Compressed thin liquid absorbing core and manufacturing method thereof
By adopting a porous structure of polyvinyl acetal foam core, the problems of heavy feeling and slow water absorption of the traditional absorbent core are solved, and the effects of fluffy and breathable after liquid absorption are achieved, high absorption rate and good liquid locking performance are achieved.
Patent Information
- Application Number
- CN202411026882.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The absorbent core of traditional sanitary products has problems such as thicker thickness, strong thicker feeling after liquid absorption, and poor body retention. The highly absorbent resin has poor compatibility with water, resulting in slower water absorption and lower water absorption rate.
The upper and lower permeable membrane layers and the intermediate structure layer using porous structure are integrated polyvinyl acetal foam cores, and the intermediate structure layer is a three-dimensional through-pore structure. The average pore diameter of the first-level micropore is 200-2000 microns, and distributed on the pore walls. The secondary micropores are formed by drilling, embossing and hollowing processing to form a compressed thin liquid absorbing core, with a liquid absorption ratio of between 12-30 times.
After absorbing liquid, the core body returns to fluffy, reduces thickness, is light to wear, and has high adsorption and locking effects after absorbing liquid. The liquid is not easy to leak and has a fast absorption speed, which prevents the problem of local concentration of liquid.
Smart Images

Figure CN118948536A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of absorbent cores, in particular to a compressed thin liquid absorbent core and a manufacturing method thereof. Background Art
[0002] Traditional sanitary products, including sanitary napkins, menstrual pants, nursing pads and other products, mainly have three-layer structures: a skin-friendly and permeable surface layer, an absorbent and liquid-locking core, and a breathable and leak-proof bottom layer. Among them, the surface layer is generally a non-woven fabric or a perforated film material, which plays a role in diversion and skin-friendly, the bottom layer is a polyethylene film or a composite material of polyethylene film and non-woven fabric, which plays a waterproof and seepage-proof role, and the absorbent core layer is mainly composed of a multi-layer composite core filled with super absorbent resin (SAP resin), or an absorbent core made of fluff pulp, cotton fiber, paper fiber and other fibers mixed with super absorbent resin.
[0003] With the development of science and technology, polymer materials have entered various life application scenarios, especially personal care products. People pay more attention to the safety, comfort and performance of materials. Therefore, various products with different performances have appeared in the market. Some of them have optimized the appearance, size and structure of the products according to the consumption needs of different groups of people to solve the problem of heterogeneity. Some are loaded with antibacterial and natural fragrance functions. Some have introduced foam materials such as polyurethane and polyacrylate as the absorption layer, aiming to solve the problems of light wearing, fast absorption, dry and breathable, comfortable and fluffy, and beautiful appearance. However, there are still problems such as thick thickness, strong heavy feeling after absorbing liquid, and poor shape retention.
[0004] For example, the Chinese patent with the announcement number CN115212040A provides a foam air core and its preparation method and application to solve the problem of poor air permeability and softness of the existing sanitary napkin cotton core. The foam air core includes an intermediate layer, which is formed by a plurality of bubble-like units connected and arranged with each other, and the upper and lower sides of the intermediate layer are respectively bonded with an upper layer and a lower layer, and a water-absorbing polymer layer is provided between the upper layer and the intermediate layer, and between the lower layer and the intermediate layer. The foam air core is provided with an intermediate layer composed of a plurality of bubble-like units, and the bubble-like units form air bubbles inside the cotton core, thereby increasing the air permeability and elasticity of the cotton core. The bubble-like unit is a hemispherical structure, and the hemispherical structure makes the bubble-like unit have good elasticity, and the diameter of the bubble-like unit is 1-5mm. However, the intermediate layer still uses a mixed material of pulp fiber, nanofiber and antibacterial fiber. Although the setting of the bubble-like unit increases the air permeability and elasticity, there are still problems such as thick size, strong heavy feeling after absorbing liquid, poor adhesion, and inconvenient movement.
