may have the same chemical composition or different chemical compositions, and the skin material 1 and the skin material 2 may have the same chemical composition or different chemical compositions.
[0075] The core material involved in the aluminum alloy brazing sheet of the first embodiment of the present invention is the same as the core material involved in the aluminum alloy brazing sheet of the second embodiment of the present invention. In addition, the skin material 1 and the skin material 2 involved in the aluminum alloy brazing sheet of the first embodiment of the present invention are the same as the skin material 1 and the skin material 2 involved in the aluminum alloy brazing sheet of the second embodiment of the present invention. The internal brazing filler metal 1 involved in the aluminum alloy brazing sheet of the first embodiment of the present invention is the same as the internal brazing filler metal 1 involved in the aluminum alloy brazing sheet of the second embodiment of the present invention. The sacrificial anode material A involved in the aluminum alloy brazing sheet of the first embodiment of the present invention is the same as the sacrificial anode material B1 and the sacrificial anode material B2 involved in the aluminum alloy brazing sheet of the second embodiment of the present invention. The outer surface brazing filler metal involved in the aluminum alloy brazing sheet of the first embodiment of the present invention is the same as the outer surface brazing filler metal involved in the aluminum alloy brazing sheet of the second embodiment of the present invention. The internal brazing filler metal 2 involved in the aluminum alloy brazing sheet of the first embodiment of the present invention is the same as the internal brazing filler metal 2 involved in the aluminum alloy brazing sheet of the second embodiment of the present invention.
[0076] The core material according to the aluminum alloy brazing sheet of the first aspect of the present invention and the aluminum alloy brazing sheet of the second aspect of the present invention is made of pure aluminum or an aluminum alloy.
[0077] When the core material is made of pure aluminum, the Al purity of the pure aluminum is not particularly limited, but is preferably 99.0 mass % or more, and particularly preferably 99.5 mass % or more. Examples of the pure aluminum material include A1100, A1050, and A1080.
[0078] In the case where the core material is formed of an aluminum alloy, the composition of the aluminum alloy forming the core material is not particularly limited as long as it can be used as a core material of an aluminum alloy brazing sheet for manufacturing an aluminum alloy heat exchanger. As the core material, a core material formed of an aluminum alloy is preferably formed, wherein the aluminum alloy contains any one or more of 1.50 mass % Si, 1.50 mass % Fe, 2.00 mass % Cu, 2.00 mass % Mn, 3.00 mass % Zn, 0.30 mass % Cr, 0.30 mass % Ti, and 0.30 mass % Zr, and the balance is aluminum and unavoidable impurities.
[0079] In the core material of the aluminum alloy, Si contributes to the improvement of strength. When the core material contains Si, the Si content in the core material is 1.50 mass % or less, preferably 0.10 to 1.00 mass %. When the Si content in the core material is within the above range, the strength of the core material becomes high. On the other hand, when the Si content in the core material exceeds the above range, the melting point becomes too low, local melting occurs during brazing, the core material is deformed, and the corrosion resistance is reduced.
[0080] Fe contributes to improving strength. When the core material contains Fe, the Fe content in the core material is less than 1.50 mass %, preferably 0.10 to 0.70 mass %. When the Fe content in the core material is within the above range, the strength of the core material becomes higher. On the other hand, when the Fe content in the core material exceeds the above range, the corrosion resistance decreases and giant precipitates are easily generated.
[0081] Cu contributes to strength improvement and potential adjustment. When the core material contains Cu, the Cu content in the core material is 2.00 mass % or less, preferably 0.10 to 1.00 mass %. When the Cu content in the core material is within the above range, the strength of the core material becomes high. On the other hand, when the Cu content in the core material exceeds the above range, intergranular corrosion is likely to occur, and the melting point becomes too low.
[0082] Mn contributes to strength improvement and potential adjustment. When the core material contains Mn, the Mn content in the core material is less than 2.00 mass %, preferably 0.30 to 1.80 mass %. By having the Mn content in the core material within the above range, the strength of the core material becomes higher and a potential adjustment effect can be obtained. When the Mn content in the core material exceeds the above range, cracks are easily generated during material rolling.
[0083] Zn contributes to potential adjustment. When the core material contains Zn, the Zn content in the core material is 3.00 mass % or less, preferably 0.50 to 3.00 mass %. By keeping the Zn content in the core material within the above range, a potential adjustment effect can be obtained. On the other hand, when the Zn content in the core material exceeds the above range, the natural electrode potential becomes too low and the corrosion resistance decreases.
[0084] Cr improves strength by solid solution strengthening, and also precipitates fine Al-Cr compounds, which contribute to grain coarsening after brazing. The Cr content in the core material is 0.30% by mass or less, preferably 0.10 to 0.20% by mass. When the Cr content in the core material is within the above range, the strength of the core material increases. On the other hand, when the Cr content in the core material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0085] Ti improves strength by solid solution strengthening. In addition, by forming a layer with high potential and a layer with low potential in the core material in a layered distribution, the corrosion morphology changes from pitting to layered, which has the effect of improving corrosion resistance. The Ti content in the core material is less than 0.30 mass%, preferably 0.10-0.20 mass%. When the Ti content in the core material is within the above range, the strength of the core material becomes higher and the corrosion resistance becomes higher. On the other hand, when the Ti content in the core material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0086] Zr improves strength by solid solution strengthening, and also precipitates fine Al-Zr compounds, which have an effect on grain coarsening after brazing. The Zr content in the core material is 0.30% by mass or less, preferably 0.10 to 0.20% by mass. When the Zr content in the core material is within the above range, the strength of the core material becomes higher, and the effect of grain coarsening after brazing can be obtained. On the other hand, when the Zr content in the core material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0087] The core material may contain Mg. In the core material of the aluminum alloy, Mg diffuses into the internal brazing material 1 or the skin material 1 during the brazing heating process, promotes the destruction of the oxide film on the surface of the material, and helps to improve the brazing performance. In the case where the core material contains Mg, the Mg content in the core material is less than 3.00 mass%, preferably 0.30 to 1.80 mass%. By having the Mg content in the core material within the above range, it is easy to obtain the effect of improving the brazing performance. On the other hand, when the Mg content in the core material exceeds the above range, cracks are likely to occur during the rolling of the material.
[0088] The core material may contain Bi. In the aluminum alloy forming the core material, when Bi melts the internal brazing material 1 or the skin material 1 during the brazing heating process, causing a part of the core material to melt, it plays a role in suppressing the reduction of the Bi concentration of the internal brazing material 1 or the skin material 1, and plays a role in promoting the destruction of the oxide film brought about by Mg. In the case where the core material contains Bi, the Bi content in the core material is less than 0.50 mass%, preferably 0.10 to 0.40 mass%. By the Bi content in the core material being within the above range, the effect of promoting the destruction of the oxide film brought about by Mg can be obtained. On the other hand, when the above range is exceeded, cracks are likely to occur during material manufacturing, and the manufacture of the brazing sheet becomes difficult.
[0089] The core material may contain 0.050 mass % or less of Ag, B, Be, Ca, Cd, Co, Ga, Ge, Hg, In, Li, Mo, Na, Ni, P, Pb, Sb, Sn, Sr, V, and Y as unavoidable impurities.
[0090] The internal brazing filler metal 1 and the internal brazing filler metal 2 involved in the aluminum alloy brazing sheet of the first embodiment of the present invention and the aluminum alloy brazing sheet of the second embodiment of the present invention are formed by the following aluminum alloy, which contains 6.00 to 13.00 mass% Si, more than 0.50 mass% and less than 4.50 mass% Mg, and 0.010 to 0.50 mass% Bi, and the balance is aluminum and inevitable impurities.
[0091] The internal brazing filler metal 1 and the internal brazing filler metal 2 contain Si. In the brazing filler metal of the aluminum alloy, Si contributes to the brazing weldability. The Si content in the internal brazing filler metal 1 and the internal brazing filler metal 2 is 6.00 to 13.00 mass %. Sufficient brazing weldability can be obtained by setting the Si content in the internal brazing filler metal 1 and the internal brazing filler metal 2 within the above range. When the Si content in the internal brazing filler metal 1 and the internal brazing filler metal 2 is lower than the above range, the weldability is poor. In addition, when the Si content exceeds the above range, cracks are easily generated during material manufacturing, and the manufacture of the brazing sheet becomes difficult.
