Resin composition, molded article, and method for manufacturing molded article
By adjusting the structural units and melting point difference of the polyamide resin, a phthalamine-based polyamide resin composition containing 7 to 16 carbon aliphatic dicarboxylic acid is formed, and the polyamide in the prior art is solved. The problem of slow crystallization speed and poor physical properties of the resin composition achieves rapid crystallization and high mechanical strength molded products, and are not easily affected by the mold temperature.
Patent Information
- Application Number
- CN202280094268.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-12
AI Technical Summary
The conventional polyamide resin composition has a slow crystallization rate and poor physical properties of the molded article, and the crystallization rate is easily affected by the mold temperature, resulting in a narrowing of the molding condition range and making it difficult to stabilize molding.
A phthalamine-based polyamide resin containing α,ω-linear aliphatic dicarboxylic acid derived from 7 to 16 carbons is used to form a resin combination by adjusting the melting point difference and structural unit ratio of the polyamide resins A and B. The polyamide resin B exists in the resin composition in a dispersed state, which promotes the crystallization of the polyamide resin A and maintains high mechanical strength at an appropriate temperature.
A resin composition with fast crystallization speed and low physical properties of molded articles is achieved. The crystallization speed is not easy to depend on the mold temperature, maintains high mechanical strength, and expands the stability of molding conditions.
Smart Images

Figure BDA0005061593600000011 
Figure BDA0005061593600000012 
Figure BDA0005061593600000231
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, a molded product, and a method for producing the molded product. Background Art
[0002] Polyamide resins have excellent mechanical strength, heat resistance, water resistance, and chemical resistance. Therefore, plastics produced from resin compositions containing polyamide resins are used in various applications such as automobiles, transportation, and electrical and electronic equipment.
[0003] When a commercially available polyamide resin is injection molded with sufficient quality, it is required to set the mold temperature to a high temperature in order to fully crystallize the polyamide resin in the mold.
[0004] In order to solve this problem, Patent Document 1 discloses a resin composition comprising a polyamide (P1) and a polyamide (P2), wherein Tm(P2) and Tm(P1) as the melting points of P2 and P1 satisfy Tm(P2)>Tm(P1), and Tc(P2) and Tc(P1) as the crystallization temperatures of P2 and P1 when the temperature is lowered satisfy Tc(P2)>Tc(P1), the weight ratio of P1 / P2 varies between 15 / 1 and 1 / 1, and P1 comprises the following structural units,
[0005] (I)
[0006]
[0007] n is 4 to 18, R1 comprises m-xylene and p-xylene in a ratio of 1:99 to 99:1 in mole %, and P2 comprises the following structural units,
[0008]
[0009] m is 6 to 18.
[0010] Furthermore, the Examples of Patent Document 1 disclose a resin composition containing about 44 to 29 parts by mass of MXD6 / PXD6 and about 5 to 20 parts by mass of PXD10. Here, MXD refers to meta-xylylenediamine, PXD refers to para-xylylenediamine, 6 refers to adipic acid, and 10 refers to sebacic acid.
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: International Publication No. 2020 / 225358 Summary of the invention
[0014] Problem that the invention aims to solve
[0015] Here, the present inventors have studied the resin composition described in Patent Document 1, and found that its crystallization rate is slow. Furthermore, it is known that the resin composition described in Patent Document 1 has a large change in half crystallization time, i.e., crystallization rate, due to mold temperature. In addition, even if the crystallization rate is fast, if the physical properties of the obtained molded product are poor, it lacks practicality.
[0016] The present invention aims to solve the above problems, and an object of the present invention is to provide a resin composition having a high crystallization rate and little deterioration in the physical properties of the obtained molded article.
[0017] Another object of the present invention is to provide a molded article formed from the above resin composition, and a method for producing the molded article.
[0018] Solutions for solving problems
[0019] The present inventors have conducted studies based on the above problems and have found that the above problems can be solved by using a xylylenediamine-based polyamide resin containing a structural unit derived from an α,ω-linear aliphatic dicarboxylic acid having 7 to 16 carbon atoms.
[0020] Specifically, the above-mentioned problems are solved by the following means.
[0021] <1> A resin composition comprising a polyamide resin A and a polyamide resin B, wherein the polyamide resin B is contained in an amount of 1 to 15 parts by mass based on 100 parts by mass of the total of the polyamide resin A and the polyamide resin B, wherein the difference (Tmb-Tma) between the melting point Tmb of the polyamide resin B measured by differential scanning calorimetry (DSC) and the melting point Tma of the polyamide resin A measured by differential scanning calorimetry (DSC) is 35 to 110°C, the polyamide resin A comprises a structural unit derived from a diamine and a structural unit derived from a dicarboxylic acid, the structural unit derived from the diamine comprising 100 to 50 mol% of a structural unit derived from m-xylylenediamine and 0 to 50 mol% of a structural unit derived from p-xylylenediamine (wherein the total of the structural unit derived from m-xylylenediamine and the structural unit derived from p-xylylenediamine is not more than 100 mol%), and 70 mol% or more of the structural unit derived from the dicarboxylic acid is derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms,
[0022] The polyamide resin B comprises a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, wherein the diamine-derived structural unit comprises 100 to 95 mol % of a p-xylylenediamine-derived structural unit and 0 to 5 mol % of a m-xylylenediamine-derived structural unit (wherein the total of the p-xylylenediamine-derived structural unit and the m-xylylenediamine-derived structural unit does not exceed 100 mol %), and 70 mol % or more of the dicarboxylic acid-derived structural unit is derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms.
[0023] <2> The resin composition according to <1>, wherein the polyamide resin A has a melting point Tma of 180 to 240°C as measured by differential scanning calorimetry (DSC).
[0024] <3> The resin composition according to <1> or <2>, wherein 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin A are derived from sebacic acid.
[0025] <4> The resin composition according to any one of <1> to <3>, wherein the polyamide resin B has a melting point Tmb of 270 to 320°C as measured by differential scanning calorimetry (DSC).
[0026] <5> The resin composition according to any one of <1> to <4>, wherein 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin B are derived from sebacic acid.
[0027] <6> The resin composition according to <1>, wherein the melting point Tma of the polyamide resin A as measured by differential scanning calorimetry (DSC) is 180 to 240°C, and 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin A are derived from sebacic acid, and the melting point Tmb of the polyamide resin B as measured by differential scanning calorimetry (DSC) is 270 to 320°C, and 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin B are derived from sebacic acid.
[0028] <7> The resin composition according to any one of <1> to <6>, further comprising 10 to 150 parts by mass of a reinforcing material based on 100 parts by mass of the total of the polyamide resin A and the polyamide resin B.
[0029] <8> A molded article formed from the resin composition according to any one of <1> to <7>.
[0030] <9> A method for producing a molded article, comprising injection molding the resin composition according to any one of <1> to <7>.
[0031] <10> The method for producing a molded article according to <9>, wherein a cylinder temperature during the injection molding is at least the melting point of the polyamide resin A + 20°C and less than the melting point of the polyamide resin B.