[0005] A Chinese patent with the announcement number CN116531176A discloses an absorbent product and a method for preparing the same. The absorbent core in the application is obtained by reacting acrylate monomers, modified acrylates, crosslinking agents, photoinitiators, emulsifiers, and initiators. Specifically, a high internal phase emulsion 1 and a high internal phase emulsion 2 are prepared, which are coated on the upper and lower surfaces of the fabric respectively, and then the absorbent core is obtained by light exposure, steam treatment, dehydration, and drying. The technology obtains upper and lower surface structures with different pore sizes by controlling emulsion 1 and emulsion 2. The absorbent core is mainly composed of a polyacrylate foam obtained by polymerizing and crosslinking acrylate monomers. However, because acrylate monomers have poor compatibility with water and are not easily soluble in water, it is difficult to completely remove the residual monomers that have not been completely reacted by washing, so there is a potential risk of residual acrylate monomers, crosslinking agents, initiators, etc. in the absorbent core. In addition, polyacrylate resin is not hydrophilic. Although it has been modified, the hydrophilicity of the foam formed by it is poor. If there is no wetting agent, the water absorption is slow and the water absorption rate is low. The highest water absorption rate in the embodiment is only 12.2 times. The mechanical properties of polyacrylate foam are also poor, with low elongation at break and tensile strength.
[0006] The Chinese patent with the announcement number CN117338519A proposes a diaper absorbent core and its production process, which solves the technical problems that the existing diaper core is not bonded to the bottom film through the core on both sides, and the three-dimensional suspension effect cannot be highlighted because the core itself is not foldable, and the absorption and leakage prevention performance are poor. To achieve the purpose, the invention adopts a pressing groove arranged on the core near the lateral sides, a bottom film arranged on the bottom surface of the core, a covering layer arranged outside the core, and an elastic root arranged on the lateral sides of the core. Through the setting of the pressing groove and the elastic root, under the action of the elastic root, the core on both sides will stand up, and the lateral sides of the core will be blocked to a certain extent, thereby improving the core absorption rate, preventing leakage from the lateral sides, and improving the absorption area and leakage prevention performance of the product. However, this process mainly relies on the shape settings such as pressing grooves and elastic roots to achieve the purpose of preventing side leakage, and cannot solve the problems existing in traditional diapers and sanitary napkins.
[0007] The Chinese patent with the announcement number CN116999247A provides a high-absorption core and sanitary products, which are used to solve the problem of local large-scale expansion and discomfort caused by the inorganic salt ion adsorption materials set in the existing disposable sanitary products to improve the absorption performance. The scheme adopted by this technology is that the high-absorption core includes a contact surface layer, an absorption layer and a fixed bottom layer, and also includes an ion adsorption layer, which is arranged between the contact surface layer and the absorption layer. The ion adsorption layer includes a hydrophilic base layer and cationic adsorption particles arranged on the hydrophilic base layer. However, its absorption layer is composed of an elastic absorption layer and a composite wood pulp layer, and the elastic absorption layer includes a plurality of hollow wrapping capsules and water-absorbing particles filled in the wrapping capsules. The composite wood pulp layer includes a wood pulp surface layer, a composite resin layer and a wood pulp bottom layer arranged in sequence. However, the core still mainly relies on fibers and water-absorbing particles for absorption, and there are problems such as not being light enough, poor air permeability after absorbing liquid, and a strong sense of heaviness. Summary of the invention
[0008] The object of the present invention is to provide a compressed thin liquid absorbing core to solve the problems raised in the above background technology.
[0009] In order to solve the above technical problems, the present invention provides the following technical solutions: a compressed thin liquid absorbing core, comprising upper and lower water-permeable membrane layers and an intermediate structural layer of a porous structure, wherein the upper and lower water-permeable membrane layers and the intermediate structural layer are an integrated polyvinyl acetal foam core;
[0010] The middle structure layer is a three-dimensional through-opening structure, the average pore size of the primary micropores in the middle structure layer is 200-2000 microns, and secondary micropores are distributed on the pore walls of the primary micropores in the middle structure layer, and the average pore size of the secondary micropores is 3-50 microns.