[0092] The internal brazing filler metal 1 and the internal brazing filler metal 2 contain Mg. The Mg content in the internal brazing filler metal 1 and the internal brazing filler metal 2 is greater than 0.50 mass % and is less than 4.50 mass %, preferably 0.60 to 4.00 mass %. When the Mg content in the internal brazing filler metal 1 and the internal brazing filler metal 2 is within the above range, sufficient brazing adhesion can be obtained. When the Mg content in the internal brazing filler metal 1 and the internal brazing filler metal 2 is less than the above range, the oxide film destruction effect becomes insufficient. In addition, when the above range is exceeded, cracks are easily generated during material manufacturing, and the manufacture of the brazing sheet becomes difficult.
[0093] The internal brazing filler metals 1 and 2 contain Bi. The Bi content in the internal brazing filler metals 1 and 2 is 0.010 to 0.50 mass%, preferably 0.020 to 0.45 mass%. When the Bi content in the internal brazing filler metals 1 and 2 is within the above range, sufficient brazing adhesion can be obtained. When the Bi content in the internal brazing filler metals 1 and 2 is lower than the above range, the effect of promoting the destruction of the oxide film by Mg becomes insufficient. In addition, when the Bi content exceeds the above range, cracks are easily generated during material manufacturing, and the manufacture of the brazing sheet becomes difficult.
[0094] The internal brazing filler metal 1 and the internal brazing filler metal 2 may contain any one or more of Na, Sr and Sb. In the aluminum alloy forming the brazing filler metal, Na, Sr and Sb play the role of refining Si particles in the brazing filler metal and improving the fluidity of the brazing filler metal. When the internal brazing filler metal 1 and the internal brazing filler metal 2 contain Na, the Na content is 0.050 mass % or less, preferably 0.005 to 0.040 mass %. When the internal brazing filler metal 1 and the internal brazing filler metal 2 contain Sr, the Sr content is 0.050 mass % or less, preferably 0.005 to 0.040 mass %. When the internal brazing filler metal 1 and the internal brazing filler metal 2 contain Sb, the Sb content is 0.050 mass % or less, preferably 0.005 to 0.040 mass %. By keeping the contents of Na, Sr and Sb in the internal brazing filler metal 1 and the internal brazing filler metal 2 within the above range, the refining effect of Si particles can be obtained. On the other hand, when the contents of Na, Sr, and Sb in the internal brazing filler metals 1 and 2 exceed the above ranges, the effects are saturated and this is not economical.
[0095] The internal brazing filler metals 1 and 2 may contain any one or two of Zn and Cu. In the aluminum alloy forming the internal brazing filler metals 1 and 2, Zn and Cu lower the melting points of the brazing filler metals 1 and 2, thereby achieving brazing at a lower temperature than the conventional brazing temperature of 600°C.
[0096] When the internal brazing filler metals 1 and 2 contain Zn, the Zn content is preferably 6.00 mass% or less, particularly preferably 1.00 to 5.50 mass%, and further preferably 3.00 to 5.00 mass%, based on the consideration that the effect of lowering the melting point of the brazing filler metals is more easily obtained. On the other hand, when the Zn content in the internal brazing filler metals 1 and 2 exceeds the above range, cracks are generated during the material manufacturing process, and the manufacture of the brazing sheet becomes difficult. In addition, when the internal brazing filler metals 1 and 2 contain Zn, the Zn content in the internal brazing filler metals 1 and 2 is preferably 3.00 mass% or less, based on the consideration that the potential of the brazing filler metals is low, the core material is corroded preferentially, and the core material is easily anti-corroded.
[0097] When the internal brazing filler metals 1 and 2 contain Cu, the Cu content is 2.00 mass % or less, preferably 0.50 to 2.00 mass %, and particularly preferably 1.00 to 2.00 mass %. When the Cu content of the internal brazing filler metals 1 and 2 is within the above range, the effect of lowering the melting point of the brazing filler metals is improved. On the other hand, when the Cu content of the internal brazing filler metals 1 and 2 exceeds the above range, cracks are generated during the material manufacturing process, and the manufacture of the brazing sheet becomes difficult.
[0098] The internal brazing filler metal 1 and the internal brazing filler metal 2 may contain Fe. In the aluminum alloy forming the brazing filler metal, Fe precipitates a coarse compound of the Al-Fe system, which has an effect on the grain refinement of the residual brazing filler metal after brazing. When the internal brazing filler metal 1 and the internal brazing filler metal 2 contain Fe, the Fe content is 1.00 mass % or less, preferably 0.10 to 0.50 mass %. By setting the Fe content in the internal brazing filler metal 1 and the internal brazing filler metal 2 to the above range, the effect of grain refinement can be easily obtained. On the other hand, when the Fe content of the internal brazing filler metal 1 and the internal brazing filler metal 2 exceeds the above range, huge intermetallic compounds are easily formed during casting, and the plastic workability is reduced.
[0099] Internal brazing filler metal 1 and internal brazing filler metal 2 may contain any one or more of Mn, Cr, Ti and Zr. In the aluminum alloy forming the brazing filler metal, Mn, Cr, Ti and Zr precipitate fine compounds of Al-Mn series, Al-Cr series, Al-Ti series and Al-Zr series, respectively, and play a role in coarsening the grains of the residual brazing filler metal after brazing.
[0100] When the internal brazing filler metals 1 and 2 contain Mn, the Mn content is 2.00 mass % or less, preferably 0.10 to 0.60 mass %. When the Mn content in the internal brazing filler metals 1 and 2 is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Mn content in the internal brazing filler metals 1 and 2 exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0101] When the internal brazing filler metals 1 and 2 contain Cr, the Cr content is 0.30 mass % or less, preferably 0.10 to 0.20 mass %. When the Cr content in the internal brazing filler metals 1 and 2 is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Cr content in the internal brazing filler metals 1 and 2 exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0102] When the internal brazing filler metals 1 and 2 contain Ti, the Ti content is 0.30 mass % or less, preferably 0.10 to 0.20 mass %. When the Ti content in the internal brazing filler metals 1 and 2 is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Ti content in the internal brazing filler metals 1 and 2 exceeds the above range, a huge intermetallic compound is easily formed during casting, and the plastic workability is reduced.
[0103] When the internal brazing filler metals 1 and 2 contain Zr, the Zr content is 0.30 mass % or less, preferably 0.10 to 0.20 mass %. When the Zr content in the internal brazing filler metals 1 and 2 is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Zr content in the internal brazing filler metals 1 and 2 exceeds the above range, a huge intermetallic compound is easily formed during casting, and the plastic workability is reduced.
[0104] Although the crystal grain size after brazing is adjusted by utilizing the above-mentioned action, the effect of the present invention can be fully obtained as long as it is within the above-mentioned range.
[0105] The internal solder 1 and the internal solder 2 may contain 0.050 mass % or less of Ag, B, Be, Ca, Cd, Co, Ga, Ge, Hg, In, Li, Mo, Ni, P, Pb, Sn, V, and Y as unavoidable impurities.
[0106] The skin material 1 and the skin material 2 involved in the aluminum alloy brazing sheet of the first embodiment of the present invention and the aluminum alloy brazing sheet of the second embodiment of the present invention are formed of an aluminum alloy containing 6.00 to 13.00 mass% Si, a Mg content of less than 0.050 mass%, a Bi content of less than 0.050 mass%, and the balance being aluminum and inevitable impurities.
