By using a sintered heat transfer component made of fluorine-based resin or fluorine-based elastomer, the problem of insufficient heat transfer in the plasma processing device is solved, high plasma resistance and long-term maintenance of adhesiveness is achieved, and the temperature stability is improved and processing efficiency.

CN118946955APending Publication Date: 2024-11-12MITSUBISHI MATERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030371.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-02-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing plasma processing device, the plasma resistance of the heat transfer component is low and the adhesion is difficult to maintain for a long time, resulting in insufficient heat transfer between parts in the chamber and affecting temperature stability.

Method used

Using sintered heat transfer parts made of fluorine-based resin or fluorine-based elastomer molded products, the plasma resistance and thermal stability of heat transfer parts are improved by controlling hardness and filler selection, thereby enhancing the adhesion between parts. .

Benefits of technology

It achieves long-term maintenance of high heat transfer and temperature stability in a vacuum environment, and improves the efficiency and reliability of the plasma processing device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946955A_ABST
    Figure CN118946955A_ABST
Patent Text Reader

Abstract

The heat transfer member is composed of a fired body of a molded article comprising a fluorine-based resin or a fluorine-based elastomer, and the hardness of the heat transfer member measured using an AM-type durometer in accordance with JIS K 6253-3: 2012 is 7 or more lower than the hardness of the molded article. The heat transfer member has high plasma resistance and can maintain a state of high adhesion to various members for a long period of time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a heat transfer component, a method for manufacturing the heat transfer component and a plasma processing device.

[0002] This application claims priority based on patent application No. 2022-057297 applied for in Japan on March 30, 2022, and its content is cited here. Background Art

[0003] When plasma processing is performed in a plasma processing device, the chamber is kept in a vacuum state. Therefore, there is a problem that the heat transfer between the parts in the chamber is low and it takes time for the temperature of each part to stabilize. Therefore, a solution of arranging a heat transfer component between the parts in the chamber is being studied.

[0004] For example, Patent Documents 1 and 2 propose to dispose a heat transfer component between an electrode for a plasma processing device and a cooling plate or between a focus ring in a chamber of a plasma processing device and its support frame. Patent Document 1 proposes to use a flexible heat transfer sheet as a heat transfer component, and describes heat-resistant silicone rubber as a flexible heat transfer sheet. Furthermore, Patent Document 2 proposes to use a fluorine-based resin or a fluorine-based elastomer as a heat transfer component.

[0005] Patent Document 1: Japanese Patent No. 5619486

[0006] Patent Document 2: Japanese Patent Application Publication No. 2021-141314

[0007] In order to improve the heat transfer between the parts in the chamber of the plasma treatment device, it is effective to improve the adhesion between the parts and the heat transfer parts by improving the flexibility of the heat transfer parts. However, as a heat transfer part with flexibility, the silicone rubber used in the past has the problem of low plasma resistance. When the heat transfer parts with low plasma resistance are used for the parts in the chamber of the plasma treatment device, there is a possibility that the adhesion with the parts will be reduced due to deterioration over time. On the other hand, although fluorine-based resins or fluorine-based elastomers have high plasma resistance, in order to improve the heat transfer characteristics, it is required to further improve the adhesion with various parts. Summary of the invention

[0008] The present invention has been completed in view of the above-mentioned situation, and its purpose is to provide a heat transfer component and its manufacturing method that have high plasma resistance and can maintain a high degree of adhesion with various components for a long time, as well as a plasma processing device that can easily stabilize the temperature of various parts in the chamber even when the chamber is in a vacuum state.

[0009] In order to solve the above-mentioned problems, the present invention includes the following means.

[0010] [Scheme 1] The heat transfer component involved in Scheme 1 of the present invention is constructed as follows: it is a heat transfer component composed of a sintered body of a molded product containing a fluorine-based resin or a fluorine-based elastomer, and the hardness of the heat transfer component measured using an AM type hardness tester in accordance with JIS K 6253-3:2012 is lower than the hardness of the molded product by at least 7.

[0011] According to the heat transfer component of scheme 1, since it contains fluorine resin and / or fluorine elastomer, it has high plasma resistance. In addition, the heat transfer component of the present invention is a sintered body, and the hardness AM value is lower than the hardness AM value of the molded product before sintering by more than 7, and the hardness is low and the flexibility is increased. Therefore, according to the heat transfer component of the present invention, the close contact between the heat transfer component and various parts is improved.

[0012] [Structure 2] Regarding the heat transfer component of Structure 2, in Structure 1, the molded product contains a filler. In this case, it is desirable that the heat conductivity of the filler is higher than that of the fluorine-based resin and the fluorine-based elastomer.

[0013] According to the heat transfer member of the second aspect, since the heat transfer property of the filler is higher than that of the fluorine-based resin and the fluorine-based elastomer, the heat transfer property of the heat transfer member is further improved.

[0014] [Scheme 3] Regarding the heat transfer component of scheme 3 of the present invention, in scheme 2, the filler is at least one inorganic substance selected from alumina, aluminum nitride, boron nitride and silicon. In this case, since the filler is the above-mentioned inorganic substance, the heat transfer performance of the heat transfer component is further improved.

[0015] [Scheme 4] The heat transfer component of scheme 4 of the present invention is a heat transfer component composed of a molded body containing a fluorine-based resin and / or a fluorine-based elastomer, and when heated at 250°C for 25 hours and the hardness is measured before and after the heating using an AM type hardness tester in accordance with JIS K6253-3:2012, the change in hardness from before heating to after heating (hardness after heating - hardness before heating) is within the range of ±5. The atmosphere during the heating treatment is in normal pressure air or in an inert gas such as nitrogen, and the temperature of the heat transfer component during the hardness measurement is room temperature.