[0011] Preferably, the core is a white sheet compressed up and down, and is punched, embossed, and hollowed out, and the liquid absorption rate of the core is between 12-30 times; after absorbing the liquid, the core recovers from the compressed state to the fluffy state, and the thickness of the core recovered to the fluffy state is 0.8-6mm.
[0012] Preferably, the core is made of polyvinyl alcohol, a crosslinking agent and an acid catalyst through crosslinking and foaming.
[0013] Preferably, the core is made of polyvinyl alcohol, a cross-linking agent, an acid catalyst and a modified substance through cross-linking and foaming.
[0014] Preferably, the modified substance includes wood pulp fiber, paper fiber, cotton fiber, chemical fiber; melamine resin, urea-formaldehyde resin, cellulose, polyethylene oxide, sodium polyacrylate, polyvinyl pyrrolidone polymer; phosphate, silicate, talcum powder, kaolin, montmorillonite, calcium chloride inorganic substances; cationic, anionic, nonionic surfactants; one, two or more of polyols such as glycerol, propylene glycol, polyethylene glycol, etc. A method for making a compressed thin liquid absorbent core, comprising the following steps:
[0015] S1: adding polyvinyl alcohol, a modified substance and water into a dissolving kettle, stirring and dispersing them together, adding an acid catalyst and a crosslinking agent after the polyvinyl alcohol is dissolved, stirring evenly, and mixing and reacting to obtain a polyvinyl alcohol pre-reaction product A;
[0016] S2: sending the pre-reaction product A to a continuous foaming unit, and introducing clean gas and a second cross-linking agent into the unit for mixing and foaming to obtain a foamed body B;
[0017] S3: The foamed body B is spread by scraping and flattening, and sent to the maturation channel through a heated conveyor belt for maturation and shaping. The shaped product is pre-cooled in a supercooled water tank;
[0018] S4: The cooled product is washed by the roller unit and then dried, and then sent to the drying channel for drying. The dried product is cooled in the cold air channel and then sent to the physical finishing process for compression and calendering. After compression, embossing or punching and hollowing treatment can be performed as needed.
[0019] Preferably, the first crosslinking agent is at least one of formaldehyde, acetaldehyde, glyoxylic acid, glyceraldehyde, glucose, maltose, and ribose, and the second crosslinking agent is methylol urea, N-methylol melamine, acetaldehyde, glyoxal, formaldehyde, glutaraldehyde, DuPont brand At least one of the organic phthalate crosslinking agent of 371 and the organic zirconium crosslinking agent of Tyzor 212 produced by DuPont; the addition temperature of the crosslinking agent 1 is 50-95°C, and the addition temperature of the crosslinking agent 2 is 40-80°C.
[0020] Preferably, in step S2, the clean gas includes any one or more of clean air, nitrogen, and carbon dioxide, and the density of the foam B is between 0.2-0.4 g / ml.
[0021] Preferably, in step S3, the temperature setting interval of the aging channel is 50-95° C., and the aging time is between 1-30 min.
[0022] Preferably, in step S4, the temperature range of the drying channel is 60-120°C; the product is cooled by cold air before compression; the thickness ratio of the product before and after compression is between 2-10:1; and the product is embossed or punched and hollowed out after compression.
[0023] Preferably, in step S4, after the product is pressure washed by the roller pressing unit, it can enter the chemical finishing tank for softening, smoothness or antibacterial finishing, and then be sent to the drying channel for drying.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The main material of the core of the present invention is polyvinyl acetal foam, which has good physical processing properties. The dry foam can maintain a relatively soft sheet shape when compressed into a thin sheet state. The hole space in the middle structural layer is compressed, and the hole walls are squeezed together. Under the condition of ensuring that the water absorption rate is not lower than that of traditional products of the same thickness, it has the advantages of ultra-thin shape and is very light when worn.
[0026] After the core sheet absorbs liquid, the holes inside the sheet stretch and recover, presenting a fluffy and breathable porous sponge structure, which is soft, comfortable and has good adhesion performance. The core body has a liquid absorption rate of 12-30 times, preferably 15-25 times. After the core body absorbs liquid, it recovers from a compressed state to a fluffy state, which is thinner than the thickness of various traditional fiber cores on the market, and has the advantages of being fluffy and breathable, not easy to wrinkle, and having a light sense of heaviness.