[0032] <11> The method for producing a molded article according to <9> or <10>, wherein, in the resin composition immediately before injection into the injection molding die, the polyamide resin A is melted and at least a portion of the polyamide resin B is not melted.
[0033] Effects of the Invention
[0034] According to the present invention, it is possible to provide a resin composition having a high crystallization rate and having little deterioration in the physical properties of the obtained molded article, a molded article formed from the resin composition, and a method for producing the molded article. DETAILED DESCRIPTION
[0035] Hereinafter, a mode for implementing the present invention (hereinafter also referred to as "this embodiment") will be described in detail. It should be noted that the following this embodiment is an example for describing the present invention, and the present invention is not limited to only this embodiment.
[0036] In addition, in this specification, "to" is used to mean that the numerical value described before and after it is included as a lower limit and an upper limit.
[0037] In this specification, various physical property values and characteristic values are values at 23° C. unless otherwise specified.
[0038] When the measurement methods and the like described in the standards in this specification differ depending on the year, unless otherwise specified, they are based on the standards as of January 1, 2022.
[0039] It should be noted that in this specification, a polyamide resin synthesized from m-xylylenediamine, p-xylylenediamine and adipic acid is sometimes referred to as MP6, and a polyamide resin synthesized from m-xylylenediamine, p-xylylenediamine and sebacic acid is sometimes referred to as MP10. In addition, a polyamide resin synthesized from m-xylylenediamine and adipic acid is sometimes referred to as MXD6, and a polyamide resin synthesized from p-xylylenediamine and sebacic acid is sometimes referred to as PXD10.
[0040] The resin composition of the present embodiment includes a polyamide resin A and a polyamide resin B, wherein the polyamide resin B is contained in an amount of 1 to 15 parts by mass relative to a total of 100 parts by mass of the polyamide resin A and the polyamide resin B, wherein the difference (Tmb-Tma) between the melting point Tmb of the polyamide resin B measured by differential scanning calorimetry (DSC) and the melting point Tma of the polyamide resin A measured by differential scanning calorimetry (DSC) is 35 to 110° C., and the polyamide resin A includes a structural unit derived from a diamine and a structural unit derived from a dicarboxylic acid, wherein the structural unit derived from the diamine includes 100 to 50 mol % of a structural unit derived from meta-xylylenediamine and 0 to 50 mol % of a structural unit derived from p-xylylenediamine (wherein the structural unit derived from meta-xylylenediamine is 0 to 50 mol %). The polyamide resin B comprises structural units derived from diamines and structural units derived from dicarboxylic acids, the structural units derived from diamines comprise 100 to 95 mol % of structural units derived from p-xylylenediamine and 0 to 5 mol % of structural units derived from m-xylylenediamine (wherein the total of structural units derived from p-xylylenediamine and structural units derived from m-xylylenediamine does not exceed 100 mol %), and 70 mol % or more of the structural units derived from dicarboxylic acids are derived from α, ω-straight-chain aliphatic dicarboxylic acids having 7 to 16 carbon atoms.
[0041] In addition, in this specification, when one polyamide resin A shows two or more melting points, the highest melting point is regarded as the melting point of the polyamide resin A. The same applies to the polyamide resin B.
[0042] By adopting such a configuration, a composition having a high crystallization rate and a small decrease in the physical properties of the obtained molded article can be obtained. Furthermore, a resin composition having a crystallization rate that is less likely to depend on the mold temperature can be provided.
[0043] The polyamide resin A represented by MP10 and MXD10 is essentially a polyamide resin with excellent mechanical properties, but it is also a polyamide resin with a not too fast crystallization rate. Therefore, when MP10 and the like are molded, in order to promote crystallization, inorganic crystallization nucleating agents such as talc are usually mixed, or resins with short semi-crystallization times such as polyamide 66 (PA66) are mixed. However, if inorganic crystallization nucleating agents such as talc are mixed, there is a tendency for the obtained molded product to have poor physical properties such as mechanical strength. In addition, if resins such as PA66 are mixed, the following phenomenon will occur: at some temperatures, the semi-crystallization time becomes shorter, that is, the crystallization rate becomes faster, and at some temperatures, the semi-crystallization time does not become shorter. Furthermore, if resins such as PA66 are mixed, the degree of progress of crystallization due to the mold temperature is greatly different. If the degree of progress of crystallization due to the mold temperature is different, the molding condition range becomes narrower and it becomes difficult to stably mold. In particular, when PA66 is blended into a polyamide resin A such as MP10, crystallization may not be completed in a low-temperature mold.
[0044] In this embodiment, by blending a polyamide resin B such as PXD10 having a melting point higher than 35°C with a polyamide resin A such as MP10, a resin composition containing a polyamide resin A such as MP10 can be provided, which has a high crystallization rate and is not easily affected by temperature. Furthermore, since the crystallization rate can be accelerated even without blending an inorganic crystal nucleating agent such as talc, physical properties such as high mechanical strength can be maintained.
[0045] The reason is speculated to be: by using a polyamide resin with a large melting point difference, at a suitable temperature for the molding of the polyamide resin A as the main component, the polyamide resin B is hardly melted in the resin composition, but exists in a dispersed state. That is, the polyamide resin B plays a role like an inorganic crystal nucleating agent, promoting the crystallization of the polyamide resin A. On the other hand, the polyamide resin B will not affect the reduction of the physical properties of the obtained molded product like an inorganic crystal nucleating agent. And then, polyamide resin B is different from PA66, etc., and the difference in the half crystallization time caused by the mold temperature can also be reduced. It is speculated that this is due to the melting point of PA66 being close to the polyamide resin A such as MP10. Therefore, it is speculated that at the molding temperature of polyamide resin A, PA66 also becomes a state of easy melting, and will not play the effect as a crystal nucleating agent as mentioned above.
[0046] Furthermore, this embodiment has an advantage that the half crystallization time is unlikely to change even if the mold temperature is lowered.
[0047] Hereinafter, the resin composition according to the present embodiment will be described in detail.
[0048] <Polyamide resin A>
[0049] The resin composition of the present embodiment includes a polyamide resin A, which includes a structural unit derived from a diamine and a structural unit derived from a dicarboxylic acid, wherein the structural unit derived from the diamine includes 100 to 50 mol% of a structural unit derived from meta-xylylenediamine and 0 to 50 mol% of a structural unit derived from para-xylylenediamine (wherein the total of the structural unit derived from meta-xylylenediamine and the structural unit derived from para-xylylenediamine does not exceed 100 mol%), and 70 mol% or more of the structural unit derived from the dicarboxylic acid is derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms. Polyamide resin A is usually a component that becomes the main component of the resin component contained in the resin composition of the present embodiment. Polyamide resin A has excellent various physical properties such as mechanical strength, and molded products obtained using such a resin are suitable for various uses.
[0050] In the polyamide resin A, the structural unit derived from diamine contains 100 to 50 mol % of the structural unit derived from meta-xylylenediamine and 0 to 50 mol % of the structural unit derived from p-xylylenediamine.