[0016] Since the heat transfer component of Scheme 4 contains fluorine-based resin and / or fluorine-based elastomer, it has high plasma resistance. In addition, since the change in the hardness of the heat transfer component of Scheme 4 after heating at 250°C for 25 hours is within the range of ±5, the heat transfer component has high thermal stability and the flexibility of the heat transfer component becomes higher. Therefore, according to the heat transfer component of Scheme 4, the adhesion between the heat transfer component and various parts is improved. In addition, since the heat transfer component of Scheme 4 has high thermal stability, it is possible to maintain a high adhesion state with various components for a long time even in a high temperature environment such as in a chamber of a plasma processing device. The heat transfer component of Scheme 4 can also meet the necessary conditions of the heat transfer component of Scheme 1.

[0017] [Scheme 5] Regarding the heat transfer component of scheme 5, the molded body may be configured to include a filler in scheme 4. In this case, since the heat conductivity of the filler is higher than that of the fluorine-based resin and the fluorine-based elastomer, the heat conductivity of the heat transfer component is further improved.

[0018] [Scheme 6] Regarding the heat transfer component of scheme 6, in scheme 5, the filler may be composed of at least one inorganic substance selected from alumina, aluminum nitride, boron nitride and silicon. In this case, since the filler is the above-mentioned inorganic substance, the heat transfer performance of the heat transfer component is further improved.

[0019] The content of the fluorine-based resin and / or the fluorine-based elastomer in the heat transfer component of Schemes 1 to 6 is not limited, but may be 10% by volume or more and 100% by volume or less, preferably 20% by volume or more and 80% by volume or less, and more preferably 40% by volume or more and 60% by volume or less. When the content of the fluorine-based resin or the fluorine-based elastomer is 20% by volume or more, it is easy to fully improve the plasma resistance, and it is easier to maintain a high degree of adhesion with various components for a long time.

[0020] Although the shape of the heat transfer component of Schemes 1 to 6 is not limited, it can be, for example, a sheet or plate shape. In this case, the heat transfer component can also be called a heat transfer sheet or a heat transfer plate. The thickness of the heat transfer component can be, for example, in the range of 20 μm to 1 mm, or in the range of 20 μm to 500 μm. The planar shape of the heat transfer component only needs to correspond to the planar shape of the boundary surface to be heat transferred. In order to improve the heat transfer characteristics, the pores in the heat transfer component are preferably less than 1 volume %, and more preferably 0 volume %.

[0021] The content of the filler in the heat transfer component of Schemes 2, 3, 5 and 6 is not limited, but may be in the range of 30% by volume or more and 90% by volume or less, more preferably in the range of 60% by volume or more and 90% by volume or less. The heat transfer component of Scheme 2 may be composed only of a fluorine-based resin and / or a fluorine-based elastomer and the filler, and may contain 10% by volume or less, more preferably 5% by volume or less of a vulcanizing agent and / or a plasticizer, etc.

[0022] [Scheme 7] The method for manufacturing a heat transfer component of Scheme 7 of the present invention is a method for manufacturing a heat transfer component comprising a fluorine-based resin or a fluorine-based elastomer, characterized in that it includes: a molding step, heating and molding the material comprising the fluorine-based resin or the fluorine-based elastomer to produce a molded product; and a firing step, firing the molded product to produce a softened fired body having a hardness of at least 7 lower than the hardness of the molded product measured by an AM type hardness tester in accordance with JIS K 6253-3:2012, wherein the heat transfer component is composed of the softened fired body.

[0023] According to the method for manufacturing a heat transfer component of claim 7, since the molded product obtained in the molding step is fired under the above-mentioned conditions in the firing step, a heat transfer component having high plasma resistance and capable of maintaining high adhesion to various components for a long period of time can be manufactured industrially advantageously. The method for manufacturing a heat transfer component of claim 7 can manufacture the heat transfer components of claims 1 to 6.

[0024] [Scheme 8] Regarding the manufacturing method of the heat transfer component of Scheme 8, in Scheme 7, it includes: a preparatory step, sintering the molded object under multiple conditions of one or both of temperature and time to obtain multiple sintered bodies, using an AM type hardness tester in accordance with JISK 6253-3:2012 to measure the hardness of the multiple sintered bodies obtained, comparing the hardness of the molded object and the hardness of the multiple sintered bodies, thereby determining the sintering temperature and sintering time that can obtain the softened sintered body whose hardness is 7 or more lower than the hardness of the molded object, and in the sintering step, sintering the molded object at the sintering temperature and sintering time determined in the preparatory step to produce the softened sintered body.

[0025] In the method for manufacturing a heat transfer component of Scheme 8, since the molded product is fired in the firing step using the firing temperature and firing time determined in the preparatory step, a heat transfer component having a hardness lower than the hardness of the molded product by 7 or more can be manufactured stably over a long period of time with a high probability. The method for manufacturing a heat transfer component of Schemes 1 to 6 can be manufactured by the method for manufacturing a heat transfer component of Schemes 8.

[0026] [Scheme 9] The plasma processing device of Scheme 9 of the present invention comprises: an electrode for a plasma processing device, having a vent hole for allowing a gas for plasma generation to pass; and a cooling plate, wherein a heat transfer component described in any one of Scheme 6 is arranged at least in a portion between the electrode for the plasma processing device and the cooling plate.

[0027] The plasma processing device of Scheme 9 is provided with a heat transfer component at least partially between the plasma processing device electrode and the cooling plate, so that the heat of the plasma processing device electrode heated by plasma can be efficiently transferred to the cooling plate. Therefore, it is easy to ensure the thermal uniformity of the plasma processing device electrode for a long time. The plasma processing device can also be called a plasma etching device.