[0107] Skin material 1 and skin material 2 contain Si. When skin material 1 and skin material 2 are fused with internal brazing filler metal 1 and internal brazing filler metal 2 respectively at the brazing temperature, the Si in skin material 1 and skin material 2 reduces the reduction of the Si content of internal brazing filler metal 1 and internal brazing filler metal 2, and contributes to the brazing weldability. The Si content in skin material 1 and skin material 2 is 6.00 to 13.00% by mass. Sufficient brazing weldability can be obtained by keeping the Si content in skin material 1 and skin material 2 within the above range. On the other hand, when the Si content in skin material 1 and skin material 2 is lower than the above range, the Si content in internal brazing filler metal 1 and internal brazing filler metal 2 is reduced, thereby reducing the brazing weldability. In addition, when the above range is exceeded, cracks are easily generated during material manufacturing, and the manufacture of brazing sheets becomes difficult.
[0108] Skin material 1 and skin material 2 preferably do not contain Mg or have as little Mg as possible. In the aluminum alloy forming skin material 1 and skin material 2, Mg promotes the growth of oxide film during the brazing heating process, which reduces the brazing performance. Therefore, the Mg content in skin material 1 and skin material 2 is limited to less than 0.050 mass% of the unavoidable impurity level. By keeping the Mg content in skin material 1 and skin material 2 within the above range, the brazing performance will not be reduced. On the other hand, when the Mg content in skin material 1 and skin material 2 exceeds the above range, the oxide film on the surface of the material that does not need to be destroyed is destroyed before the brazing material melts during the brazing heating process, and a thick oxide film grows until the brazing material melts. Furthermore, since the thick oxide film contains Mg, it is difficult to produce the reduction and destruction of the oxide film caused by the same Mg, which reduces the brazing performance.
[0109] The skin material 1 and the skin material 2 may contain Bi. The Bi content in the skin material 1 is set so as to satisfy the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 described later. The Bi content in the skin material 1 is limited to, for example, 0.050 mass % or less of the inevitable impurity level. In addition, the Bi content in the skin material 2 is preferably set so as to satisfy the average Bi concentration in the thickness direction of the internal solder 2 and the skin material 2 described later.
[0110] Skin material 1 and skin material 2 may contain any one or more of Na, Sr and Sb. In the aluminum alloy forming skin material 1 and skin material 2, Na, Sr and Sb play the role of miniaturizing Si particles in skin material 1 and skin material 2 and improving the fluidity of solder. When skin material 1 and skin material 2 contain Na, the Na content is 0.050 mass% or less, preferably 0.005-0.040 mass%. When skin material 1 and skin material 2 contain Sr, the Sr content is 0.050 mass% or less, preferably 0.005-0.040 mass%. When skin material 1 and skin material 2 contain Sb, the Sb content is 0.050 mass% or less, preferably 0.005-0.040 mass%. By keeping the contents of Na, Sr and Sb in skin material 1 and skin material 2 within the above range, the miniaturization effect of Si particles can be obtained. On the other hand, when the contents of Na, Sr, and Sb in the skin material 1 and the skin material 2 exceed the above ranges, the effects are saturated and it is not economical.
[0111] Skin material 1 and skin material 2 may contain any one or two of Zn and Cu. In the aluminum alloy forming skin material 1 and skin material 2, Zn and Cu lower the melting point of skin material 1 and skin material 2, and achieve fusion with internal brazing material 1 and internal brazing material 2 at a temperature lower than the conventional brazing temperature of 600°C.
[0112] When the skin material 1 and the skin material 2 contain Zn, the Zn content is preferably 6.00 mass% or less, particularly preferably 1.00 to 5.50 mass%, and further preferably 3.00 to 5.00 mass%, based on the consideration that the effect of lowering the melting point of the skin material 1 and the skin material 2 is more easily obtained. On the other hand, when the Zn content in the skin material 1 and the skin material 2 exceeds the above range, cracks are generated during the material manufacturing process, and the manufacture of the brazing sheet becomes difficult. In addition, when the skin material 1 and the skin material 2 contain Zn, the Zn content in the skin material 1 and the skin material 2 is preferably 3.00 mass% or less, based on the consideration that the potential of the skin material 1 and the skin material 2 is low, and the core material is corroded preferentially, thereby easily obtaining the core material corrosion protection effect.
[0113] When the skin material 1 and the skin material 2 contain Cu, the Cu content is 2.00 mass % or less, preferably 0.50 to 2.00 mass %, and particularly preferably 1.00 to 2.00 mass %. When the Cu content in the skin material 1 and the skin material 2 is within the above range, the effect of lowering the melting point of the skin material 1 and the skin material 2 is improved. On the other hand, when the Cu content in the skin material 1 and the skin material 2 exceeds the above range, cracks are generated during the material manufacturing process, and the manufacture of the brazing sheet becomes difficult.
[0114] Skin material 1 and skin material 2 may contain Fe. In the aluminum alloy forming skin material 1 and skin material 2, Fe precipitates a coarse compound of the Al-Fe system, fuses with the brazing material during brazing, and has an effect on the grain refinement of the residual brazing material after brazing. In the case where skin material 1 and skin material 2 contain Fe, the Fe content is less than 1.00 mass%, preferably 0.10 to 0.50 mass%. By making the Fe content in skin material 1 and skin material 2 within the above range, the effect of grain refinement can be easily obtained. On the other hand, when the Fe content of skin material 1 and skin material 2 exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0115] Skin material 1 and skin material 2 may contain any one or more of Mn, Cr, Ti and Zr. In the aluminum alloy forming skin material 1 and skin material 2, Mn, Cr, Ti and Zr precipitate fine compounds of Al-Mn series, Al-Cr series, Al-Ti series and Al-Zr series, respectively, and play a role in coarsening the grains of the residual brazing material after brazing.
[0116] When the skin material 1 and the skin material 2 contain Mn, the Mn content is 2.00 mass % or less, preferably 0.10 to 0.60 mass %. When the Mn content in the skin material 1 and the skin material 2 is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Mn content in the skin material 1 and the skin material 2 exceeds the above range, a huge intermetallic compound is easily formed during casting, and the plastic workability is reduced.
[0117] When the skin material 1 and the skin material 2 contain Cr, the Cr content is 0.30 mass % or less, preferably 0.10 to 0.20 mass %. When the Cr content in the skin material 1 and the skin material 2 is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Cr content in the skin material 1 and the skin material 2 exceeds the above range, a huge intermetallic compound is easily formed during casting, and the plastic workability is reduced.
[0118] When the skin material 1 and the skin material 2 contain Ti, the Ti content is 0.30 mass % or less, preferably 0.10 to 0.20 mass %. When the Ti content in the skin material 1 and the skin material 2 is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Ti content in the skin material 1 and the skin material 2 exceeds the above range, a huge intermetallic compound is easily formed during casting, and the plastic workability is reduced.
[0119] When the skin material 1 and the skin material 2 contain Zr, the Zr content is 0.30 mass % or less, preferably 0.10 to 0.20 mass %. When the Zr content in the skin material 1 and the skin material 2 is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Zr content in the skin material 1 and the skin material 2 exceeds the above range, a huge intermetallic compound is easily formed during casting, and the plastic workability is reduced.
[0120] Although the crystal grain size after brazing is adjusted by utilizing the above-mentioned action, the effect of the present invention can be fully obtained as long as it is within the above-mentioned range.
[0121] Skin material 1 and skin material 2 may contain 0.050 mass % or less of Ag, B, Be, Ca, Cd, Co, Ga, Ge, Hg, In, Li, Mo, Ni, P, Pb, Sn, V, and Y as unavoidable impurities.
[0122] Moreover, in the first embodiment of the aluminum alloy brazing sheet of the present invention and the second embodiment of the aluminum alloy brazing sheet of the present invention, the average Mg concentration of the internal brazing material 1 and the skin material 1 in the thickness direction is greater than 0.50 mass%, and the average Bi concentration of the internal brazing material 1 and the skin material 1 in the thickness direction is greater than 0.050 mass%.