[0051] In the polyamide resin A, preferably 80 mol % or more, more preferably 90 mol % or more, further preferably 95 mol % or more, and even more preferably 99 mol % or more of the structural units derived from diamine are derived from xylylenediamine.
[0052] As described above, the xylylenediamine contains 100-50 mol % of m-xylylenediamine and 0-50 mol % of p-xylylenediamine, preferably 90-50 mol % of m-xylylenediamine and 10-50 mol % of p-xylylenediamine, and more preferably 80-60 mol % of m-xylylenediamine and 20-40 mol % of p-xylylenediamine.
[0053] Examples of diamines other than p-xylylenediamine and m-xylylenediamine that can be used as the raw material diamine component of the polyamide resin A include aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, 2-methylpentanediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, dodecamethylenediamine, 2,2,4-trimethyl-hexamethylenediamine, and 2,4,4-trimethylhexamethylenediamine; and 1,3 - Alicyclic diamines such as bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminomethyl)decalin, and bis(aminomethyl)tricyclodecane, and diamines having an aromatic ring such as bis(4-aminophenyl)ether, p-phenylenediamine, and bis(aminomethyl)naphthalene, etc., which can be used alone or in combination of two or more.
[0054] In the polyamide resin A, 70 mol% or more, preferably 75 mol% or more, more preferably 80 mol% or more, further preferably 85 mol% or more, even more preferably 90 mol% or more, still more preferably 95 mol% or more, and still more preferably 99 mol% or more of the structural units derived from dicarboxylic acid are derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms (preferably sebacic acid).
[0055] There is a tendency that the crystallization half time becomes less likely to be dependent on the mold temperature by increasing the ratio of the α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms.
[0056] Examples of the α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms include pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, and tetradecanedioic acid. Sebacic acid and dodecanedioic acid are preferred, and sebacic acid is more preferred.
[0057] Examples of dicarboxylic acids other than the above-mentioned α,ω-straight-chain aliphatic dicarboxylic acids having 7 to 16 carbon atoms include straight-chain aliphatic dicarboxylic acids having 6 or less carbon atoms such as adipic acid, phthalic acid compounds such as isophthalic acid, terephthalic acid, and phthalic acid, and isomers of naphthalene dicarboxylic acids such as 1,2-naphthalene dicarboxylic acid, 1,3-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, and 2,7-naphthalene dicarboxylic acid. These can be used alone or in combination of two or more.
[0058] The polyamide resin A in the present embodiment is composed of the structural unit derived from diamine and the structural unit derived from dicarboxylic acid as the main component, and the structural units other than these are not completely excluded. It is self-evident that the structural unit derived from aliphatic aminocarboxylic acids such as lactams such as ε-caprolactam, laurolactam, aminocaproic acid, and aminoundecanoic acid may also be included. The main component here refers to the structural unit that constitutes the polyamide resin A, and the total number of the structural unit derived from diamine and the structural unit derived from dicarboxylic acid is the largest among all structural units. In the present embodiment, the total of the structural unit derived from diamine and the structural unit derived from dicarboxylic acid in the polyamide resin A preferably accounts for more than 90% by mass of all structural units, more preferably more than 95% by mass, and further preferably more than 98% by mass.
[0059] The melting point Tma of the polyamide resin A according to differential scanning calorimetry (DSC) is preferably 180°C or more, more preferably 185°C or more, further preferably 195°C or more, more preferably 200°C or more, and even more preferably 210°C or more. By setting it to be above the aforementioned lower limit, there is a tendency that the mold temperature dependence of the half crystallization time becomes lower. The aforementioned melting point Tma is preferably 240°C or less, more preferably 235°C or less, further preferably 230°C or less, more preferably 225°C or less, and even more preferably 220°C or less. By setting it to be below the aforementioned upper limit, the range of conditions that can be stably molded is widened, so it is preferred.
[0060] <Polyamide resin B>
[0061] The resin composition of the present embodiment includes a polyamide resin B, which includes a structural unit derived from a diamine and a structural unit derived from a dicarboxylic acid, wherein the structural unit derived from the diamine includes 100 to 95 mol% of a structural unit derived from p-xylylenediamine and 0 to 5 mol% of a structural unit derived from m-xylylenediamine (wherein the total of the structural unit derived from p-xylylenediamine and the structural unit derived from m-xylylenediamine does not exceed 100 mol%), and 70 mol% or more of the structural unit derived from the dicarboxylic acid is derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms. By including the polyamide resin B, the excellent physical properties of the obtained resin composition can be maintained, and the half-crystallization time of the resin composition can be shortened.
[0062] In the polyamide resin B, the structural unit derived from diamine includes 100 to 95 mol% of the structural unit derived from p-xylenediamine and 0 to 5 mol% of the structural unit derived from m-xylenediamine. By increasing the proportion of p-xylenediamine, the melting point of the polyamide resin B can be increased. In this embodiment, the structural unit derived from diamine is preferably 95 mol% or more, more preferably 96 mol% or more, further preferably 97 mol% or more, more preferably 98 mol% or more, and even more preferably 99 mol% or more derived from p-xylenediamine. The upper limit is 100 mol% of p-xylenediamine.
[0063] The polyamide resin B may contain a structural unit derived from a diamine other than p-xylylenediamine and m-xylylenediamine. The diamine in this case has the same meaning as the diamine other than p-xylylenediamine and m-xylylenediamine described in the section of the polyamide resin A.
[0064] In the polyamide resin B, 70 mol% or more, preferably 75 mol% or more, more preferably 80 mol% or more, further preferably 85 mol% or more, even more preferably 90 mol% or more, still more preferably 95 mol% or more, and still more preferably 99 mol% or more of the structural units derived from dicarboxylic acid are derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms (preferably sebacic acid).
[0065] Examples of the α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms include pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, and tetradecanedioic acid. Sebacic acid and dodecanedioic acid are preferred, and sebacic acid is more preferred.
[0066] The dicarboxylic acids other than the above-mentioned α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms have the same meanings as those described in the section of the polyamide resin A above.
[0067] The polyamide resin B in the present embodiment is composed of the structural unit derived from diamine and the structural unit derived from dicarboxylic acid as the main component, but the structural units other than these are not completely excluded, and the structural units derived from aliphatic aminocarboxylic acids such as lactams such as ε-caprolactam, laurolactam, aminocaproic acid, and aminoundecanoic acid may also be included, which is self-evident. The main component here refers to the structural unit that constitutes the polyamide resin B, and the total number of the structural unit derived from diamine and the structural unit derived from dicarboxylic acid is the largest among all structural units. In the present embodiment, the total of the structural unit derived from diamine and the structural unit derived from dicarboxylic acid in the polyamide resin B preferably accounts for more than 90% by mass of all structural units, more preferably more than 95% by mass, and further preferably more than 98% by mass.
[0068] The melting point Tmb of the polyamide resin B according to differential scanning calorimetry (DSC) is preferably 270°C or higher, more preferably 275°C or higher, further preferably 280°C or higher, further preferably 285°C or higher, and further preferably 288°C or higher. The melting point Tmb is preferably 320°C or lower, more preferably 310°C or lower, further preferably 305°C or lower, further preferably 300°C or lower, and further preferably 295°C or lower.