[0028] [Scheme 10] Regarding the plasma processing device of scheme 10, in scheme 9, the electrode for the plasma processing device can be directly joined to the heat transfer component described in any one of schemes 1 to 6.

[0029] In the plasma processing apparatus of claim 10, by directly joining the plasma processing apparatus electrode to the heat transfer member, the heat of the plasma processing apparatus electrode can be transferred to the cooling plate with higher efficiency.

[0030] [Scheme 11] Regarding the plasma processing device of Scheme 11, in Scheme 9 or Scheme 10, it has a focusing ring and a support frame supporting the focusing ring, and a heat transfer component described in any one of Schemes 1 to 6 is arranged at least in a portion between the focusing ring and the support frame.

[0031] In the plasma processing apparatus of claim 11, since a heat transfer member is disposed at least partially between the focus ring and the support frame, the heat of the focus ring heated by plasma can be efficiently transferred to the support frame. Therefore, it is easy to perform plasma processing on the object to be processed stably for a long time.

[0032] [Solution 12] Regarding the plasma processing apparatus of Solution 12, in any one of Solutions 9 to 11, the focus ring is directly bonded to the heat transfer member. In this case, since the focus ring is directly bonded to the heat transfer member, the heat of the focus ring can be transferred to the cooling plate with higher efficiency.

[0033] As described above, according to the various schemes of the present invention, there can be provided a heat transfer component having high plasma resistance and capable of maintaining a high degree of adhesion with various components for a long period of time, and a method for manufacturing the heat transfer component, as well as a plasma processing device in which the temperature of each part in the chamber can be easily stabilized even when the chamber is in a vacuum state. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1This is a flowchart showing a method for manufacturing a heat transfer member according to one embodiment of the present invention.

[0035] Figure 2 It is a longitudinal sectional view showing a plasma processing apparatus according to one embodiment of the present invention. DETAILED DESCRIPTION

[0036] Hereinafter, a heat transfer member, a method for manufacturing the same, and a plasma processing apparatus according to embodiments of the present invention will be described with reference to the drawings.

[0037] The plasma processing device involved in the present embodiment is, for example, a plasma processing device such as a plasma etching device or a plasma CVD device used in a semiconductor device manufacturing process. The heat transfer component involved in the present embodiment is used, for example, as: a heat transfer component arranged between an electrode for a plasma processing device having a vent hole for passing a gas for plasma generation and a cooling plate to transfer the heat of the electrode for the plasma processing device to the cooling plate; and / or a heat transfer component arranged between a focusing ring and a support frame supporting the focusing ring to transfer the heat of the focusing ring to the cooling plate. However, the uses of the heat transfer component involved in the present invention are not limited to these, and the heat transfer component of the present invention can be arranged and used as long as it is located between two components arranged inside a plasma processing device that should transfer heat to each other.

[0038] <Heat transfer parts>

[0039] (First Embodiment)

[0040] The heat transfer component involved in the first embodiment of the present invention is composed of a sintered body of a molded product containing a fluorine-based resin or a fluorine-based elastomer. The molded product is formed in a shape that can be used as a heat transfer component. The molded product of this embodiment is a sintered body obtained by sintering the above-mentioned molded product. The manufacturing method of the molded product and the sintering method of the molded product will be described later.

[0041] The use of the heat transfer component (sintered body) complies with JIS K 6253-3 (Vulcanized rubber and thermoplastic rubber - Method for determining hardness - Part 3: Durometer hardness): The hardness value measured by the AM type hardness meter of 2012 (hereinafter referred to as "hardness AM" in this specification) is 7 or more lower than the hardness AM value of the above-mentioned molded product. That is, the heat transfer component involved in the first embodiment has a lower hardness and higher flexibility than the molded product. Therefore, the heat transfer component involved in the first embodiment can be deformed to match the surface shapes of various parts. As a hardness measurement method using an AM type hardness meter, it is sufficient to use the method described later.

[0042] The hardness AM of the heat transfer member is preferably within a range of 20 to 70. From the viewpoint of adhesion with other parts, the smaller the hardness AM of the heat transfer member, the better. Therefore, it is preferably 50 or less, and more preferably 30 or less.

[0043] The heat transfer component may contain a fluorine resin or a fluorine elastomer alone, or a mixture of a fluorine resin and a fluorine elastomer. The content of the fluorine resin and the fluorine elastomer in the heat transfer component is not limited, but may be 10% by volume or more and 100% by volume or less, preferably 20% by volume or more and 80% by volume or less, and more preferably 40% by volume or more and 60% by volume or less. When the content of the fluorine resin or the fluorine elastomer is 20% by volume or more, it is easy to fully improve the plasma resistance, and it is easier to maintain a high adhesion state with various components for a long time.

[0044] The heat transfer member preferably contains a filler. The heat transfer member preferably has a structure in which at least one of a fluorine-based resin and a fluorine-based elastomer as an organic component is used as a matrix binder and a filler component is dispersed in the matrix binder.

[0045] The fluorine-based resin is preferably a resin having a fluorine-containing group on the main chain. The fluorine-based resin may also be a gel-like resin having a three-dimensional crosslinked structure. The fluorine-based elastomer is preferably a fluorine-containing three-dimensional crosslinked compound having a fluorine-containing group and a three-dimensional crosslinked structure. Examples of the fluorine-containing group include perfluoroalkylene-(CF2) x -(x is an integer greater than 1) and a perfluoropolyether group. Examples of the perfluoropolyether group include -(CF2CF2O) m (CF2O) n -(m, n are integers greater than 1), -(CF2CF2CF2O) p -(p is an integer greater than or equal to 1), -(CF2CF(CF3)O) q -(q is an integer greater than or equal to 1), etc.