[0027] After the core absorbs the liquid, its abundant primary pore structure and the secondary micropore structure on the pore wall have a good adsorption and locking effect on the liquid. It has the advantages of high absorption rate, good liquid locking performance, and liquid is not easy to leak.
[0028] The porous membrane structure of the upper and lower skins of the core is conducive to the rapid diffusion of liquid on the surface of the core, with the advantages of instantaneous dispersion and fast absorption, and preventing the local concentration of liquid. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is the overall structure diagram of the present invention;
[0030] Figure 2 This is an electron microscope image of the inner pore walls of the core body pressed against each other in the compressed state of the present invention;
[0031] Figure 3 This is an electron microscope image of the internal morphology of the core of the present invention after absorbing water and restoring its fluffy state;
[0032] Figure 4 The electron microscope image of the secondary micropores distributed on the inner pore wall of the core body of the present invention;
[0033] Figure 5 This is an electron microscope image of the porous membrane layer on the upper and lower surfaces of the core of the present invention. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] See also Figure 1-5 This embodiment provides a compressed thin liquid absorption core, the core structure includes: a fast water-permeable film layer 2 with a porous structure, and an intermediate structure layer 1 with a three-dimensional through-opening structure, the upper and lower water-permeable film layers and the intermediate structure layer are an integrated polyvinyl alcohol acetal foam core. The average pore size of the primary micropores in the intermediate structure layer is 200-2000 microns, preferably 200-600 microns. On the pore walls of the primary micropores in the intermediate structure layer, secondary micropores are distributed (secondary micropores can be formed during foaming), and the average pore size of the secondary micropores is 3-50 microns, preferably 3-10 microns.
[0036] The core is a white sheet compressed from top to bottom, and can be punched, embossed, hollowed out, etc. as needed. The thickness of the core sheet is 0.3-3 mm, preferably 0.6-1.6 mm, and the liquid absorption rate of the core is between 12-30 times, preferably 15-25 times. After absorbing liquid, the core recovers from the compressed state to the fluffy state, and the thickness of the core that recovers to the fluffy state is 0.8-6 mm, preferably 2-3 mm.
[0037] The core is obtained by cross-linking and foaming polyvinyl alcohol, aldehyde cross-linking agent and acid catalyst. During the foaming process, a modified substance can be added. The modified substance is a selected substance and may not be added or may be added according to the application requirements. The modified substance can be selected from wood pulp fiber, paper fiber, cotton fiber, chemical fiber; melamine resin, urea-formaldehyde resin, cellulose, polyethylene oxide, sodium polyacrylate, polyvinyl pyrrolidone polymer; phosphate, silicate, talc, kaolin, montmorillonite, calcium chloride inorganic substances; one, two or more of polyols such as glycerol, propylene glycol, polyethylene glycol, etc., and a mixture of cationic, anionic and non-ionic surfactants can also be selected to achieve uniform foaming, pore opening, wetting and the like. The above modified substances can be added alone or in mixtures of two or more.
[0038] The core production process is as follows:
[0039] S1: Add polyvinyl alcohol, modified substance and water into a dissolving kettle, stir and disperse them together, add acid catalyst and cross-linking agent 1 after polyvinyl alcohol is dissolved, stir evenly, and mix to obtain polyvinyl alcohol pre-reaction product A; wherein the cross-linking agent 1 is at least one of formaldehyde, acetaldehyde, glyoxylic acid, glyceraldehyde, glucose, maltose and ribose, and the adding temperature of the cross-linking agent 1 is 50-95°C.