[0069] The content of the polyamide resin B in the resin combination of the present embodiment is preferably more than the 0.5 mass % of resin combination, more preferably more than the 1 mass %, further preferably more than the 2 mass %, more preferably more than the 4 mass %.In addition, the content of the polyamide resin B in the resin combination of the present embodiment is preferably less than the 15 mass % of resin combination, more preferably less than the 11 mass %, further preferably less than the 10 mass %, further preferably less than the 8 mass %, more preferably less than the 6 mass %.By being set to such scope, there is a tendency to more effectively play the effect of the present invention.
[0070] <Relationship between polyamide resin A and polyamide resin B>
[0071] In the resin composition of the present embodiment, 1 to 15 parts by mass of polyamide resin B are included relative to a total of 100 parts by mass of polyamide resin A and polyamide resin B. By setting it to above the aforementioned lower limit, the half-crystallization time can be shortened. By setting it to below the aforementioned upper limit, there is a tendency to suppress the reduction of mechanical properties. Furthermore, in the present embodiment, relative to a total of 100 parts by mass of polyamide resin A and polyamide resin B, the content of polyamide resin B is preferably 2 parts by mass or more, and is preferably 14 parts by mass or less, more preferably 12 parts by mass or less, and may also be 10 parts by mass or less.
[0072] The total amount of the polyamide resin A and the polyamide resin B in the resin composition of the present embodiment is preferably 40% by mass or more, more preferably 45% by mass or more, and may be 50% by mass or more. In addition, the total amount of the polyamide resin A and the polyamide resin B in the resin composition of the present embodiment is preferably 80% by mass or less, more preferably 75% by mass or less in the resin composition.
[0073] In addition, relative to the total amount of the resin composition contained in the resin combination of the present embodiment, the total amount of polyamide resin A and polyamide resin B is preferably more than 95 mass %, more preferably more than 97 mass %, further more preferably more than 99 mass %.Relative to the total amount of the resin composition contained in the resin combination of the present embodiment, as the upper limit of the total amount of polyamide resin A and polyamide resin B, is 100 mass %.
[0074] In the resin composition of the present embodiment, the polyamide resin A and the polyamide resin B may contain only one kind or two or more kinds, respectively. When containing two or more kinds, it is preferable that the total amount is within the above range.
[0075] In the resin composition of the present embodiment, the difference (Tmb-Tma) between the melting point Tmb of the polyamide resin B by differential scanning calorimetry (DSC) and the melting point Tma of the polyamide resin A by differential scanning calorimetry (DSC) is 35 to 110° C. By setting the value to be greater than or equal to the lower limit and less than or equal to the upper limit, the half crystallization time can be made less likely to depend on the mold temperature.
[0076] In the present embodiment, the aforementioned (Tmb-Tma) is preferably 40°C or more, more preferably 55°C or more, further preferably 60°C or more, more preferably 65°C or more, and even more preferably 70°C or more. By setting it to be above the aforementioned lower limit, it becomes possible to stably mold. In addition, the aforementioned (Tmb-Tma) is preferably 105°C or less, more preferably 95°C or less, further preferably 90°C or less, more preferably 85°C or less, and even more preferably 80°C or less. By setting it to be below the aforementioned upper limit, there is a tendency to make the mold temperature dependence of the half crystallization time lower.
[0077] In the present embodiment, when two or more types of polyamide resins A are included, the melting point of the polyamide resin A is set to the melting point of the component with the largest content. The same applies to the polyamide resin B.
[0078] The resin composition of the present embodiment is particularly preferably: the melting point Tma of the polyamide resin A according to differential scanning calorimetry (DSC) is 180 to 240°C (preferably 180 to 230°C), 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin A are derived from sebacic acid, the melting point Tmb of the polyamide resin B according to differential scanning calorimetry (DSC) is 270 to 320°C, and 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin B are derived from sebacic acid. It is further preferred that the difference (Tmb-Tma) between the melting point Tmb of the polyamide resin B according to differential scanning calorimetry (DSC) and the melting point Tma of the polyamide resin A according to differential scanning calorimetry (DSC) is 55 to 110°C (preferably 70 to 105°C).
[0079] Furthermore, in the resin composition of the present embodiment, preferably, 95 mol% or more (more preferably 98 mol% or more, and further preferably 99 mol% or more) of all the structural units derived from dicarboxylic acid contained in the polyamide resin A and the polyamide resin B are derived from sebacic acid, and 95 mol% or more (more preferably 98 mol% or more, and further preferably 99 mol% or more) of all the structural units derived from diamine contained in the polyamide resin A and the polyamide resin B are derived from m-xylylenediamine or p-xylylenediamine.
[0080] <Other ingredients>
[0081] The resin composition of the present embodiment can also include the components except polyamide resin A and polyamide resin B. Specifically, polyamide resin except polyamide resin A and polyamide resin B, thermoplastic resin except polyamide resin, reinforcing material, inorganic crystal nucleating agent (such as talcum), mold release agent, coloring agent, light stabilizer, antioxidant, heat stabilizer, flame retardant, flame retardant auxiliary agent, ultraviolet light absorber, fluorescent whitening agent, anti-dripping agent, antistatic agent, antifogging agent, anti-blocking agent, fluidity improver, weatherability improver, light resistance improver, plasticizer, dispersant, antibacterial agent etc. can be listed. These components can only use 1 kind, and 2 or more kinds can also be used in combination. These can refer to the records of paragraphs 0130~0155 of Japanese Patent Gazette No. 4894982 in detail, and these contents are grouped in this specification.
[0082] In particular, regarding the release agent used in the present embodiment, reference can be made to the description in paragraph 0030 of JP-A-2021-188029, the contents of which are incorporated into the present specification.
[0083] In particular, regarding the inorganic crystal nucleating agent used in the present embodiment, reference may be made to the descriptions in paragraphs 0031 and 0032 of JP-A-2021-188029, the contents of which are incorporated into the present specification.
[0084] It should be noted that the resin composition of the present embodiment may also be a composition that does not substantially contain an inorganic crystal nucleating agent. Substantially free means that, for example, the inorganic crystal nucleating agent is less than 0.01% by mass, preferably less than 0.001% by mass, in the resin composition. In the present embodiment, it is preferred from the perspective of shortening the semi-crystallization time even if the amount of inorganic crystal nucleating agents such as talc is small or not mixed.
[0085] <<Reinforcement Materials>>
[0086] The resin composition of the present embodiment preferably contains a reinforcing material. The reinforcing material may be an organic reinforcing material or an inorganic reinforcing material, and is preferably an inorganic reinforcing material.
[0087] Examples of the reinforcing material include filler, particle, and fiber, and fiber is preferred.
[0088] The reinforcing material used in this embodiment is preferably plant fiber, carbon fiber, glass fiber, alumina fiber, boron fiber, ceramic fiber, aramid fiber, etc., more preferably selected from carbon fiber and glass fiber, and further preferably glass fiber.