[0123] Since the Mg added to the brazing material layer has a lower free energy of oxide formation than aluminum, it can reduce and destroy the surface oxide film with aluminum as the main component during the brazing heating process. However, in the two-layer aluminum alloy brazing sheet composed of the brazing material and the core material, since the material with Mg added to the brazing material forms MgO during the heat treatment process in the material manufacturing process, it cannot be brazed, and it is necessary to remove the MgO through pretreatment, etc. On this basis, before the brazing material melts during the brazing heating process, the Mg in the brazing material will also destroy the oxide film on the surface of the material that does not need to be destroyed, and a thick and strong oxide film will grow until the brazing material melts. Furthermore, since the oxide film contains Mg, it is difficult to produce the reduction and destruction of the oxide film caused by the same Mg, and sufficient brazing properties cannot be obtained.
[0124] In addition, in a two-layer aluminum alloy brazing sheet composed of a brazing filler metal and a core material, the material with Mg added to the core material is advantageous in that MgO can be prevented from being formed during the material manufacturing process and the brazing heating process because Mg does not exist in the brazing filler metal. However, due to limitations such as formability, the amount of Mg that can be added to the core material is limited, so high-temperature and long-term brazing heating is required to diffuse the Mg in the core material into the oxide film. In the case of a practical brazing atmosphere, high-temperature and long-term brazing promotes the oxidation of aluminum itself, and the oxide film grows thicker, so the brazing properties are significantly reduced.
[0125] In addition, by coating an intermediate layer with a high Mg concentration between the brazing material and the core material, Mg can be supplied from the intermediate layer without adding Mg to the brazing material, thereby effectively destroying the oxide film to a certain extent. The material has high brazing properties even under relatively short brazing heating. However, in the case of a practical brazing atmosphere, a thick and strong oxide film grows due to oxidation of the aluminum itself, so unless the brazing conditions are suitable for the material, practical brazing properties cannot be obtained.
[0126] On this basis, the destruction of the oxide film by Mg proceeds relatively slowly due to the influence of temperature and time. Therefore, in practical products containing Mg, when a temperature difference occurs in the product during brazing, the fillet formation is uneven due to the generation of parts where the destruction of the oxide film by Mg proceeds quickly and parts where it proceeds slowly. In this case, the molten brazing material flows into the joint where the fillet was previously formed by capillary force, and flows out of the joint where the fillet has not been formed, and even if the oxide film is destroyed thereafter, the fillet cannot be formed. Therefore, in practical products with a large number of joints, fatal non-joining may occur. Therefore, in order to obtain sufficient brazing properties in practical products containing Mg, it is important to perform brazing by uniformly and instantly inducing the destruction of the oxide film caused by Mg.
[0127] In order to destroy the oxide film uniformly and instantly, it is effective to add Mg to the brazing material layer and then coat the surface of the brazing material layer opposite to the core material with a skin material layer that does not contain Mg or has a very low Mg content. That is, before the brazing material heated for brazing melts, the skin material layer located on the outermost surface does not contain Mg, so the oxide film on the surface of the material remains thin, but if the brazing material layer melts, the Mg contained in the brazing material layer can immediately reach the surface of the skin material layer and destroy the oxide film. However, even in the material provided with a skin material layer as described above, since the Mg concentration of the brazing material layer is as low as a few percent, the effect of reducing and destroying the oxide film is slow, and sufficient brazing properties cannot be obtained in practical products. On the other hand, if a large amount of Mg is added to the brazing material, cracks are likely to occur during material manufacturing, and the manufacture of brazing sheets becomes difficult.
[0128] Therefore, the present inventors have conducted intensive studies and found that a method using Bi is effective as a method for increasing the Mg concentration acting on the material surface when the brazing material is melted without increasing the Mg content added to the brazing material layer.
[0129] Bi combines with Mg to form 3 Bi 2 Intermetallic compounds, but Mg 3 Bi 2 The Mg concentration in the compound is extremely high at 85% by mass. 3 Bi 2It acts on the oxide film, which can rapidly intensify the destructive effect of the oxide film and achieve practical brazing performance. 3 Bi 2 In addition, the Mg concentration in the brazing material layer is reduced, and the Mg and Bi concentrations are reduced by melting and mixing the brazing material layer and the skin material layer. 3 Bi 2 It decomposes in the molten brazing material before acting on the oxide film. To this end, the inventors conducted in-depth research on the concentrations of Mg and Bi that can achieve good brazing properties, and found that the desired brazing properties can be obtained by controlling the average value of the concentrations of Mg and Bi added to the brazing material layer and the skin material layer in the thickness direction.
[0130] That is, the average Mg concentration in the thickness direction of the internal brazing filler metal 1 and the skin material 1 is set to a concentration exceeding 0.50 mass %, and the average Bi concentration in the thickness direction of the internal brazing filler metal 1 and the skin material 1 is set to a concentration exceeding 0.050 mass %.
[0131] The average Mg concentration in the thickness direction of the internal brazing filler metal 1 and the skin material 1 is greater than 0.50 mass %, more preferably 0.65 mass % or more, and further preferably 0.80 mass % or more. 3 Bi 2 The stability is increased, and the effect of delaying the decomposition in the molten solder can be fully obtained. It should be noted that the average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 is preferably higher from the viewpoint of brazing properties, and the upper limit concentration is not specified, but is determined by the upper limit of the Mg content of the internal solder 1 recorded separately.
[0132] The average Bi concentration in the thickness direction of the internal brazing material 1 and the skin material 1 is greater than 0.050 mass%, more preferably 0.065 mass% or more, and further preferably 0.080 mass% or more. When the average Bi concentration in the thickness direction of the internal brazing material 1 and the skin material 1 is within the above range, Mg 3 Bi 2 The stability is increased, and the effect of delaying the decomposition in the molten solder can be fully obtained. It should be noted that the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 is preferably higher from the viewpoint of brazing performance, and the upper limit concentration is not specified, but is determined by the upper limit of the Bi content of the internal solder 1 recorded separately.
[0133] It should be noted that in the present invention, the average Mg concentration of the internal solder 1 and the skin material 1 in the thickness direction and the average Bi concentration of the internal solder 1 and the skin material 1 in the thickness direction are denoted by A.1 mass %, the Bi content of the internal brazing material 1 is denoted as B 1 mass %, the Mg content of the leather material 1 is C 1 The Bi content of the leather material 1 is D 1 Mass %, the thickness of the internal brazing material 1 is T 1 (mm), the thickness of the leather material 1 is t 1 (mm), it can be calculated as follows.
[0134] Average Mg concentration in the thickness direction of the internal brazing material 1 and the skin material 1 (%) = (A 1 ×T 1 +C 1 ×t 1 ) / (T 1 +t 1 )
[0135] Average Bi concentration in the thickness direction of the internal brazing material 1 and the skin material 1 (%) = (B 1 ×T 1 +D 1 ×t 1 ) / (T 1 +t 1 )
[0136] The thickness of the internal brazing material 1 is preferably 15.0 μm or more. The thicker the internal brazing material 1, the greater the Mg 3 Bi 2 The greater the absolute amount of the compound, the more the destruction of the oxide film is promoted. Moreover, by making the thickness of the internal solder 1 15.0 μm or more, it is easy to adjust the average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 and the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 to a specified concentration. It should be noted that the upper limit of the thickness of the internal solder 1 is not specified, but the thickness of the internal solder 1 required for practical products is in the range of about 15.0 to 400 μm.
[0137] The thickness of the skin material 1 is preferably greater than 5.0 μm. Since the thicker the skin material 1 is, the more difficult it is for the Mg in the internal solder 1 to diffuse to the surface of the skin material 1, the brazing property is improved. When the thickness of the skin material 1 is greater than 5.0 μm, the Mg in the internal solder 1 is difficult to diffuse to the surface of the skin material 1, and the antioxidant effect of Mg is easily obtained. It should be noted that there is no upper limit to the thickness of the skin material 1, but based on the consideration of the ease of adjusting the average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 and the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1, the thickness of the skin material 1 is preferably less than 120 μm. Therefore, the practical range of the thickness of the skin material 1 is about 5.0 to 120 μm.