[0040] S2: The pre-reaction product A is sent to a continuous foaming unit, and clean gas and a second cross-linking agent are introduced to mix and foam together to obtain a foamed body B; wherein the second cross-linking agent is methylol urea, N-methylol melamine, acetaldehyde, glyoxal, formaldehyde, glutaraldehyde, DuPont brand At least one of the organic phthalate crosslinking agent of 371 and the organic zirconium crosslinking agent of Tyzor 212 produced by DuPont; the adding temperature of the crosslinking agent II is 40-80° C. The clean gas includes any one or more of clean air, nitrogen and carbon dioxide, and the density of the foam B is between 0.2-0.4 g / ml.
[0041] S3: The foam B is spread by scraping and flattening, and sent to the maturation channel through a heated conveyor belt for maturation and shaping. The shaped product is pre-cooled in a supercooling water tank; the cooling water and generated water, residual inorganic acid, and residual cross-linking agent are recycled, part of which is used for the dispersion and dissolution of polyvinyl alcohol and modified fillers in step S1, and the rest is used for circulating cooling.
[0042] The temperature setting interval of the aging channel is 50-95°C, and the aging time is between 1-30 minutes, preferably 2-8 minutes.
[0043] S4: The pre-cooled product is washed and pressed dry by the roller pressing unit, and then sent to the drying channel for drying. The temperature range of the drying channel is 60-120℃; the dried product is cooled in the cold air channel and then sent to the compression roller for compression. The thickness ratio of the product before and after compression is between 2-10:1; after compression, embossing or punching and hollowing treatment can be performed as needed.
[0044] The polyvinyl alcohol is a completely alcoholysed polyvinyl alcohol with a polymerization degree of 1000-2600; the acid catalyst is one or more of hydrochloric acid, phosphoric acid, sulfuric acid, oxalic acid and sulfonic acid.
[0045] The above steps S1 to S4, from the continuous foaming unit to the aging, pre-cooling, cleaning, rolling, drying, pre-cooling, compression embossing, trimming and winding units, are prepared for a continuous production equipment production line.
[0046] In step S3, the foam B can be directly scraped or spread on a heating roller or a heating transmission belt and sent into a maturation channel. The foam B can also be coated on gauze, glass fiber cloth, non-woven fabric or other materials. It can be coated on one side or on both sides and then sent into a maturation channel for maturation and shaping to obtain a sponge composite product.
[0047] In step S4, after being pressure washed by the roller pressing unit, the fabric can enter the chemical finishing tank for softening, smoothing or antibacterial finishing, and then be sent to the drying channel for drying.
[0048] Example 1
[0049] The method for making the core comprises the following steps:
[0050] S1: 1 part of polyvinyl alcohol (model 1799), 0.05 part of fatty alcohol polyoxyethylene ether and 6.0 parts of water are added into a dissolving kettle and stirred and dispersed together. After the polyvinyl alcohol is dissolved, 0.8 part of sulfuric acid catalyst and 0.3 part of crosslinking agent 1 are added at 85°C, stirred evenly, mixed and reacted for 0.5-1.5 hours, and then the pH is adjusted to between 0.5-4 to obtain polyvinyl alcohol pre-reaction product A;
[0051] S2: sending the pre-reaction product A to a continuous foaming unit, introducing clean air and 0.3 parts of the second cross-linking agent at the same time, mixing and foaming, controlling the density of the foamed mixture to be between 0.2-0.3 g / ml, and obtaining a foamed body B;
[0052] S3: Spread the foam B on the conveyor belt with a scraper to control the thickness of the scraper to 3.5±1mm, blow it flat with airflow, and send it into the aging channel for aging at 80℃ for 6min. The aging and shaping product is pre-cooled in a cold water tank, and the temperature of the cold water tank is controlled below 60℃;
[0053] S4: After the product passes through the cooling tank, it is washed twice by rollers under spraying, enters the finishing tank containing smooth and soft finishing agent, and then squeezed by the roller unit, and then sent to the drying tunnel for drying at a drying temperature of 110°C. The dried product is cooled in the air cooling channel and then sent to the compression roller for compression, with a compression thickness of 1.2±0.5mm.
[0054] The compressed products are trimmed, rolled, sorted and packaged, and then stored for sale.
[0055] It should be noted that, in this embodiment, "parts" refer to mass fractions.