[0089] As the glass fiber, fibers obtained by melt spinning commonly available E glass, C glass, A glass, S glass, alkali-resistant glass, etc. can be used, and any glass fiber can be used without particular limitation as long as it can be made into glass fiber. In the present embodiment, E glass is preferably included.
[0090] The glass fiber is preferably surface treated with a surface treatment agent such as a silane coupling agent such as γ-methacryloxypropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, and γ-aminopropyltriethoxysilane. The amount of the surface treatment agent attached is preferably 0.01 to 1% by mass of the glass fiber. It is also possible to use a glass fiber obtained by surface treatment with a resin having film-forming ability such as a fatty acid amide compound, a lubricant such as silicone oil, an antistatic agent such as a quaternary ammonium salt, an epoxy resin, a urethane resin, or a mixture of a resin having film-forming ability and a heat stabilizer, a flame retardant, etc. as needed.
[0091] The glass fiber used in the resin composition of the present embodiment can be obtained as a commercial product. As commercial products, examples include: T-275H, T-286H, T-756H, T-289, T-289DE, T-289H, T-296GH manufactured by Nippon Electric Glass (NEG); DEFT2A manufactured by Owens Corning, HP3540 manufactured by PPG; CSG3PA-810S and CSG3PA-820 manufactured by Nittobo Co., Ltd.; EFH50-31 manufactured by Central Glass Co., Ltd. (all trade names), etc.
[0092] The cross section of the reinforcing material can be any of a circular shape and a non-circular shape (oval, oblong, rectangular, a shape with a semicircle on the two short sides of a rectangle, a cocoon shape, etc.), preferably a circular shape. When the present invention uses a reinforcing material having a circular cross section, the improvement effect of flame retardancy and mechanical strength is particularly significant.
[0093] The meaning of circle here includes not only a perfect circle in a geometric sense, but also shapes generally referred to as a circle in the technical field of the present invention.
[0094] Examples of the reinforcing material having a non-circular cross section include the flat reinforcing material described in paragraphs 0048 to 0052 of Japanese Patent Application Laid-Open No. 2012-214819, and the contents thereof are incorporated into the present specification.
[0095] The number average fiber length (cut length) of the reinforcing material in the resin composition of the present embodiment is preferably 100 μm or more, more preferably 150 μm or more, and further preferably 200 μm or more. The upper limit is preferably 10 mm or less, more preferably 8 mm or less, and further preferably 5 mm or less.
[0096] The reinforcing material used in the resin composition of the present embodiment preferably has a number average fiber diameter of 1 μm or more, more preferably 2 μm or more, and further preferably 5 μm or more, and an upper limit of preferably 50 μm or less, more preferably 30 μm or less, and further preferably 20 μm or less.
[0097] About the content of the reinforcing material (preferably glass fiber) in the resin composition of the present embodiment, relative to the total 100 mass parts of polyamide resin A and polyamide resin B, preferably more than 10 mass parts, more preferably more than 20 mass parts, and further preferably more than 30 mass parts. In addition, as the upper limit of the content of the aforementioned reinforcing material, relative to the total 100 mass parts of polyamide resin A and polyamide resin B, preferably less than 150 mass parts, more preferably less than 120 mass parts, can also be less than 100 mass parts, can also be less than 80 mass parts.
[0098] About the content of the reinforcing material (preferably glass fiber) in the resin combination of the present embodiment, the lower limit is preferably more than 20 mass % of the resin combination, more preferably more than 25 mass %.The upper limit of the aforementioned content is preferably below 60 mass %, more preferably below 55 mass %, and can also be below 50 mass %.By being set to more than the above-mentioned lower limit, there is a tendency that mechanical strength improves significantly.On the other hand, by the amount of the reinforcing material being set to below the above-mentioned upper limit, there is a tendency that moldability further improves.
[0099] The resin composition of the present embodiment may contain only one reinforcing material, or may contain two or more reinforcing materials. When containing two or more reinforcing materials, it is preferred that the total amount is within the above range.
[0100] <<Other polyamide resins>>
[0101] As other polyamide resins, an aliphatic polyamide resin or a semi-aromatic polyamide resin may be used, and an aliphatic polyamide resin is preferred.
[0102] Examples of the aliphatic polyamide resin include polyamide 6, polyamide 66, polyamide 666, polyamide 10, polyamide 610, polyamide 11, and polyamide 12.
[0103] Examples of the semi-aromatic polyamide resin include polyamide 6T, polyamide 9T, polyamide 10T, polyamide 6I, polyamide 9I, polyamide 6T / 6I, and polyamide 9T / 9I.
[0104] Regarding the content of the polyamide resin other than the polyamide resin A and the polyamide resin B in the resin composition of the present embodiment, when all the polyamide resins are set to 100 parts by mass, it is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, further preferably 1 part by mass or less, and can also be 0.1 parts by mass or less, 0.01 parts by mass or less, or 0.001 parts by mass or less. The lower limit of the content of the polyamide resin other than the polyamide resin A and the polyamide resin B can also be 0 parts by mass.
[0105] Regarding the content of the aliphatic polyamide resin in the resin composition of the present embodiment, when all the polyamide resins are set to 100 parts by mass, it is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, further preferably 1 part by mass or less, and can also be less than 0.1 parts by mass, 0.01 parts by mass or less, or 0.001 parts by mass or less. The lower limit of the content of the aliphatic polyamide resin can also be 0 parts by mass.
[0106] The total content of polyamide 6 and polyamide 66 in the resin composition of the present embodiment is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and further preferably 1 part by mass or less, and may be less than 0.1 parts by mass, 0.05 parts by mass or less, 0.01 parts by mass or less, or 0.001 parts by mass or less, based on 100 parts by mass of all polyamide resins. The lower limit of the total content of polyamide 6 and polyamide 66 may also be 0 parts by mass.
[0107] <Difference in half-crystallization time of resin composition>
[0108] The difference between the semi-crystallization time at 110° C. and the semi-crystallization time at 150° C. of the resin composition of the present embodiment is preferably 12.0 seconds or less, more preferably 10.0 seconds or less, further preferably 8.0 seconds or less, further preferably 5.0 seconds or less, further preferably 2.0 seconds or less, and further more preferably 1.0 second or less. The lower limit of the difference between the semi-crystallization time at 110° C. and the semi-crystallization time at 150° C. is ideally 0 seconds, but it is more practical to be 0.01 seconds or more.
[0109] <Method for producing resin composition>
[0110] The resin composition of the present embodiment can be produced by a known method for producing a thermoplastic resin composition.
[0111] As one embodiment of the method for producing the resin composition of the present embodiment, it is preferred that the polyamide resin A, the polyamide resin B, and other components blended as required are blended and kneaded. An example of such a resin composition is a pellet.