[0138] In addition, in the case where the aluminum alloy brazing sheet of the first embodiment of the present invention or the aluminum alloy brazing sheet of the second embodiment of the present invention has an internal brazing material 2 and a skin material 2, it is preferred that the average Mg concentration of the internal brazing material 2 and the skin material 2 in the thickness direction is greater than 0.50 mass%, and the average Bi concentration of the internal brazing material 2 and the skin material 2 in the thickness direction is greater than 0.050 mass%.
[0139] The sacrificial anode material A involved in the first embodiment of the aluminum alloy brazing sheet of the present invention, the sacrificial anode material B1 involved in the second embodiment of the aluminum alloy brazing sheet of the present invention, and the sacrificial anode material B2 involved in the second embodiment of the aluminum alloy brazing sheet of the present invention are formed of the following aluminum alloy, the aluminum alloy contains any one or more of 5.00 mass% Si, 1.50 mass% Fe, 2.00 mass% Cu, 2.00 mass% Mn, 3.00 mass% Mg, 6.00 mass% Zn, 0.30 mass% Cr, 0.30 mass% Ti, and 0.30 mass% Zr, and the balance is aluminum and unavoidable impurities. It should be noted that the sacrificial anode material A, the sacrificial anode material B1, and the sacrificial anode material B2 are hereinafter referred to as "sacrificial anode materials".
[0140] In the sacrificial anode material of aluminum alloy, Si contributes to improving the strength. When the sacrificial anode material contains Si, the Si content in the sacrificial anode material is less than 5.00 mass%, preferably 0.10-1.50 mass%, and particularly preferably 0.10-1.00 mass%. When the Si content in the sacrificial anode material is within the above range, the strength of the sacrificial anode material becomes higher. In addition, the Si content in the sacrificial anode material is 1.50-5.00 mass%, particularly preferably 2.50-4.50 mass%. When the content is in the range of 1.50-5.00 mass%, it becomes a semi-molten state during the brazing heating process, and a trace amount of liquid phase brazing material is supplied, and the brazing property is improved when the sacrificial anode material surface becomes a brazing surface. On the other hand, when the Si content in the sacrificial anode material exceeds the above range, the melting point becomes too low, local melting occurs during brazing, and deformation occurs on the sacrificial anode material.
[0141] Fe contributes to improving strength. When the sacrificial anode material contains Fe, the Fe content in the sacrificial anode material is less than 1.50 mass %, preferably 0.10 to 0.70 mass %. When the Fe content in the sacrificial anode material is within the above range, the strength of the sacrificial anode material becomes higher. On the other hand, when the Fe content in the sacrificial anode material exceeds the above range, the corrosion resistance is reduced and giant precipitates are easily generated.
[0142] Cu contributes to strength improvement and potential adjustment. When the sacrificial anode material contains Cu, the Cu content in the sacrificial anode material is 2.00 mass % or less, preferably 0.10 to 1.00 mass %. When the Cu content in the sacrificial anode material is within the above range, the strength of the sacrificial anode material becomes high. On the other hand, when the Cu content in the sacrificial anode material exceeds the above range, intergranular corrosion is likely to occur, and the melting point becomes too low.
[0143] Mn contributes to strength improvement and potential adjustment. When the sacrificial anode material contains Mn, the Mn content in the sacrificial anode material is 2.00 mass % or less, preferably 0.30 to 1.80 mass %. By keeping the Mn content in the sacrificial anode material within the above range, the strength of the sacrificial anode material increases, and a potential adjustment effect can be obtained. When the Mn content in the sacrificial anode material exceeds the above range, cracks are easily generated during rolling of the material.
[0144] Mg contributes to strength improvement. When the sacrificial anode material contains Mg, the Mg content in the sacrificial anode material is 3.00 mass % or less, preferably 0.30 to 1.80 mass %. By keeping the Mg content in the sacrificial anode material within the above range, it is easy to obtain the effect of improving strength. On the other hand, when the Mg content in the sacrificial anode material exceeds the above range, cracks are easily generated during rolling of the material.
[0145] Zn contributes to potential adjustment. When the sacrificial anode material contains Zn, the Zn content in the sacrificial anode material is 6.00 mass % or less, preferably 3.00 mass % or less. When the Zn content in the sacrificial anode material is within the above range, the sacrificial anti-corrosion effect becomes higher. On the other hand, when the Zn content in the sacrificial anode material exceeds the above range, the potential of the sacrificial anode material may be excessively reduced, accelerating the progress of corrosion.
[0146] Cr improves the strength by solid solution strengthening, and also precipitates fine Al-Cr compounds, which contributes to the coarsening of grains after brazing. The Cr content in the sacrificial anode material is 0.30 mass % or less, preferably 0.10 to 0.20 mass %. When the Cr content in the sacrificial anode material is within the above range, the strength of the sacrificial anode material becomes high. On the other hand, when the Cr content in the sacrificial anode material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0147] Ti improves strength by solid solution strengthening. In addition, by forming a layer with high potential and a layer with low potential in the sacrificial anode material in a layered distribution, the corrosion morphology changes from pitting to layered, which has the effect of improving corrosion resistance. The Ti content in the sacrificial anode material is less than 0.30 mass%, preferably 0.10-0.20 mass%. When the Ti content in the sacrificial anode material is within the above range, the strength of the sacrificial anode material becomes higher and the corrosion resistance becomes higher. On the other hand, when the Ti content in the sacrificial anode material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0148] Zr improves the strength by solid solution strengthening, and also precipitates fine Al-Zr compounds, which has an effect on the coarsening of grains after brazing. The Zr content in the sacrificial anode material is 0.30% by mass or less, preferably 0.10 to 0.20% by mass. By having the Zr content in the sacrificial anode material within the above range, the strength of the sacrificial anode material becomes higher, and the effect of coarsening grains after brazing can be obtained. On the other hand, when the Zr content in the sacrificial anode material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0149] The sacrificial anode material may contain less than 0.050 mass % of Ag, B, Be, Bi, Ca, Cd, Co, Ga, Ge, Hg, In, Li, Mo, Na, Ni, P, Pb, Sb, Sn, Sr, V, and Y as unavoidable impurities.
[0150] The outer surface brazing filler metal involved in the first embodiment of the aluminum alloy brazing sheet of the present invention and the outer surface brazing filler metal involved in the second embodiment of the aluminum alloy brazing sheet of the present invention are formed by the following aluminum alloy, wherein the aluminum alloy contains 6.00 to 13.00 mass% of Si, and also contains any one or more of 1.00 mass% or less of Fe, 2.00 mass% or less of Cu, 2.00 mass% or less of Mn, 4.50 mass% or less of Mg, 6.00 mass% or less of Zn, 0.50 mass% or less of Bi, 0.30 mass% or less of Cr, 0.30 mass% or less of Ti, and 0.30 mass% or less of Zr, and the balance is aluminum and unavoidable impurities.
[0151] The outer surface brazing filler metal contains Si. In the outer surface brazing filler metal of the aluminum alloy, Si contributes to the brazing weldability. The Si content in the outer surface brazing filler metal is 6.00 to 13.00 mass %. Sufficient brazing weldability can be obtained by keeping the Si content in the outer surface brazing filler metal within the above range. When the Si content in the outer surface brazing filler metal is lower than the above range, the weldability is poor. In addition, when the Si content exceeds the above range, cracks are easily generated during material manufacturing, and the manufacture of the brazing sheet material becomes difficult.
[0152] When the outer surface brazing material contains Fe, the Fe content in the outer surface brazing material is less than 1.00 mass %, preferably 0.10 to 0.50 mass %. When the Fe content in the outer surface brazing material is within the above range, the effect of grain refinement is easily obtained. On the other hand, when the Fe content of the outer surface brazing material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0153] When the outer surface brazing material contains Cu, the Cu content in the outer surface brazing material is 2.00 mass % or less, preferably 0.50 to 2.00 mass %. When the Cu content in the outer surface brazing material is within the above range, the effect of lowering the melting point of the brazing material is improved. On the other hand, when the Cu content in the outer surface brazing material exceeds the above range, cracks are generated during the material manufacturing process, and the manufacturing of the brazing sheet becomes difficult.