[0056] The core coil obtained by steps S1-S4 is characterized by a polyvinyl acetal foam material, which can be made into coils of different widths. The core coil can be used as the absorption core of sanitary napkins, the absorption layer of diapers, pads and the absorption layer core of various highly absorbent absorbent products. It can also be used as various medical bandages and nursing dressings, and can also be used as imitation chamois towels, anti-static sponge paper, dust-free sponge paper and other products. Compared with traditional cotton absorption layers, pulp absorption layers, non-woven absorption layers and other materials, the product has a greater competitive advantage. In addition, the product can also be made into imitation chamois towels or composite rags by built-in mesh ribs or coating the foam on a cloth base for maturation and molding. It is widely used in various occasions such as homes, dining tables, furniture, floors, tableware, home appliances, beauty salons, baths, swimming pools, indoors, electrical appliances, high-end cars, etc., as a cleaning tool for utensils and items. The product can also be made into thin sponge dust-free paper, which can be used for equipment and tool maintenance and workbench cleaning in laboratories, chemical laboratories, machinery manufacturing, mold processing, petrochemicals, aviation, automobiles, electronics, food, clean rooms and other industries. It is expected to become an effective supplement and potential iterative product for traditional products such as cotton fiber, paper fiber, and non-woven fabrics.
[0057] Example 2
[0058] The difference between this embodiment and embodiment 1 is that in step S1 of embodiment 1, 0.3 parts of pulp fiber is added. Other materials and preparation process are the same as those of embodiment 1.
[0059] Example 3
[0060] The difference between this embodiment and embodiment 1 is that 0.3 parts of sodium silicate is further added in step S1 of embodiment 1. Other materials and preparation process are the same as those of embodiment 1.
[0061] Example 4
[0062] The difference between this embodiment and embodiment 1 is that in step S3 of embodiment 1, the foam B is coated on the upper and lower surfaces of the gauze made of cotton fiber, so that the gauze is buried in the foam to become the reinforcing rib of the foam. Other materials and preparation processes are the same as those in embodiment 1.
[0063] The core of the present invention is used as a sanitary napkin core, and the comparison sample is selected as a common commercially available sanitary napkin:
[0064] Take a commercially available liquid sanitary napkin (Whisper flexfoam liquid sanitary napkin), cut it open along the four sides of the sponge core, peel off the surface layer, take out the sponge core, and obtain comparative sample 1;
[0065] Take a commercially available pure cotton sanitary napkin (Kao pure cotton sanitary napkin), peel off the release paper, remove the adhesive layer, cut off the wings, and obtain a pure cotton absorbent core, i.e., comparative sample 2;
[0066] Take a commercially available fluff fiber sanitary napkin (Seven Dimensions Sanitary Napkin), peel off the release paper, remove the adhesive layer, cut off the leak-proof side wings, and obtain an absorbent core, i.e., comparative sample 3;
[0067] Take a commercially available nighttime sanitary napkin (Mia sanitary napkin), peel off the release paper, remove the adhesive layer, cut off the leak-proof side wings, and obtain a composite fiber absorbent core containing SAP particles, i.e., comparative sample 4;
[0068] To test the lightness and absorption performance of the samples, the thickness of the samples before and after water absorption, the water absorption rate of the samples, and the absorption speed are all tested according to the GB / T 8939-2018 method. To test the shape retention and wrinkle resistance of the samples after water absorption, the shape retention of the samples after water absorption can be judged by the compression permanent deformation of the samples after water absorption, and the air permeability of the samples after water absorption can also be judged from the side. The compression permanent deformation is tested according to GB / T6669-2008 method B.