[0112] Specifically, polyamide resin A, polyamide resin B and other components mixed as required are for example pre-mixed using various mixers such as barrel mixer, Henschel mixer (Henschel mixer), by Banbury mixer (Banbury mixer), roller, Brabender mixer, single screw mixing extruder, twin screw mixing extruder, kneader and other mixers to carry out the method for melt mixing. Reinforcement material is preferably supplied from the midway of extruder, to suppress the fragmentation during mixing. In addition, more than two components can also be selected from each component to mix in advance, mix.
[0113] When the polyamide resin B is fed into the extruder, its shape includes powder and pellets. More specifically, the polyamide resin B is preferably a solid having a size of 5 μm or more, more preferably 10 μm or more, particularly preferably 15 μm or more, and preferably 100 μm or less.
[0114] The temperature (e.g., the set temperature of the extruder) when the resin composition of the present embodiment is melt-kneaded is preferably 320°C or less, more preferably 290°C or less, further preferably 280°C or less, more preferably 275°C or less, and further preferably 265°C or less. In addition, the temperature during the melt-kneading is preferably 240°C or more, more preferably 245°C or more, further preferably 250°C or more, and further preferably 255°C or more. By setting it to the above lower limit value or more, there is a tendency for the dispersibility to become good.
[0115] <Molding products>
[0116] The molded article of the present embodiment is formed from the resin composition of the present embodiment.
[0117] The method for producing the molded article of the present embodiment is not particularly limited.
[0118] For example, the molded article of the present embodiment may be formed directly by various molding methods after melt-kneading the components, or may be formed by melt-kneading the components and pelletizing them, then melt-kneading them again, and then forming them by various molding methods.
[0119] There are no particular restrictions on the method for molding the molded product, and a conventionally known molding method can be used, such as injection molding, injection compression molding, extrusion molding, profile extrusion, transfer molding, hollow molding, gas-assisted hollow molding, blow molding, extrusion blow molding, IMC (in-mold coating) molding, rotational molding, multilayer molding, two-color molding, insert molding, sandwich molding, foaming molding, press molding, etc., preferably injection molding.
[0120] The resin composition of the present embodiment is preferably molded using a method using a mold such as injection molding, and is particularly preferably molded at a low mold temperature. An example of a method for manufacturing a molded product of the present embodiment is a method for manufacturing a molded product as follows: comprising molding the resin composition of the present embodiment using a mold, and the mold temperature is less than 100°C (preferably 80 to 99°C).
[0121] Furthermore, the resin composition of the present embodiment is preferably subjected to injection molding. The barrel temperature during the aforementioned injection molding is preferably less than the melting point of polyamide resin B ℃, more preferably below the melting point of polyamide resin B -5 ℃, further preferably less than the melting point of polyamide resin B -10 ℃, more preferably below the melting point of polyamide resin B -15 ℃, and even more preferably below the melting point of polyamide resin B -20 ℃. By setting it below the aforementioned upper limit value, polyamide resin B can be dispersed in a more non-melting state. In addition, the barrel temperature during the aforementioned injection molding is preferably above the melting point of polyamide resin A + 10 ℃, more preferably above the melting point of polyamide resin A + 15 ℃, further preferably above the melting point of polyamide resin A + 20 ℃, and even more preferably above the melting point of polyamide resin A + 25 ℃.
[0122] The cylinder temperature in this embodiment refers to the set temperature of the injection molding machine.
[0123] Furthermore, in the method for manufacturing a molded article of the present embodiment, it is preferred that, in the resin composition immediately before being injected into the injection molding mold, the polyamide resin A is melted and at least a portion of the polyamide resin B is not melted. By setting such a configuration, the polyamide resin B can play an effect as a crystallization nucleating agent and can shorten the semi-crystallization time. Such a condition is achieved by setting the barrel temperature during injection molding to the melting point of the polyamide resin A+20°C or more and less than the melting point of the polyamide resin B.
[0124] It should be noted that the polyamide resin A being melted includes not only the case where it is 100% completely melted but also the case where it is recognized as melted by a person skilled in the art of the present invention. For example, the case where the polyamide resin A contains a small amount of unmelted parts is equivalent to being melted.
[0125] In addition, the polyamide resin B is preferably partially unmelted, and preferably 50 mass % or more of the polyamide resin B is unmelted. The polyamide resin B is preferably present in the resin composition during molding in a state such as a powder or pellet.
[0126] In the molded article of the present embodiment, it is preferred that the polyamide resin B is present in the polyamide resin A as a solid having a size of, for example, 5 μm or more, further 10 μm or more, particularly 15 μm or more, and further 100 μm or less. By dispersing the polyamide resin B in the polyamide resin A with such a size, there is a tendency to more effectively exert the effect of the present invention. It should be noted that in the present embodiment, during the melt kneading of the polyamide resin A and the polyamide resin B, the polyamide resin B may also be completely melted. In the present embodiment, it is ideal that at least a portion of the polyamide resin B exists in an unmelted state during molding.
[0127] The shape of the molded product of this embodiment is not particularly limited and can be appropriately selected according to the use and purpose of the molded product. For example, the shape includes: plate-shaped, plate-shaped, rod-shaped, thin sheet-shaped, film-shaped, cylindrical, ring-shaped, circular, elliptical, gear-shaped, polygonal, irregular, hollow, frame-shaped, box-shaped, panel-shaped, etc.
[0128] There is no particular limitation on the application field of the molded product of this embodiment, and the molded product can be widely used in transportation machinery parts such as automobiles, general machinery parts, precision machinery parts, electronic and electrical equipment parts, OA equipment parts, building materials and housing equipment related parts, medical devices, leisure and sports goods, game equipment, medical products, daily necessities such as food packaging films, national defense and aerospace products, etc.
[0129] Example
[0130] The present invention is described in more detail below by enumerating examples. The materials, usage amounts, ratios, processing contents, processing steps, etc. shown in the following examples can be appropriately changed without departing from the gist of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below.
[0131] When the measuring device used in the examples is difficult to obtain due to discontinuation of production or the like, another device having the same performance may be used for measurement.
[0132] 1. Raw materials
[0133] <Synthesis of MP10 (70 / 30)>
[0134] Sebacic acid (manufactured by CASDA) was added to a jacketed reactor equipped with a stirrer, a partial condenser, a cooler, a thermometer, a drip tank, and a nitrogen inlet pipe, and the atmosphere was fully replaced with nitrogen. After heating and melting at 170°C, a mixed amine of m-xylylenediamine and p-xylylenediamine (molar ratio: 70:30) (manufactured by Mitsubishi Gas Chemical Co., Ltd., MPXDA) was slowly dripped in a molar ratio of 1:1 with sebacic acid while stirring the contents, and the temperature was raised to 240°C. After the dripping was completed, the internal temperature was raised to 260°C and maintained for 20 minutes. Then, the internal pressure of the reaction system was continuously reduced to 0.08 MPa, and the reaction was continued. After the reaction was completed, a pressure of 0.2 MPa was applied to the reactor with nitrogen, and the polymer was taken out from the nozzle at the bottom of the polymerization tank in the form of strands, and after water cooling, it was pelletized by a pelletizer to obtain.
[0135] The melting point of the obtained MP10 (70 / 30) was 215°C.