[0154] When the outer surface brazing material contains Mn, the Mn content in the outer surface brazing material is less than 2.00 mass %, preferably 0.10 to 0.60 mass %. When the Mn content in the outer surface brazing material is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Mn content in the outer surface brazing material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0155] When the outer surface brazing filler metal contains Mg, the Mg content in the outer surface brazing filler metal is 4.50 mass % or less, preferably 0.60 to 4.00 mass %. When the Mg content in the outer surface brazing filler metal is within the above range, sufficient brazing adhesion can be obtained. When the Mg content in the outer surface brazing filler metal is below the above range, the oxide film destruction effect becomes insufficient. In addition, when the Mg content exceeds the above range, cracks are easily generated during material manufacturing, and the manufacture of the brazing sheet becomes difficult.
[0156] In the case where the outer surface brazing material contains Zn, the Zn content in the outer surface brazing material is preferably 6.00 mass% or less based on the consideration that it is easier to obtain the effect of lowering the melting point of the brazing material. On the other hand, when the Zn content in the outer surface brazing material is greater than 6.00 mass%, cracks are generated during the material manufacturing process, and the manufacture of the brazing sheet becomes difficult. In addition, in the case where the outer surface brazing material contains Zn, based on the consideration that the potential of the brazing material is low, the core material is corroded preferentially, thereby easily obtaining the core material anti-corrosion effect, the Zn content in the outer surface brazing material is preferably 3.00 mass% or less.
[0157] When the outer surface brazing filler metal contains Bi, the Bi content in the outer surface brazing filler metal is 0.50 mass % or less. When the Bi content in the outer surface brazing filler metal is within the above range, sufficient brazing adhesion can be obtained. When the Bi content in the outer surface brazing filler metal is lower than the above range, the effect of promoting the destruction of the oxide film brought by Mg becomes insufficient. In addition, when the Bi content exceeds the above range, cracks are easily generated during material manufacturing, and the manufacture of the brazing sheet becomes difficult.
[0158] When the outer surface brazing material contains Cr, the Cr content in the outer surface brazing material is 0.30 mass % or less, preferably 0.10 to 0.20 mass %. When the Cr content in the outer surface brazing material is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Cr content in the outer surface brazing material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0159] When the outer surface brazing material contains Ti, the Ti content in the outer surface brazing material is less than 0.30 mass %, preferably 0.10 to 0.20 mass %. When the Ti content in the outer surface brazing material is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Ti content in the outer surface brazing material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0160] When the outer surface brazing material contains Zr, the Zr content in the outer surface brazing material is less than 0.30 mass %, preferably 0.10 to 0.20 mass %. When the Zr content in the outer surface brazing material is within the above range, the effect of grain coarsening is easily obtained. On the other hand, when the Zr content in the outer surface brazing material exceeds the above range, huge intermetallic compounds are easily formed during casting, and plastic workability is reduced.
[0161] Although the crystal grain size after brazing is adjusted by utilizing the above-mentioned action, the effect of the present invention can be fully obtained as long as it is within the above-mentioned range.
[0162] The outer surface brazing filler metal may contain any one or more of Na, Sr and Sb. In the aluminum alloy forming the outer surface brazing filler metal, Na, Sr and Sb play the role of refining Si particles in the brazing filler metal and improving the fluidity of the brazing filler metal. When the outer surface brazing filler metal contains Na, the Na content in the outer surface brazing filler metal is less than 0.050 mass %, preferably 0.005 to 0.040 mass %. When the outer surface brazing filler metal contains Sr, the Sr content in the outer surface brazing filler metal is less than 0.050 mass %, preferably 0.005 to 0.040 mass %. When the outer surface brazing filler metal contains Sb, the Sb content in the outer surface brazing filler metal is less than 0.050 mass %, preferably 0.005 to 0.040 mass %. By keeping the contents of Na, Sr and Sb in the outer surface brazing filler metal within the above range, the refining effect of Si particles can be obtained. On the other hand, when the contents of Na, Sr and Sb in the outer surface brazing filler metal exceed the above range, the effect is saturated and uneconomical.
[0163] The outer surface brazing material may contain 0.050 mass % or less of Ag, B, Be, Ca, Cd, Co, Ga, Ge, Hg, In, Li, Mo, Ni, P, Pb, Sn, V, and Y as unavoidable impurities.
[0164] As a method for manufacturing the aluminum alloy brazing sheet of the first embodiment of the present invention and the aluminum alloy brazing sheet of the second embodiment of the present invention, the following manufacturing methods can be cited. First, an aluminum alloy ingot having the composition of the core material involved in the aluminum alloy brazing sheet of the first embodiment of the present invention and the aluminum alloy brazing sheet of the second embodiment of the present invention is manufactured, and the aluminum alloy ingot for the core material is formed into a specified thickness. In addition, an aluminum alloy ingot having the composition of the aluminum alloy ingot for cladding (skin material 1, skin material 2, internal brazing filler metal 1, internal brazing filler metal 2, sacrificial anode material A, sacrificial anode material B1, sacrificial anode material B2, outer surface brazing filler metal) involved in the aluminum alloy brazing sheet of the first embodiment of the present invention and the aluminum alloy brazing sheet of the second embodiment of the present invention is manufactured, and the specified thickness is formed by hot rolling or the like. Next, the aluminum alloy ingot for the core material is homogenized at 450 to 630°C for 1 to 100 hours as needed. Next, the aluminum alloy ingot for the core material and the aluminum alloy ingot for the cladding material are stacked in a predetermined stacking order and hot rolled at 400 to 550° C. Next, one or more passes of cold rolling are performed until the predetermined thickness is reached and intermediate annealing and / or final annealing are performed at 250 to 450° C. for 1 to 24 hours as required, thereby obtaining the aluminum alloy brazing sheet of the first embodiment of the present invention or the aluminum alloy brazing sheet of the second embodiment of the present invention.
[0165] The aluminum alloy brazing sheet of the first embodiment of the present invention and the aluminum alloy brazing sheet of the second embodiment of the present invention are processed into a specified shape of a component of a heat exchanger and combined with other components for a heat exchanger as a part of a heat exchanger. Then, the heat exchanger is obtained by brazing by heating at a temperature of 580 to 630°C for 1 to 10 minutes without using a flux and in an inert gas atmosphere.
[0166] The aluminum alloy brazing sheet material of the first embodiment of the present invention and the aluminum alloy brazing sheet material of the second embodiment of the present invention have excellent brazing properties in brazing under an inactive gas atmosphere. The brazing properties of clad sheet materials are generally evaluated by a gap filling test (LWS T 8801). However, since the gap filling test forms a fillet and grows from one point, it is not sufficient to evaluate practical brazing properties such as the inflow and outflow of brazing material between multiple joints. To this end, in order to solve this problem, the inventors of the present invention developed an "open overlap test" to evaluate the brazing properties of each test material. The open overlap test shown below is the following test method: As Figure 1 As shown, a test material cut into a specified size, such as 15 mm wide and 25 mm long, and a bare material of A3003-O with a plate thickness of 1.0 mm cut into a specified size, such as 15 mm wide and 25 mm long, are overlapped in such a way that the surface covered with the skin material 1 and the internal brazing material 1 becomes the inner side, one side of the bare material is lifted, and a spacer with a diameter of 1.6 mm is inserted, so that the bare material on the opposite side of the spacer is linearly contacted with the test material, thereby preparing a test product with a small gap between the test material and the bare material, and the test product is brazed in a posture where the linear contact portion of the test material and the bare material is parallel to gravity. In the brazing heating in the open overlap test, after the test material is assembled on the open overlap test product, the brazing heating is performed in a furnace in a nitrogen atmosphere without using a flux. The brazing heating conditions are as follows: when the test product is above 400°C during the heating process, the oxygen concentration in the furnace is controlled to be below 50 ppm and the dew point is below -45°C. When the test product temperature is above 570°C, the oxygen concentration is controlled to be below 10 ppm and the dew point is below -60°C. The arrival temperature of the test product is set to 600°C. In this open overlap test, for example, when the destruction of the upper oxide film is delayed compared to the lower side in the gravity direction, since the fillet is formed first on the lower side, the brazing material that should have formed a fillet on the upper side flows out to the lower side where the fillet is formed. This is an extremely excellent evaluation method that can easily evaluate the inflow and outflow of the brazing material in practical products. Therefore, according to this open overlap test, the practical brazing properties such as the inflow and outflow of the brazing material between multiple joints can be appropriately evaluated.