[0069] The samples obtained in Examples 1-3 were compared with Comparative Samples 1-4, and the comparison results are as follows:
[0070]
[0071]
[0072] As can be seen from the table above, compared with a certain international brand of liquid sanitary napkin, i.e., comparative sample 1, the thickness of Examples 1 to 3 of the present invention after water absorption is comparable, and the water absorption rate and compression permanent deformation are also basically the same, indicating that the porosity and resilience of the foam absorption core are relatively good, and it has better shape retention. However, the advantage of the samples of the embodiments of the present invention is that the thickness of the samples before water absorption is about one-third of that of the liquid sanitary napkin, the product transportation and packaging costs are lower, and it is easier to use and wear. In addition, because the porous water-permeable membrane layer of the technical product of the present invention is conducive to the rapid diffusion of water, the large number of secondary micropores distributed on the pore wall are conducive to enriching the capillary action, therefore, the absorption speed of the technical product of the present invention is within 10 seconds, and it has a better wetting and absorption speed.
[0073] Compared with comparative samples 2 and 3, it can be seen that the examples 1 to 3 of the present invention have thinner dimensions, higher water absorption ratios, and much faster absorption speeds than the comparative samples before and after water absorption. This is because the comparative samples are mainly made of fluffy fibers, so the internal water storage space is smaller than the sponge structure, and the fluffiness deteriorates after water absorption, and it is difficult to recover to the original size after compression.
[0074] Compared with Examples 1 to 3 of the present invention and Comparative Sample 4, the water absorption rate of Comparative Sample 4 is much greater than that of the embodiments of the present invention. This is because a highly absorbent resin is added to Comparative Sample 4, and the resin expands greatly after absorbing water, resulting in an increase in thickness and a strong sense of heaviness. It also has a large deformation after compression and is difficult to restore to its original state.
[0075] Compared with Examples 1 to 3 of the present invention, Example 4 of the present invention has gauze as a skeleton, which greatly increases its tensile strength and tear strength, and its breaking strength increases from 10KPa to 12MPa. In Examples 1 to 4 of the present invention, the elongation at break is greater than 120%, which is much better than Comparative Sample 1, and the breaking strength is better than all comparative samples.
[0076] The core of the present invention is a compressed sheet, and its original color is white. Because the main material of the core is polyvinyl alcohol acetal foam, this kind of material has good physical processing properties, the dry foam can maintain the sheet shape when compressed into a sheet state, the hole space in the middle structure layer is compressed, and the hole walls are squeezed together (such as Figure 2 As shown), after compression, the 3mm thick fluffy sponge can be compressed to the thinnest 0.5mm. Therefore, the absorbent core of the present invention has the advantages of ultra-thin shape and being very light when worn while ensuring that the water absorption rate is not lower than that of traditional products of the same thickness.
[0077] After the core sheet absorbs the liquid, the holes inside the sheet stretch and recover, presenting a fluffy and breathable porous sponge structure (such as Figure 3 The core has a liquid absorption rate of 12-30 times, preferably 15-25 times. After absorbing liquid, the core recovers from a compressed state to a fluffy state, and the thickness of the recovered fluffy core is 0.8-6mm, preferably 2-3mm, which is still thinner than the thickness of various traditional fiber cores on the market. Therefore, the absorbent core of the present invention has the advantages of being fluffy and breathable, not easy to wrinkle, and having a light sense of heaviness.
[0078] After the core absorbs liquid, its abundant primary pore structure and secondary microporous structure (such as Figure 4 As shown), it has good adsorption and locking effect on liquids, and has the advantages of high absorption rate, good liquid locking performance, and liquid is not easy to leak.
[0079] The core has a porous membrane structure on the upper and lower skins (such as Figure 5 As shown), it is conducive to the rapid diffusion of liquid on the surface of the core, has the advantages of instantaneous dispersion and fast absorption, and prevents large amounts of liquid from being concentrated locally.
[0080] The core is completely naturally degradable, which helps alleviate environmental pressure compared to chemical fiber absorbent cores such as hydrophilic non-woven fabrics.
[0081] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A compressed thin liquid absorbing core, characterized in that: It includes upper and lower water-permeable membrane layers and a middle structural layer with a porous structure, wherein the upper and lower water-permeable membrane layers and the middle structural layer are an integrated polyvinyl acetal foam core; The middle structure layer is a three-dimensional through-opening structure, the average pore size of the primary micropores in the middle structure layer is 200-2000 microns, and secondary micropores are distributed on the pore walls of the primary micropores in the middle structure layer, and the average pore size of the secondary micropores is 3-50 microns.