[0046] As the three-dimensional crosslinked structure, there can be mentioned an organosilicon structure having a silicon-carbon bond, a silicone structure having a siloxane bond, an epoxy structure having an epoxy bond, a polyurethane structure having a polyurethane bond, etc. A single fluorine-containing three-dimensional crosslinked compound can be used alone, or two or more can be used in combination. The fluorine-based elastomer is preferably a compound having a silicone structure composed of a perfluoropolyether skeleton and having a siloxane bond.

[0047] As materials for fillers, aluminum oxide (Al2O3), aluminum oxide hydrate, aluminum nitride (AlN), boron nitride (BN), silicon (Si), silicon dioxide (SiO2), silicon carbide (SiC), titanium oxide (TiO2), etc. can be used. Among these materials, aluminum oxide, aluminum nitride, boron nitride, and silicon are particularly preferred. The filler can be used alone or in combination of two or more. In addition, the two or more fillers can be two or more fillers with different materials, or can be fillers with the same material and physical properties such as average particle size (d50) of two or more. By using two or more fillers with different average particle sizes, the heat transfer component can be filled with fillers at a higher density. When using two or more fillers with different average particle sizes, the average particle size of the filler with a relatively large average particle size (large particle size filler) is preferably in the range of 1.5 times or more and 10 times or less of the average particle size of the filler with a relatively small average particle size (small particle size filler). More preferably, with respect to the average particle size, the average particle size of the large particle size filler can also be in the range of 2 times or more and 8 times or less of the average particle size of the small particle size filler.

[0048] The content of the filler component in the heat transfer component is preferably in the range of 30 volume % or more and 90 volume % or less, more preferably in the range of 60 volume % or more and 90 volume % or less. When the content of the filler component is 30 volume % or more, the heat transfer property of the heat transfer component is improved, and when the content of the filler component is 90 volume % or less, the shape stability of the heat transfer component is improved. The heat transfer component may be composed of only fluorine-based resin and / or fluorine-based elastomer and filler, and in addition to these, it may also contain a vulcanizing agent and / or a plasticizer, etc.

[0049] The shape of the heat transfer component may vary depending on the parts used, but it may be in the form of a sheet or a plate. In this case, it may also be called a heat transfer sheet or a heat transfer plate. The thickness of the heat transfer component is not limited, but may be, for example, in the range of 20 μm to 1 mm, or in the range of 20 μm to 500 μm. The planar shape of the heat transfer component may be a shape corresponding to the planar shape of the boundary surface to be heat transferred. In order to facilitate the use of the heat transfer component, a plastic release sheet may be attached to both sides of the heat transfer component in advance, and the heat transfer component may be used by peeling off the release sheet. Furthermore, an adhesive layer may be provided on the surface of the release sheet on the side of the heat transfer component, and the adhesive layer has a weaker adhesive force. The heat transfer component may be provided in the shape of a roll, or may be provided by being wound on any core material.

[0050] The heat transfer component of the present embodiment constructed as above has high plasma resistance because it contains fluorine resin or fluorine elastomer. In addition, the heat transfer component of the present embodiment is a sintered body, and the hardness AM value is lower than the hardness AM value of the molded product before sintering by more than 7, and the hardness is low and the flexibility is increased. Therefore, according to the heat transfer component of the present embodiment, the close contact between the heat transfer component and various parts is improved.

[0051] In the heat transfer component of this embodiment, when the molded article contains a filler, the heat transfer property of the heat transfer component is further improved. When the filler is at least one inorganic substance selected from alumina, aluminum nitride, boron nitride and silicon, the heat transfer property of the heat transfer component is further improved.

[0052] (Second Embodiment)

[0053] The heat transfer component involved in the second embodiment of the present invention is composed of a molded body containing a fluorine resin or a fluorine elastomer. The molded body can also be a sintered body of a molded product containing a fluorine resin or a fluorine elastomer. In this case, similarly to the heat transfer component of the first embodiment, the hardness AM of the sintered body can be lower than the hardness AM of the molded product by 7 or more.

[0054] Regarding the heat transfer component of the second embodiment, the change in hardness AM after heating at 250°C for 25 hours, that is, the value obtained by subtracting the hardness AM before heating from the hardness AM after heating at 250°C for 25 hours is within the range of ±5, so the thermal stability is high and it is fully softened. Due to the high thermal stability and sufficient softening, it is possible to maintain a high degree of adhesion with various components for a long time even in a high temperature environment such as in the chamber of a plasma processing device. The change in hardness AM after heating at 250°C for 25 hours is preferably within the range of ±3. The atmosphere during the heat treatment is in normal pressure air or in an inert gas such as nitrogen, and the temperature of the heat transfer component during the hardness measurement is room temperature.

[0055] The hardness AM of the heat transfer component is preferably within the range of 25 or more and 70 or less. Furthermore, the heat transfer component may contain a fluorine resin or a fluorine elastomer alone, or a mixture of a fluorine resin and a fluorine elastomer. The heat transfer component preferably contains a filler. The heat transfer component preferably has a structure in which at least one of the fluorine resin and the fluorine elastomer as organic components is used as a matrix adhesive and a filler component is dispersed in the matrix adhesive. The materials of the fluorine resin, the fluorine elastomer and the filler, the content of the filler component in the heat transfer component and the shape of the heat transfer component are the same as those of the first embodiment.

[0056] The heat transfer component of the present embodiment constructed as described above has high plasma resistance because it contains fluorine-based resin or fluorine-based elastomer. In addition, the heat transfer component of the present embodiment has high thermal stability and high flexibility because the change in hardness AM after heating at 250°C for 25 hours is within the range of ±5. Therefore, according to the heat transfer component of the present embodiment, the adhesion between the heat transfer component and various parts is improved. Furthermore, since the heat transfer component of the present embodiment has high thermal stability, it is possible to maintain a high adhesion state with various components for a long time even in a high temperature environment such as in a chamber of a plasma processing device.