[0167] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to the Examples shown below.
[0168] Example
[0169] (Examples and Comparative Examples)
[0170] Ingots were cast by continuous casting to obtain ingots for core material, ingots for internal brazing filler metal, and ingots for skin material having the compositions shown in Table 1. For the ingot for core material, the obtained ingot was face milled to a size of 163 mm in length, 163 mm in width, and 27 mm in thickness. For the ingot for skin material and ingot for brazing filler metal, the obtained ingot was hot rolled at 500° C. to a thickness of 3 mm, cold rolled to a specified thickness, and cut to a size of 163 mm in length and 163 mm in width.
[0171] [Table 1]
[0172] Alloy No. Si Fe Cu Mn Mg Zn Ti Bi A3003 core material 0.28 0.61 0.16 1.20 0.01 0.02 0.01 <0.01 C01 Leather 7.30 0.19 <0.01 <0.01 <0.01 <0.01 <0.01 <0.01 F01 Internal solder 7.50 0.19 <0.01 <0.01 0.33 <0.01 <001 0.15 F02 Internal solder 7.50 0.19 <0.01 <0.01 1.10 <0.01 <001 0.14 F03 Internal solder 7.50 0.19 <0.01 <0.01 1.00 <0.01 <0.01 0.31 F04 Internal solder 7.70 0.20 <0.01 <0.01 2.00 <0.01 <0.01 0.13 F05 Internal solder 7.90 0.20 <0.01 <0.01 2.40 <0.01 <001 <0.01 F06 Internal solder 7.80 0.20 <0.01 <0.01 2.50 <0.01 <001 0.12 F07 Internal solder 7.50 0.19 <0.01 <0.01 2.50 <0.01 <0.01 0.25 F08 Internal solder 8.00 0.19 <0.01 <0.01 4.20 <0.01 <0.01 0.08
[0173] The prepared core material ingot, internal brazing material ingot, and skin material ingot were stacked in the combination shown in Table 2, hot rolled and cold rolled to a thickness of 0.6 mm, and then finally annealed at 360°C by a conventional method to obtain a soft clad sheet material stacked in the order of skin material 1 / internal brazing material 1 / core material (Comparative Example 1 is internal brazing material 1 / core material). The obtained clad sheet material was used as a test material.
[0174] [Table 2]
[0175]
[0176] Next, the following open overlap test was performed using the obtained clad plate material. The results are shown in Table 3.
[0177] <Opening overlap test>
[0178] like Figure 1 As shown, a test material cut into pieces with a width of 15 mm and a length of 25 mm and a bare material of A3003-O with a thickness of 1.0 mm cut into pieces with a width of 15 mm and a length of 25 mm are overlapped in such a way that the surface coated with the skin material 1 and the internal solder 1 becomes the inner side, one side of the bare material is lifted and a spacer with a diameter of 1.6 mm is inserted, so that the bare material on the opposite side of the spacer is in linear contact with the test material, thereby preparing a test product with a small gap between the test material and the bare material.
[0179] Next, after assembling the test material onto the open overlap test product, the test product was brazed and heated in a furnace without flux in a nitrogen atmosphere, with the linear contact portion of the test material and the bare material parallel to gravity. The brazing heating conditions were as follows: when the test product was above 400°C during the heating process, the oxygen concentration in the furnace was controlled to be below 50 ppm and the dew point was below -45°C; when the test product temperature was above 570°C, the oxygen concentration was controlled to be below 10 ppm and the dew point was below -60°C; and the final temperature of the test product was set to 600°C.
[0180] After the brazing heating, the fillet shape formed in the micro gap of the open overlapped test product was photographed by X-ray CT. The imaging conditions were set to tube voltage 160 kV and tube current 100 μA, and the entire test product was photographed. Figure 2 A schematic diagram of the obtained X-ray CT image is shown in FIG. The fill corners are represented in white. Figure 2 The left side is the gravity lower side, and the right side is the gravity upper side. The obtained X-ray CT images were analyzed using ImageJ. The X-ray CT images were converted to black and white binary, the gravity direction was set as the x-axis, and the fillet length in the direction perpendicular to the x-axis was digitized. Based on the analysis results, the following three indicators were judged as ○×.
[0181] (Indicator 1) Within the range excluding the two ends of the image without fillet, if the fillet length = 0, that is, if there is no fillet, it is judged that there is a fillet break (×); otherwise, it is judged that there is no fillet break (0).
[0182] (Indicator 2) When the end of the fillet under gravity is set to x=0, the minimum fillet length of x=12-13mm is set to the center (B), the minimum fillet length of x=22-23mm is set to the gravity upper side (C), and the maximum fillet length of x=0-1mm is set to the gravity lower side (A), "((B+C) / 2) / A" is defined as the gravity influence coefficient of the fillet length. The larger the coefficient is, the more uniform the fillet is formed against gravity. The case of 0.35 or more is judged as (0), and the case of less than 0.34 is judged as (×).
[0183] [Table 3]
[0184]
[0185] According to the above results, it can be seen that the aluminum alloy brazing sheet according to the first mode of the present invention has an internal brazing material 1 and a skin material 1 whose chemical composition is within the specified range of the present invention, and their average Mg concentration and average Bi concentration in the thickness direction are within the specified range of the present invention, and has excellent brazing properties in brazing in an inactive gas atmosphere without using a flux.
[0186] In addition, according to the above results, it can be seen that the aluminum alloy brazing sheet of the second mode of the present invention, which has a skin material 1 with a chemical composition within the specified range of the present invention in the outermost layer, an internal brazing material 1 with a chemical composition within the specified range of the present invention on one of its inner sides, and their average Mg concentration and average Bi concentration in the thickness direction are within the specified range of the present invention, has excellent brazing properties in brazing in an inactive gas atmosphere without using a flux. Therefore, it can be inferred that the aluminum alloy brazing sheet of the second mode of the present invention, which has a skin material 1 with a chemical composition within the specified range of the present invention in the outermost layer, an internal brazing material 1 with a chemical composition within the specified range of the present invention on one of its inner sides, and their average Mg concentration and average Bi concentration in the thickness direction are within the specified range of the present invention, also has excellent brazing properties in brazing in an inactive gas atmosphere without using a flux.
Claims
1. An aluminum alloy brazing sheet, characterized in that: A brazing solder 1 and a skin material 1 are provided, which are used for brazing in an inert gas atmosphere without using a flux, and which have a core material formed of pure aluminum or an aluminum alloy, and an internal brazing solder 1 and a skin material 1 coated on at least one surface of the core material in the order of skin material 1 / internal brazing solder 1 / core material. The internal brazing filler metal 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and inevitable impurities. The skin material 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the remainder being aluminum and unavoidable impurities. The average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.50 mass %, and the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.050 mass %.
2. The aluminum alloy brazing sheet according to claim 1, characterized in that: It also has a sacrificial anode material A coated on the other side of the core material in the order of skin material 1 / internal brazing material 1 / core material / sacrificial anode material A, The sacrificial anode material A is formed by an aluminum alloy containing any one or more of less than 5.00 mass% Si, less than 1.50 mass% Fe, less than 2.00 mass% Cu, less than 2.00 mass% Mn, less than 3.00 mass% Mg, less than 6.00 mass% Zn, less than 0.30 mass% Cr, less than 0.30 mass% Ti, and less than 0.30 mass% Zr, with the remainder being aluminum and unavoidable impurities.