2. A compressed thin liquid absorbing core according to claim 1, characterized in that: The core is a compressed white sheet that is punched, embossed and hollowed out, and the liquid absorption rate of the core is between 12 and 30 times; after absorbing liquid, the core recovers from the compressed state to a fluffy state, and the thickness of the recovered fluffy core is 0.8 to 6 mm.
3. A compressed thin liquid absorbing core according to claim 1, characterized in that: The core is made of polyvinyl alcohol, a crosslinking agent and an acid catalyst through crosslinking and foaming.
4. A compressed thin liquid absorbing core according to claim 1, characterized in that: The core is made of polyvinyl alcohol, aldehyde cross-linking agent, acid catalyst and modified substance through cross-linking and foaming.
5. A compressed thin liquid absorbing core according to claim 4, characterized in that: The modified substances include wood pulp fibers, paper fibers, cotton fibers, chemical fiber materials; melamine resins, urea-formaldehyde resins, cellulose, polyethylene oxide, sodium polyacrylate, polyvinyl pyrrolidone polymers; phosphates, silicates, talc, kaolin, montmorillonite, calcium chloride inorganic substances; cationic, anionic, nonionic surfactants; one or a mixture of two or more of polyols such as glycerol, propylene glycol, polyethylene glycol, etc.
6. A method for manufacturing a compressed thin liquid absorbing core, characterized in that: The steps include: S1: adding polyvinyl alcohol, a modified substance and water into a dissolving kettle, stirring and dispersing them together, adding an acid catalyst and a crosslinking agent after the polyvinyl alcohol is dissolved, stirring evenly, and mixing and reacting to obtain a polyvinyl alcohol pre-reaction product A; S2: sending the pre-reactant A to a continuous foaming unit, and simultaneously introducing clean gas and a cross-linking agent into the mixture for foaming to obtain a foamed body B; S3: The foamed body B is spread by scraping and flattening, and sent to the maturation channel through a heated conveyor belt for maturation and shaping. The shaped product is pre-cooled in a supercooled water tank; S4: The pre-cooled product is washed by the roller unit and then dried, and then sent to the drying channel for drying. The dried product is pre-cooled in the cold air channel and then sent to the physical finishing process for compression and calendering. After compression, embossing or punching and hollowing treatment can be performed as needed.
7. The method for manufacturing a compressed thin liquid absorbing core according to claim 6, characterized in that: The first crosslinking agent is at least one of formaldehyde, acetaldehyde, glyoxylic acid, glyceraldehyde, glucose, maltose, and ribose; the second crosslinking agent is methylol urea, N-methylol melamine, acetaldehyde, glyoxal, formaldehyde, glutaraldehyde, DuPont brand At least one of the organic phthalate crosslinking agent of 371 and the organic zirconium crosslinking agent of Tyzor 212 produced by DuPont; the addition temperature of the crosslinking agent 1 is 50-95°C, and the addition temperature of the crosslinking agent 2 is 30-80°C.
8. The method for manufacturing a compressed thin liquid absorbing core according to claim 6, characterized in that: In step S2, the clean gas includes any one or more of clean air, nitrogen, and carbon dioxide, and the density of the foam B is between 0.2-0.4 g / ml.
9. The method for manufacturing a compressed thin liquid absorbing core according to claim 6, characterized in that: In step S3, the temperature setting range of the aging channel is 50-95° C., and the aging time is between 1-30 min.
10. The method for manufacturing a compressed thin liquid absorbing core according to claim 6, characterized in that: In step S4, the temperature range of the drying channel is 60-120°C; the product is cooled by cold air before compression, and the thickness ratio of the product before and after compression is between 2-10:1; after compression, it is embossed or punched and hollowed out.
11. A method for manufacturing a compressed thin liquid absorbing core according to claim 6, characterized in that: In step S4, after being pressure washed by the roller pressing unit, the fabric enters the chemical finishing tank for softening, smoothness or antibacterial finishing, and then is sent to the drying channel for drying.