[0057] In the heat transfer component of this embodiment, when the molded article contains a filler, the heat transfer property of the heat transfer component is further improved. When the filler is at least one inorganic substance selected from alumina, aluminum nitride, boron nitride and silicon, the heat transfer property of the heat transfer component is further improved.

[0058] <Method for manufacturing heat transfer component>

[0059] Next, a method for manufacturing the heat transfer member according to the present embodiment will be described.

[0060] Figure 1 1 is a flow chart showing a method for manufacturing a heat transfer component according to the present embodiment. Figure 1 As shown in the figure, there are a molding step S01 and a firing step S02.

[0061] The molding process S01 is a process for making a molded product by heat molding the raw material composition. The raw material composition is composed of a material containing a fluorine resin or a fluorine elastomer, and contains fillers as needed. The material containing a fluorine resin or a fluorine elastomer preferably has thermal crosslinking properties that are crosslinked by heating. As fluorine resins and fluorine elastomers with thermal crosslinking properties, commercial products can be used. As commercial products of fluorine resins and fluorine elastomers, for example, SHIN-ETSU SIFEL (registered trademark) series manufactured by Shin-Etsu Chemical. Co., Ltd. can be used.

[0062] The heat molding of the raw material composition can be performed, for example, by placing the raw material composition into a mold and heating it while applying pressure using a hot press. The heating using the hot press can be used as the primary vulcanization, and the secondary vulcanization can be performed. The secondary vulcanization can be performed, for example, by taking out the primary sulfide obtained by the primary vulcanization from the mold and heating it at a temperature higher than the heating temperature during the primary vulcanization. Although the heating temperature of the primary vulcanization varies depending on the type or amount of the fluorine-based resin and the fluorine-based elastomer contained in the raw material composition, it is, for example, in the range of 120°C to 200°C. The pressurization pressure of the primary vulcanization is, for example, 15MPa. The heating temperature of the secondary vulcanization is a temperature higher than the heating temperature of the primary vulcanization, and is a temperature below the thermal decomposition temperature of the primary sulfide. The heating temperature of the secondary vulcanization can be, for example, a temperature in the range of 10°C to 50°C higher than the heating temperature of the primary vulcanization.

[0063] The firing step S02 is a step of firing the molded product obtained in the molding step S01 to produce a softened fired body having a hardness AM lower by 7 or more when compared with the hardness AM of the molded product. The heating temperature of the firing step S02 is a temperature higher than the heating temperature of the secondary vulcanization and a temperature below the thermal decomposition temperature of the molded product. The heating temperature of the firing step S02 can be, for example, a temperature in the range of 10°C or more higher than the heating temperature of the secondary vulcanization and 150°C or less. The heating temperature of the firing step S02 is, for example, 200°C or more, preferably 250°C or more, and more preferably 300°C or more.

[0064] In order to determine the firing temperature and firing time in the firing step S02 , a preliminary step may be performed.

[0065] In the preliminary step, the molded product obtained in the molding step S01 is fired under a plurality of conditions with different temperatures and times, thereby obtaining a plurality of fired products. Next, the hardness AM of the plurality of fired products is measured. Furthermore, by comparing the hardness AM of the molded product with the hardness AM of the plurality of fired products, the firing temperature and firing time that can obtain a softened fired product whose hardness AM is lower than the hardness AM of the molded product by 7 or more are determined.

[0066] In the firing step S02, the molded product is fired at the firing temperature and firing time obtained in the preliminary step to produce a softened fired body. By firing the molded product at the firing temperature and firing time obtained in the preliminary step, a softened fired body having a specified hardness AM can be obtained with a high probability.

[0067] In the preparatory step, it is preferred to further determine a firing temperature and firing time that can obtain a softened fired body whose change is ±5 compared to before heating after heating at 250° C. for 25 hours. By firing the molded product at this firing temperature and firing time, a softened fired body having a specified hardness AM and high thermal stability of the hardness AM can be obtained.

[0068] According to the method for manufacturing a heat transfer component of the present embodiment constructed as described above, since the molded product obtained in the molding step S01 is fired under the above conditions in the firing step S02, a heat transfer component having a hardness AM lower than the hardness AM of the molded product by 7 or more can be manufactured industrially advantageously.

[0069] In the manufacturing method of the heat transfer component of this embodiment, by using the firing temperature and firing time calculated in the above-mentioned preliminary step to fire the molded product in the firing step S02, a heat transfer component with a hardness AM lower than the hardness AM of the molded product by 7 or more can be manufactured stably for a long time with a higher probability.

[0070] In the manufacturing method of the heat transfer component of the present embodiment, although the raw material composition is placed in the mold and heated in the molding step S01, the method for making the molded product is not limited to this. For example, the raw material composition can be applied to one of a pair of parts that clamp the heat transfer component, and the obtained coating film can be heated to make a molded product. In addition, the coating film can be heated while pressurizing the coating film. In addition, the primary sulfide can be arranged on one of the pair of parts that clamp the heat transfer component, and the primary sulfide can be pressed on the part while performing secondary vulcanization. Furthermore, the molded product can be arranged on one of the pair of parts that clamp the heat transfer component and the molded product can be pressed while performing the sintering step S02.

[0071] <Plasma processing equipment>

[0072] Next, a plasma processing apparatus using the heat transfer member of this embodiment will be described.

[0073] Figure 2 It is a longitudinal sectional view showing an example of a plasma etching apparatus according to an embodiment of the present invention.

[0074] Figure 2 The plasma etching apparatus 100 shown includes a chamber 3 having an airtight space therein, an etching gas introduction unit 1 provided at the upper side of the chamber 3 , and a processing object support unit 2 provided at the lower side of the chamber 3 .