[0136] <Synthesis of MP10 (60 / 40)>
[0137] The above-mentioned <Synthesis of MP10 (70 / 30)> was carried out in the same manner except that the molar ratio of the mixed amine of meta-xylylenediamine and para-xylylenediamine was changed to 60 / 40.
[0138] The melting point of the obtained MP10 (60 / 40) was 223°C.
[0139] <Synthesis of MXD10>
[0140] Sebacic acid (manufactured by CASDA) was added to a jacketed reactor equipped with a stirrer, a partial condenser, a cooler, a thermometer, a drip tank, and a nitrogen inlet pipe, and the atmosphere was fully replaced with nitrogen. After heating and melting at 170°C, meta-xylylenediamine (manufactured by Mitsubishi Gas Chemical Co., Ltd., MXDA) was slowly dripped in a molar ratio of 1:1 with sebacic acid while stirring the contents, and the temperature was raised to 240°C. After the dripping was completed, the temperature was raised to 260°C and continued for 20 minutes. Then, the pressure in the reaction system was continuously reduced to 0.08 MPa, and the reaction was continued. After the reaction was completed, a pressure of 0.2 MPa was applied to the reactor with nitrogen, so that the polymer was taken out from the nozzle at the bottom of the polymerization tank in the form of strands, and after water cooling, it was pelletized by a pelletizer to obtain it.
[0141] The melting point of the obtained MXD10 was 190°C.
[0142] <Synthesis of MP6 (70 / 30)>
[0143] Into a jacketed reactor equipped with a stirrer, a partial condenser, a cooler, a thermometer, a dropping tank and a nitrogen inlet pipe, 7220 g (49.4 mol) of adipic acid (produced by Roadia) and 11.66 g of sodium acetate / sodium hypophosphite monohydrate (molar ratio = 1 / 1.5) were added, the atmosphere was fully replaced with nitrogen, and the mixture was heated and melted at 170°C. Then, while the contents were stirred, 6647 g of a mixed xylylenediamine (34.16 mol of m-xylylenediamine and 14.64 mol of p-xylylenediamine, produced by Mitsubishi Gas Chemical Co., Ltd.) having a molar ratio of m-xylylenediamine to p-xylylenediamine of 70 / 30 was added dropwise to the melt in the reaction vessel under stirring, and the generated condensation water was discharged to the outside of the system while the internal temperature was continuously raised to 260°C over 2.5 hours. After the dropwise addition was completed, the internal temperature was raised, and when it reached 270° C., the pressure in the reaction vessel was reduced, and the internal temperature was further raised, and the melt polycondensation reaction was continued at 280° C. for 20 minutes. Then, the system was pressurized with nitrogen, and the obtained polymer was taken out from the strand die and pelletized to obtain a polyamide resin.
[0144] The melting point of the obtained MP6 was 258°C.
[0145] <Synthesis of PXD10>
[0146] Sebacic acid (manufactured by CASDA) was added to a jacketed reactor equipped with a stirrer, a partial condenser, a cooler, a thermometer, a dropping tank, and a nitrogen inlet pipe, and the atmosphere was fully replaced with nitrogen. After heating and melting at 170°C, p-phenylenediamine (manufactured by Showa Denko, PXDA) was slowly added dropwise in a molar ratio of 1:1 with sebacic acid while stirring the contents, and the temperature was raised to 290°C. After the addition was completed, the internal temperature was raised to 300°C and maintained for 20 minutes. Then, the internal pressure of the reaction system was continuously reduced to 0.08 MPa, and the reaction was continued for 20 minutes. After the reaction was completed, a pressure of 0.2 MPa was applied to the reactor with nitrogen, so that the polymer was taken out from the nozzle at the bottom of the polymerization tank in the form of strands, and after water cooling, it was pelletized by a pelletizer to obtain it.
[0147] The melting points of the obtained PXD10 were 280° C. and 290° C. In this example, the higher melting point was treated as Tmb=290° C.
[0148] <Inorganic crystal nucleating agent>
[0149] Talc: Micron White 5000S manufactured by Lin Huacheng Co., Ltd.
[0150] <Reinforcement materials>
[0151] Glass fiber (GF): round cross-section glass fiber, manufactured by Nippon Electric Glass Co., Ltd., T-275H, E glass, chopped strand mat, number average fiber diameter 10 μm
[0152] <Determination of Melting Point of Polyamide Resin>
[0153] Using a differential scanning calorimeter (DSC), 5 mg of the obtained polyamide resin pellets were cut into 1-3 mm lengths with scissors, nitrogen was passed as an atmosphere gas at 50 mL / min, and the mixture was heated from room temperature to a temperature of the expected melting point + 20°C to 30°C at a heating rate of 10°C / min. After rapid cooling, the mixture was heated again from room temperature to a temperature of the expected melting point + 20°C to 30°C at a heating rate of 10°C / min. The melting point was determined from the peak top temperature of the endothermic peak observed during melting.
[0154] A differential scanning calorimeter (DSC) was used, DSC-60 manufactured by SHIMADZU CORPORATION.
[0155] 2. Examples 1 to 9, Comparative Examples 1 to 4, Reference Examples 1 to 4
[0156] <Mixed>
[0157] In order to form the composition shown in Table 1 or Table 2 described later, each component (the compounding amount of each component is expressed in parts by mass) is weighed respectively, and after dry mixing, a twin-screw weight-loss feeder (Cassette Weighing Feeder) (KUBOTA Corporation. system, CE-W-1-MP) is used to feed from the screw root of a twin-screw extruder (TEM26SS made by Shibaura Machinery Co., Ltd.). In addition, for glass fiber, a vibration-type weight-loss feeder (KUBOTA Corporation. system, CE-V-1B-MP) is used to feed from the side of the extruder into the above-mentioned twin-screw extruder, and melt-mixed with a thermoplastic resin component, etc. to obtain a resin composition (pellet). The temperature setting of the extruder is set to the temperature shown in Table 1 or Table 2. In addition, in Table 1 or Table 2, in the embodiment or comparative example where the polyamide resin (B) is recorded as "25 μm powder", it means that PXD10 in a powder form with an average diameter of 25 μm is fed into the extruder, and in the embodiment or comparative example where it is recorded as "pellet", it means that PXD10 in the form of pellets is directly fed into the extruder.
[0158] <Crystallization during injection molding (crystallization temperature in the mold)>
[0159] After drying the pellets obtained above at 120°C for 8 hours, the pellets were injection molded by an injection molding machine (SE130DU manufactured by Sumitomo Heavy Industries) at the conditions of the barrel temperature and mold temperature of 80°C or 90°C as described in Table 1 or Table 2 to form plates of 100 mm in length and 60 mm in width, and three sections of plates of 3 mm in thickness (40 mm in length), 2 mm in thickness (30 mm in length), and 1 mm in thickness (30 mm in length). Then, the 1 mm thick portion was determined by the presence or absence of crystallization heat when the temperature was raised at 10°C / min using DSC-60 (manufactured by Shimadzu Corporation) to determine whether crystallization occurred.