3. The aluminum alloy brazing sheet according to claim 1, characterized in that: It also has an outer surface solder coated on the other side of the core material in the order of skin material 1 / internal solder 1 / core material / outer surface solder, The outer surface brazing filler metal is formed by an aluminum alloy containing 6.00 to 13.00 mass % Si, and also containing any one or more of less than 1.00 mass % Fe, less than 2.00 mass % Cu, less than 2.00 mass % Mn, less than 4.50 mass % Mg, less than 6.00 mass % Zn, less than 0.50 mass % Bi, less than 0.30 mass % Cr, less than 0.30 mass % Ti, and less than 0.30 mass % Zr, with the balance being aluminum and unavoidable impurities.
4. The aluminum alloy brazing sheet according to claim 2, characterized in that: The invention also comprises an outer surface brazing material coated on the surface of the sacrificial anode material A opposite to the core material in the order of skin material 1 / internal brazing material 1 / core material / sacrificial anode material A / outer surface brazing material, The outer surface brazing filler metal is formed by an aluminum alloy containing 6.00 to 13.00 mass % Si, and also containing any one or more of less than 1.00 mass % Fe, less than 2.00 mass % Cu, less than 2.00 mass % Mn, less than 4.50 mass % Mg, less than 6.00 mass % Zn, less than 0.50 mass % Bi, less than 0.30 mass % Cr, less than 0.30 mass % Ti, and less than 0.30 mass % Zr, with the balance being aluminum and unavoidable impurities.
5. The aluminum alloy brazing sheet according to claim 2, characterized in that: The invention also comprises an internal brazing material 2 and a skin material 2 which are coated on the surface of the sacrificial anode material A opposite to the core material in the order of skin material 1 / internal brazing material 1 / core material / sacrificial anode material A / internal brazing material 2 / skin material 2. The internal brazing filler metal 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and unavoidable impurities. The skin material 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the balance being aluminum and inevitable impurities.
6. The aluminum alloy brazing sheet according to claim 1, characterized in that: It also has an internal brazing material 2 and a skin material 2 coated on the other side of the core material in the order of skin material 1 / internal brazing material 1 / core material / internal brazing material 2 / skin material 2, The internal brazing filler metal 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and unavoidable impurities. The skin material 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the balance being aluminum and inevitable impurities.
7. An aluminum alloy brazing sheet, characterized in that: A core material formed of pure aluminum or aluminum alloy, and a sacrificial anode material B1, an internal brazing material 1, and a skin material 1 coated on at least one surface of the core material in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material, which is used for brazing in an inert gas atmosphere without using a flux, The internal brazing filler metal 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and 4.50 mass % or less of Mg, and 0.010 to 0.50 mass % or less of Bi, with the remainder being aluminum and unavoidable impurities. The skin material 1 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the remainder being aluminum and unavoidable impurities. The sacrificial anode material B1 contains any one or more of 5.00 mass % or less of Si, 1.50 mass % or less of Fe, 2.00 mass % or less of Cu, 2.00 mass % or less of Mn, 3.00 mass % or less of Mg, 6.00 mass % or less of Zn, 0.30 mass % or less of Cr, 0.30 mass % or less of Ti, and 0.30 mass % or less of Zr, and the balance is aluminum and unavoidable impurities. The average Mg concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.50 mass %, and the average Bi concentration in the thickness direction of the internal solder 1 and the skin material 1 is greater than 0.050 mass %.
8. The aluminum alloy brazing sheet according to claim 7, characterized in that: It also has a sacrificial anode material B2 coated on the other side of the core material in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / sacrificial anode material B2, The sacrificial anode material B2 is an aluminum alloy containing any one or more of less than 5.00 mass% Si, less than 1.50 mass% Fe, less than 2.00 mass% Cu, less than 2.00 mass% Mn, less than 3.00 mass% Mg, less than 6.00 mass% Zn, less than 0.30 mass% Cr, less than 0.30 mass% Ti, and less than 0.30 mass% Zr, with the balance being aluminum and unavoidable impurities.
9. The aluminum alloy brazing sheet according to claim 7, characterized in that: It also has an outer surface brazing material coated on the other side of the core material in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / outer surface brazing material, The outer surface brazing filler metal is an aluminum alloy containing 6.00 to 13.00 mass % Si, and also containing any one or more of less than 1.00 mass % Fe, less than 2.00 mass % Cu, less than 2.00 mass % Mn, less than 4.50 mass % Mg, less than 6.00 mass % Zn, less than 0.50 mass % Bi, less than 0.30 mass % Cr, less than 0.30 mass % Ti, and less than 0.30 mass % Zr, with the balance being aluminum and unavoidable impurities.
10. The aluminum alloy brazing sheet according to claim 8, characterized in that: It also has an outer surface brazing filler coated on the surface of the sacrificial anode material 2 opposite to the core material in the order of skin material 1 / internal brazing filler 1 / sacrificial anode material B1 / core material / sacrificial anode material B2 / outer surface brazing filler, The outer surface brazing filler metal is an aluminum alloy containing 6.00 to 13.00 mass % Si, and also containing any one or more of less than 1.00 mass % Fe, less than 2.00 mass % Cu, less than 2.00 mass % Mn, less than 4.50 mass % Mg, less than 6.00 mass % Zn, less than 0.50 mass % Bi, less than 0.30 mass % Cr, less than 0.30 mass % Ti, and less than 0.30 mass % Zr, with the balance being aluminum and unavoidable impurities.
11. The aluminum alloy brazing sheet according to claim 8, characterized in that: It also has an internal brazing material 2 and a skin material 2 coated on the surface of the sacrificial anode material 2 opposite to the core material in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / sacrificial anode material B2 / internal brazing material 2 / skin material 2, The internal brazing filler metal 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and unavoidable impurities. The skin material 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the balance being aluminum and inevitable impurities.
12. The aluminum alloy brazing sheet according to claim 7, characterized in that: It also has an internal brazing material 2 and a skin material 2 coated on the other side of the core material in the order of skin material 1 / internal brazing material 1 / sacrificial anode material B1 / core material / internal brazing material 2 / skin material 2, The internal brazing filler metal 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, more than 0.50 mass % and less than 4.50 mass % of Mg, and 0.010 to 0.50 mass % of Bi, with the remainder being aluminum and unavoidable impurities. The skin material 2 is formed of an aluminum alloy containing 6.00 to 13.00 mass % of Si, 0.050 mass % or less of Mg, 0.050 mass % or less of Bi, and the balance being aluminum and inevitable impurities.
13. The aluminum alloy brazing sheet according to any one of claims 1 to 12, characterized in that: The core material is formed by an aluminum alloy containing any one or more of 1.50 mass % Si, 1.50 mass % Fe, 2.00 mass % Cu, 2.00 mass % Mn, 3.00 mass % Mg, 3.00 mass % Zn, 0.50 mass % Bi, 0.30 mass % Cr, 0.30 mass % Ti, and 0.30 mass % Zr, with the balance being aluminum and unavoidable impurities.
14. The aluminum alloy brazing sheet according to any one of claims 1 to 13, characterized in that The internal brazing material 1 or the internal brazing material 2 further contains any one or two or more of 1.00 mass % or less of Fe, 2.00 mass % or less of Cu, 2.00 mass % or less of Mn, 6.00 mass % or less of Zn, 0.30 mass % or less of Cr, 0.30 mass % or less of Ti, and 0.30 mass % or less of Zr.
15. The aluminum alloy brazing sheet according to any one of claims 1 to 14, characterized in that The skin material 1 or the skin material 2 further contains any one or two or more of 1.00 mass % or less of Fe, 2.00 mass % or less of Cu, 2.00 mass % or less of Mn, 6.00 mass % or less of Zn, 0.30 mass % or less of Cr, 0.30 mass % or less of Ti, and 0.30 mass % or less of Zr.
16. The aluminum alloy brazing sheet according to any one of claims 1 to 15, characterized in that The thickness of the leather material 1 or the leather material 2 is greater than 5.0 μm.
17. The aluminum alloy brazing sheet according to any one of claims 1 to 16, characterized in that: The thickness of the internal brazing material 1 or the internal brazing material 2 is 15.0 μm or more.