[0075] The etching gas introduction part 1 includes a plasma processing device electrode 12 and a cooling plate 15 for cooling the plasma processing device electrode 12. The above-mentioned sheet-shaped heat transfer member 13 is arranged at least in a portion between the plasma processing device electrode 12 and the cooling plate 15. The heat transfer member 13 is preferably arranged in an area of ​​80% or more of the area of ​​the opposing portion where the plasma processing device electrode 12 and the cooling plate 15 are opposed to each other, and more preferably arranged in the entire opposing portion.

[0076] In addition, for reasons such as ease of assembly and alignment, it is preferred to directly join the plasma processing device electrode 12 and the heat transfer member 13 to integrate the two in advance. As a method for directly joining the plasma processing device electrode 12 and the heat transfer member 13, for example, a method of heating the plasma processing device electrode 12 and the heat transfer member 13 in a contact state can be used. In addition, the plasma processing device electrode 12 and the heat transfer member 13 can be heated while applying pressure.

[0077] The plasma processing device electrode 12 has a plurality of vents 11 through which a gas for plasma generation passes. On the other hand, through holes 16 are formed in the cooling plate 15 in a manner that matches the vents 11 of the plasma processing device electrode 12 and at the same intervals as the vents 11. The cooling plate 15 is supported in an insulated state in the chamber 3 by an insulator 14. The plasma processing device electrode 12 is connected to a high frequency power supply 50 and functions as an electrode portion.

[0078] The object support 2 includes a support frame 21, an electrostatic chuck 22 disposed at the center of the support frame 21, and a focus ring 23 disposed around the electrostatic chuck 22. The above-mentioned sheet-shaped heat transfer member 24 is disposed at least in a portion between the support frame 21, the focus ring 23, and the support frame 21. The heat transfer member 24 is preferably disposed in an area of ​​80% or more of the area of ​​the opposing portion where the support frame 21 and the focus ring 23 are opposed to each other, and more preferably disposed in the entire opposing portion.

[0079] For reasons such as ease of assembly and alignment, it is preferred to directly bond the focus ring 23 and the heat transfer member 24 to integrate the two in advance. As a method for directly bonding the focus ring 23 and the heat transfer member 24, for example, a method of heating the focus ring 23 and the heat transfer member 24 in a contact state can be used. In addition, the heating of the focus ring 23 and the heat transfer member 24 can be performed while applying pressure.

[0080] A heat sink 25 is disposed between the support frame 21 and the electrostatic chuck 22. A wafer (substrate to be processed) 40 is placed on the electrostatic chuck 22 in a state where its peripheral portion is supported by the focus ring 23. An O-ring 26 is disposed between the support frame 21 and the focus ring 23. The support frame 21 has a refrigerant flow path 27 therein and also functions as a cooling unit. In addition, the support frame 21 is connected to a ground 28 and also functions as an electrode unit.

[0081] An etching gas supply pipe 31 is disposed on the upper side of the chamber 3. An exhaust port 33 is disposed on the side of the chamber 3. The etching gas sent from the etching gas supply pipe 31 passes through the diffusion component 32 and is then supplied to the wafer 40 from the vent hole 11 of the plasma processing device electrode 12. By applying a high frequency (RF) voltage between the plasma processing device electrode 12 and the support frame 21, the etching gas supplied to the wafer 40 becomes a plasma state, and the wafer 40 is etched.

[0082] According to the plasma etching apparatus 100 of the present embodiment as described above, since the heat transfer member 13 is disposed at least partially between the plasma processing apparatus electrode 12 and the cooling plate 15, the heat of the plasma processing apparatus electrode 12 heated by plasma can be efficiently transferred to the cooling plate 15. Therefore, it is easy to ensure the thermal uniformity of the plasma processing apparatus electrode 12 for a long time. In addition, by directly bonding the plasma processing apparatus electrode 12 to the heat transfer member 13, the heat of the plasma processing apparatus electrode 12 can be transferred to the cooling plate 15 with higher efficiency.

[0083] Furthermore, according to the plasma etching apparatus 100 of the present embodiment, since the heat transfer member 24 is disposed at least partially between the focus ring 23 and the support frame 21, the heat of the focus ring 23 heated by plasma can be efficiently transferred to the support frame 21. Therefore, it is easy to perform a long-term stable plasma treatment on the object to be processed. Furthermore, by directly bonding the focus ring 23 to the heat transfer member 24, the heat of the focus ring 23 can be transferred to the heat sink 25 with higher efficiency.

[0084] Although the embodiments of the present invention have been described above, the present invention is not limited thereto and can be appropriately modified within the scope of the technical concept of the present invention.

[0085] Example

[0086] [Example 1 of the present invention]

[0087] (1) Preparation of raw material composition

[0088] As an organic component, a liquid fluorine-based elastomer having a perfluoropolyether group and having thermal crosslinking properties (X-71-358-4, manufactured by Shin-Etsu Chemical. Co., Ltd.) was prepared. In addition, as a first filler, a large-particle-size alumina filler (AA-18, manufactured by Sumitomo Chemical Co., Ltd., average particle size (d50): 18 μm) was prepared, and as a second filler, a small-particle-size alumina filler (AA-3, manufactured by Sumitomo Chemical Co., Ltd., average particle size (d50): 3 μm) was prepared.

[0089] The organic component was 10 parts by mass (40 parts by volume as the amount of the organic component), the first filler was 19.5 parts by mass (36 parts by volume), and the second filler was 13 parts by mass (24 parts by volume). The obtained mixture was deaerated and kneaded using a rotation-revolution vacuum mixer (Degassing Rentaro ARV-310, manufactured by THINKY CORPORATION) to prepare a raw material composition.