[0160] A: Crystallization heat is 0.1 J / g or more (crystallization occurs at 80°C or 90°C)
[0161] B: Crystallization heat is less than 0.1 J / g (no crystallization at 80°C or 90°C)
[0162] <Half crystallization time of resin composition>
[0163] The obtained resin composition (pellets) was used to prepare a 0.1 mm thick film-shaped sample, which was sandwiched between a glass slide. The sample was placed in an air bath set at the melting point + 20°C for 3 minutes. Then, the sample was placed between the light from the light source of the oil bath set at the measurement temperature, which passed through the polarizing plate and reached the sensor, and the half-crystallization time at 110°C and 150°C was calculated from the voltage difference before and after crystallization.
[0164] Furthermore, the difference between the half crystallization time at 110°C and the half crystallization time at 150°C was calculated.
[0165] <Charpy impact strength with notch>
[0166] The pellets obtained above were dried at 120°C for 4 hours and then injection molded into ISO tensile test pieces (4 mm thick) using an injection molding machine (NEX140III, manufactured by Nissei Plastic Industries, Ltd.) at the injection molding temperature (cylinder temperature) shown in Table 1 or Table 2 and a mold temperature of 110°C.
[0167] The notched Charpy impact strength (unit: kJ / m) was measured using the ISO tensile test piece (4 mm thick) in an environment of 23°C and 50% humidity using a 1J hammer according to ISO179-1 and 2. 2 ). The results are shown in Table 1 or Table 2.
[0168] <Retention rate of Charpy impact strength>
[0169] The retention rate of Charpy impact strength was measured compared with the case where the polyamide resin B and the inorganic crystal nucleating agent (Micron White) were not added.
[0170] In each example and comparative example, the resin composition (pellets) was obtained in the same manner except that the polyamide resin B and the inorganic crystal nucleating agent were not blended. Furthermore, the notched Charpy impact strength was measured in the same manner as above using the obtained pellets.
[0171] The retention rate of Charpy impact strength compared with the case where the polyamide resin B and the inorganic crystal nucleating agent (Micron White) were not added was calculated (unit: %).
[0172] Retention rate = [Charpy impact strength of a molded article molded from the resin composition of the example or comparative example / Charpy impact strength of a molded article molded from a composition obtained by excluding the polyamide resin B and the inorganic crystal nucleating agent from the resin composition of the example or comparative example] × 100
[0173] <Dispersion size of PXD10>
[0174] The test piece prepared above was cut into a thickness of 5 μm to 10 μm using an ultramicrotome (manufactured by Leica), and the dispersion size of PXD10 was measured using a digital microscope (manufactured by KEYENCE).
[0175] [Table 1]
[0176]
[0177] [Table 2]
[0178]
[0179] In the above Table 1 or Table 2, the MXDA / PXDA ratio represents a molar ratio.
[0180] From the above results, it is clear that the resin composition of the present invention has a high crystallization rate, the obtained molded article has a small decrease in physical properties, and the crystallization rate is less likely to depend on the mold temperature (Examples 1 to 9).
[0181] On the other hand, when polyamide 66 was used instead of polyamide resin B (Comparative Example 1), the half crystallization time changed significantly depending on the mold temperature.
[0182] In the case where 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin A are not derived from α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms (Comparative Examples 2 and 3), the half crystallization time greatly changes depending on the mold temperature.
[0183] Furthermore, when the polyamide resin B was not blended (Reference Examples 1 to 4), the half crystallization time greatly changed depending on the mold temperature.
[0184] On the other hand, when talc was blended even without blending the polyamide resin B (Comparative Example 4), although the half crystallization time did not depend on the mold temperature, the property retention rate decreased significantly.
[0185] In the molded article formed from the resin composition of the present invention, PXD10 is dispersed and it can be said that PXD10 is not melted in the resin composition immediately before injection into the injection molding mold (inside the cylinder).
Claims
1. A resin composition comprising a polyamide resin A and a polyamide resin B, The polyamide resin A and the polyamide resin B contain 1 to 15 parts by mass of the polyamide resin B relative to 100 parts by mass of the total of the polyamide resin A and the polyamide resin B. The difference Tmb-Tma between the melting point Tmb of the polyamide resin B measured by differential scanning calorimetry DSC and the melting point Tma of the polyamide resin A measured by differential scanning calorimetry DSC is 35 to 110° C., The polyamide resin A comprises a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, wherein the diamine-derived structural unit comprises 100 to 50 mol % of a meta-xylylenediamine-derived structural unit and 0 to 50 mol % of a para-xylylenediamine-derived structural unit, wherein: The total amount of the structural unit derived from m-xylylenediamine and the structural unit derived from p-xylylenediamine does not exceed 100 mol%, and 70 mol% or more of the structural unit derived from the dicarboxylic acid is derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms, The polyamide resin B comprises a structural unit derived from a diamine and a structural unit derived from a dicarboxylic acid, wherein the structural unit derived from the diamine comprises 100 to 95 mol % of a structural unit derived from p-xylylenediamine and 0 to 5 mol % of a structural unit derived from m-xylylenediamine, wherein the total of the structural unit derived from p-xylylenediamine and the structural unit derived from m-xylylenediamine does not exceed 100 mol %, and 70 mol % or more of the structural unit derived from the dicarboxylic acid is derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 7 to 16 carbon atoms.
2. The resin composition according to claim 1, wherein The melting point Tma of the polyamide resin A measured by differential scanning calorimetry (DSC) is 180 to 240°C.
3. The resin composition according to claim 1 or 2, wherein 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin A are derived from sebacic acid.
4. The resin composition according to any one of claims 1 to 3, wherein The melting point Tmb of the polyamide resin B measured by differential scanning calorimetry (DSC) is 270 to 320°C.
5. The resin composition according to any one of claims 1 to 4, wherein 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin B are derived from sebacic acid.
6. The resin composition according to claim 1, wherein The melting point Tma of the polyamide resin A measured by differential scanning calorimetry (DSC) is 180 to 240° C. At least 70 mol% of the structural units derived from dicarboxylic acid in the polyamide resin A are derived from sebacic acid, The melting point Tmb of the polyamide resin B measured by differential scanning calorimetry (DSC) is 270 to 320° C. 70 mol% or more of the structural units derived from dicarboxylic acid in the polyamide resin B are derived from sebacic acid.
7. The resin composition according to any one of claims 1 to 6, wherein The polyamide resin A and the polyamide resin B may contain 10 to 150 parts by mass of a reinforcing material relative to 100 parts by mass of the total. 8 . A molded article formed from the resin composition according to claim 1 . 9 . A method for producing a molded article, comprising injection molding the resin composition according to claim 1 .
10. The method for producing a molded article according to claim 9, wherein: The cylinder temperature during the injection molding is greater than or equal to the melting point of the polyamide resin A+20° C. and less than the melting point of the polyamide resin B.
11. The method for producing a molded article according to claim 9 or 10, wherein: In the resin composition immediately before being injected into the injection molding die, the polyamide resin A is melted, and at least a part of the polyamide resin B is not melted.