[0090] (2) Production of molded products

[0091] The raw material composition obtained in the above (1) was placed in a mold and subjected to primary vulcanization at 150°C for 10 minutes using a hot press to obtain a sheet-like primary vulcanized product. The thickness of the primary vulcanized product was 200 μm. Next, the obtained primary vulcanized product was taken out of the mold and subjected to secondary vulcanization at 200°C for 4 hours. Thus, a molded product was obtained.

[0092] (3) Production of sintered body

[0093] The molded product obtained in the above (2) was fired at 300° C. for 5 hours to obtain a fired body.

[0094] [Examples 2 to 3, 5 to 7 of the present invention, comparative examples 1 to 2]

[0095] In the preparation of the raw material composition of the above (1), as an organic component, materials of the types shown in the following Table 1 are used, and the content of the first filler in the filler component and the content of the filler component in the raw material composition are set to the amounts shown in the following Table 1. The raw material composition is prepared in the same manner as in Example 1 of the present invention, except that. In addition, the fluorine-based elastomers of Examples 2 to 3 and 5 of the present invention use the same fluorine-based elastomer as in Example 1 of the present invention. The fluorine-based elastomer of Example 6 of the present invention uses X-71-359 manufactured by Shin-Etsu Chemical. Co., Ltd. The fluorine-based resin of Example 7 of the present invention uses a fluorine-based resin obtained by blending equal parts by mass of X-71-6053-6A and X-71-6053-6B manufactured by Shin-Etsu Chemical. Co., Ltd. The silicone rubber of Comparative Example 2 was a silicone rubber obtained by blending KE-1950-10A and KE-1950-10B manufactured by Shin-Etsu Chemical Co., Ltd. in equal parts by mass.

[0096] In the preparation of the molded product in (2), the molded product was prepared in the same manner as in Inventive Example 1 except that the temperature and time of the primary vulcanization and the secondary vulcanization were set to the temperature and time shown in the following Table 1. In Inventive Example 6, the secondary vulcanization was not performed.

[0097] In the preparation of the sintered body in (3) above, a sintered body was prepared in the same manner as in Inventive Example 1 except that the heating temperature and the heating time were set to the temperature and time shown in the following Table 1. The thickness of the obtained sintered body was about 200 μm.

[0098] [Example 4 of the present invention]

[0099] In the preparation of the raw material composition of the above (1), the raw material composition was prepared in the same manner as in Example 1 of the present invention, except that the ratio of the first filler was set to 42 parts by volume and the ratio of the second filler was set to 18 parts by volume. In the preparation of the molded product of the above (2), the obtained raw material composition was used, and the molded product was obtained in the same manner as in Example 1 of the present invention. The obtained molded product and a silicon wafer were superimposed and sintered at 350° C. for 1 hour to produce a sintered body of the molded product, thereby producing a silicon wafer with a sintered body.

[0100] [Example 8 of the present invention]

[0101] A liquid fluorine-based elastomer (X-71-358-4, manufactured by Shin-Etsu Chemical. Co., Ltd.) was applied to the surface of a silicon wafer to form a coating film with a thickness of 50 μm. Next, the silicon wafer with the coating film was subjected to a primary vulcanization at 150°C for 10 minutes, and then a secondary vulcanization at 200°C for 4 hours, and the coating film was used as a molded product. Next, the silicon wafer with the molded product was fired at 300°C for 5 hours to generate a fired body of the molded product, thereby producing a silicon wafer with a fired body.

[0102]

[0103] [evaluate]

[0104] The obtained molded product and sintered body were measured for hardness AM and thermal resistance by the following method. In addition, the sintered body was measured for hardness AM after heating at 250° C. for 25 hours by the following method. The results are shown in Table 2.

[0105] (Measurement method of hardness AM)

[0106] The measurement was carried out using a rubber hardness tester equipped with a push pin of an AM type hardness tester in accordance with the method of JIS K 6253-3:2012. The durometer hardness is the value obtained by the depth of the indentation when a specified push pin is pressed vertically into the test piece under specified conditions. The diameter of the pressure plate of the AM type hardness tester is 9.0±0.3mm, and a center hole with a diameter of 1.19±0.03mm is opened in the center. The indentation depth is measured by pressing the sample horizontally with the pressure plate while the push pin is passed through the center hole of the pressure plate and pressed on the surface of the sample. The AM type requires the sample thickness to be more than 1.5mm. When this thickness is not met, the heat transfer components are stacked and measured until it exceeds 1.5mm. In the AM type, a total of five measurements are made at measurement positions more than 0.8mm apart, and their central values ​​are taken.

[0107] (Thermal resistance measurement method)

[0108] The thermal resistance value was measured by the steady-state method in accordance with JIS H7903:2008 and ASTM D5470-1. An upper alumina block in contact with the heating part and a lower alumina block in contact with the cooling part were set in the chamber, and five thermocouples were installed at intervals of 6 mm on each of the upper and lower alumina blocks. In addition, a stacked body was prepared in which silicon wafers, samples (molded products, sintered bodies), and aluminum plates treated with a single-sided alumina film were stacked in this order from top to bottom. Heat transfer grease was applied to the opposing surfaces of the upper alumina block and the lower alumina block, and the above-mentioned stacked body was set between them. A hammer was set on the upper part of the upper alumina block in such a way that a load of 16 kPa was applied to the sample, and the pressure in the chamber was set to 5 Pa, and the thermal resistance value was measured.

[0109] (Method for measuring hardness AM after heating at 250°C for 25 hours)

[0110] The sintered body of the sample was placed in an electric furnace and heated at 250° C. for 25 hours in the atmosphere. After cooling to room temperature, the hardness AM was measured.

[0111] [Table 2]

[0112]

[0113] From the results in Table 2, it can be seen that the thermal resistance value of the laminated body of the sintered bodies of Examples 1 to 8 of the present invention, which have a hardness AM reduced by 7 or more relative to the hardness AM of the molded body, is greatly reduced. It is believed that this is because the adhesion between the silicon wafer and the aluminum plate treated with a single-sided aluminum oxide film is improved by reducing the hardness AM of the sintered body. From this result, it is confirmed that the sintered bodies of Examples 1 to 8 of the present invention are useful as heat transfer components. In particular, the thermal resistance value of the sintered bodies obtained in Examples 1, 3, 4, 6, and 7 of the present invention, in which the content of the filler component in the raw material composition is 60% by volume or more, is 10 cm 2 Furthermore, the thermal resistance of the sintered bodies obtained in Examples 1, 4, 6, and 7 of the present invention, in which the heating temperature during the preparation of the sintered bodies was 300° C. or higher, was 8 cm 2 K / W or less. On the other hand, the thermal resistance value of the laminated body using the sintered body of Comparative Example 1, in which the decrease in hardness AM relative to the molded body is small, is almost the same as the thermal resistance value of the laminated body using the molded body. Furthermore, in Comparative Example 2 using silicone rubber, the hardness AM increases due to sintering.

[0114] (Evaluation of plasma resistance)

[0115] In Comparative Example 2 where the heat transfer component is molded from silicone rubber, the portion exposed to plasma becomes slightly hardened, but in Examples 1 to 8 of the present invention and Comparative Example 1 where the heat transfer component is molded from fluorine-based resin or fluorine-based elastomer, the portion exposed to plasma does not become hardened.

[0116] Industrial Applicability

[0117] According to the present invention, a heat transfer component having high plasma resistance and capable of maintaining high adhesion with various components for a long time and a method for manufacturing the same, as well as a plasma processing device in which the temperature of each component in the chamber is easily stabilized even when the chamber is in a vacuum state can be provided.

[0118] Explanation of symbols

[0119] 1 Etching gas inlet

[0120] 2. Processing object support

[0121] 3 Chambers

[0122] 11 Ventilation holes

[0123] 12Electrodes for plasma processing equipment

[0124] 13 Heat transfer components

[0125] 14 Insulator

[0126] 15 Cooling Plate

[0127] 16 Through hole

[0128] 21 Support frame

[0129] 22 Electrostatic chuck

[0130] 23 Focus ring

[0131] 24 Heat transfer components

[0132] 25 Heat sink

[0133] 26 O-ring

[0134] 27 Refrigerant flow path

[0135] 28 Ground

[0136] 31 Etching gas supply pipe

[0137] 32 Diffuser

[0138] 33 Exhaust port

[0139] 40 chips

[0140] 50 High frequency power supply

[0141] 100 Plasma Etching Device

Claims

1. A heat transfer component comprising a sintered body of a molded product containing a fluorine-based resin or a fluorine-based elastomer, wherein: The hardness of the heat transfer member measured using an AM type hardness tester in accordance with JIS K 6253-3:2012 is lower than the hardness of the molded article by 7 or more.

2. The heat transfer component according to claim 1, wherein: The shaped article contains a filler.

3. The heat transfer component according to claim 2, wherein: The filler is at least one inorganic substance selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride and silicon.

4. A heat transfer component, which is a heat transfer component composed of a molded body containing a fluorine-based resin or a fluorine-based elastomer, wherein: The hardness of the heat transfer member measured using an AM type hardness tester in compliance with JIS K 6253-3:2012 has a change in the range of ±5 after heating at 250° C. for 25 hours compared with that before heating.

5. The heat transfer component according to claim 4, wherein: The shaped body contains a filler.

6. The heat transfer component according to claim 5, wherein: The filler is at least one inorganic substance selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride and silicon.

7. A method for manufacturing a heat transfer component, which is a method for manufacturing a heat transfer component containing a fluorine-based resin or a fluorine-based elastomer, characterized in that: include: A molding step of heating and molding a material containing the fluorine-based resin or the fluorine-based elastomer to produce a molded product; as well as a calcining step of calcining the molded product to produce a softened calcined body having a hardness lower than the hardness of the molded product measured by an AM type hardness tester in accordance with JIS K 6253-3:2012 by 7 or more, The heat transfer component is composed of the softened sintered body.

8. A method for manufacturing a heat transfer component, characterized in that: The manufacturing method is the manufacturing method of the heat transfer component according to claim 7, comprising: a preparatory step of sintering the molded product under a plurality of conditions of different temperatures and times to obtain a plurality of sintered products, measuring the hardness of the plurality of sintered products obtained using an AM type hardness tester in accordance with JIS K 6253-3:2012, comparing the hardness of the molded product with the hardness of the plurality of sintered products, thereby determining a sintering temperature and sintering time for obtaining the softened sintered product having a hardness of the sintered product lower by 7 or more than the hardness of the molded product, In the firing step, the molded product is fired at the firing temperature and the firing time determined in the preparatory step to produce the softened fired body.

9. A plasma processing device, comprising: an electrode for a plasma processing device having a vent hole for passing a gas for plasma generation; and a cooling plate, wherein: The heat transfer member according to any one of claims 1 to 6 is disposed at least in a portion between the plasma processing apparatus electrode and the cooling plate.

10. The plasma processing device according to claim 9, characterized in that: The plasma processing device electrode is directly bonded to the heat transfer member.

11. A plasma processing device comprising a focus ring and a support frame for supporting the focus ring, wherein: The heat transfer member according to any one of claims 1 to 6 is disposed at least in a portion between the focus ring and the support frame.

12. The plasma processing device according to claim 11, characterized in that: The focus ring is directly engaged with the heat transfer component.