Preparation method of polyolefin ether

By using cationic polymerization of trifluoromethylsulfonate and olefin-based ether monomers, the problems of high initiator cost and storage difficulties in the prior art are solved, and low-cost and efficient preparation of polyolefin-based ethers are achieved. The molecular weight and stereoregulation are adjustable, suitable for industrial production.

CN118955770AActive Publication Date: 2024-11-15ZHEJIANG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411310137.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-15
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

The initiator/starter used in the prior art for polyolefin-based ether polymerization is costly, difficult to obtain, and difficult to store, and is used in a harsh reaction environment, which limits the industrial scale production of polymer materials.

Method used

Trifluoromethylsulfonate is used as an initiator and mixed with olefin-based ether monomers to generate polymer products through the cationic ring opening polymerization mechanism, precipitation is used for inert solvents and the reaction conditions are regulated to achieve a low-cost and easy-to-operate polymerization process.

Benefits of technology

It realizes a low-cost, simple structure and high activity polymerization process. The molecular weight and stereoregulation of the product can be adjusted, suitable for industrial large-scale preparation, and the initiator can be used at room temperature and stored in a non-inert atmosphere.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005050406190000081
    Figure BDA0005050406190000081
  • Figure BDA0005050406190000091
    Figure BDA0005050406190000091
  • Figure BDA0005050406190000092
    Figure BDA0005050406190000092
Patent Text Reader

Abstract

The invention discloses a preparation method of polyolefin ether, and belongs to the technical field of polymer preparation. The preparation method comprises the following steps: mixing an initiator with an alkylene ether monomer, and precipitating by using an inert solvent after the reaction is completed, so as to obtain the polyolefin ether, the initiator comprises trifluoromethyl sulfonate. Aiming at the defects that an initiator for cationic polymerization of ether monomers is high in preparation cost, not easy to obtain and store, not suitable for industrial-scale generation of corresponding high polymer materials and the like, the invention provides a trifluoromethyl sulfonate initiator which is low in cost, simple in structure, high in activity and very convenient to use; the cationic polymerization principle for initiating ether monomers is simple, the operation is easy, polymerization can be performed at room temperature, the molecular weight and molecular weight distribution of the product can be regulated and controlled, the performance is excellent, and the cationic polymerization initiator can be applied to the fields of thermoplastics, rubber, elastomers, adhesives, coatings, chemical additives and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer preparation, and in particular relates to a method for preparing polyolefin ether. Background Art

[0002] Ether monomers based on petrochemicals and bio-fermentation (such as vinyl methyl ether, vinyl ethyl ether, vinyl butyl ether, vinyl isobutyl ether, vinyl cyclohexane ether, allyl ethyl ether, vinyl n-octyl ether, vinyl dodecyl ether, vinyl octadecyl ether, 2,3-dihydrofuran, 3,4-dihydropyran, 1,3-dioxolane, etc.) are widely present in the chemical industry, and many polymer materials with practical value can be obtained through cationic polymerization. At present, the initiators / starters used for the polymerization of such monomers mainly include Lewis acids (including but not limited to titanium tetrachloride, ferric chloride, zinc dichloride, silver hexafluoroantimonate, etc.), non-metallic reagents (such as trifluoromethanesulfonic acid / ester / anhydride, cyclopentadiene-1,2,3,4,5-pentacarboxylic acid methyl ester), and salts that can be photoinduced to generate cations (such as tetrafluoroborate, etc.). These chemical initiators / starters all need to be used in relatively harsh reaction or production environments, such as anhydrous and oxygen-free conditions. At the same time, some initiators / starters are relatively expensive (such as silver hexafluoroantimonate, tetrafluoroborate, cyclopentadiene-1,2,3,4,5-pentacarboxylic acid methyl ester), which are not suitable for industrial mass production; some initiators / starters are not easy to preserve, such as titanium tetrachloride, ferric chloride, etc., which are easily affected by moisture and water absorption in general environments, thereby deteriorating, and cannot be used on a large scale for large-scale low-cost preparation of polyether polymer materials, thereby limiting the widespread application of such materials. Summary of the invention

[0003] In order to solve the above problems in the prior art, the present invention provides a method for preparing polyolefin ether.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing polyolefin ether, comprising mixing an initiator with an olefin ether monomer, and performing precipitation with an inert solvent after the reaction is completed, to obtain the polyolefin ether;

[0006] The initiator includes triflate.

[0007] As a preferred embodiment of the present invention, a ligand is also added when the initiator and the olefin ether monomer are mixed.

[0008] As a preferred embodiment of the present invention, the olefin ether monomer includes one or more of vinyl methyl ether, vinyl ethyl ether, vinyl butyl ether, vinyl cyclohexane ether, ethyl propylene ether, long-chain alkyl propylene ether, 2,3-dihydrofuran, 3,4-dihydropyran, tetrahydrofuran and 1,3-dioxolane.

[0009] As a preferred embodiment of the present invention, the trifluoromethanesulfonate includes one or more of lithium trifluoromethanesulfonate, sodium trifluoromethanesulfonate, potassium trifluoromethanesulfonate, magnesium trifluoromethanesulfonate, calcium trifluoromethanesulfonate, aluminum trifluoromethanesulfonate, barium trifluoromethanesulfonate, zinc trifluoromethanesulfonate, nickel trifluoromethanesulfonate, cobalt trifluoromethanesulfonate, ferrous trifluoromethanesulfonate, iron trifluoromethanesulfonate, tin trifluoromethanesulfonate, lead trifluoromethanesulfonate, copper trifluoromethanesulfonate, mercuric trifluoromethanesulfonate, gallium trifluoromethanesulfonate, boron trifluoromethanesulfonate, scandium trifluoromethanesulfonate, ammonium trifluoromethanesulfonate, manganese trifluoromethanesulfonate, silver trifluoromethanesulfonate and pyridine trifluoromethanesulfonate.

[0010] The above olefin ether monomers are all commonly used monomers in polymer chemical industry and can be obtained commercially (purchased from reagent manufacturers). The above trifluoromethanesulfonate initiators / starters initiate addition polymerization of olefin ether monomers by generating cations, and follow the cationic ring-opening polymerization mechanism to generate polymer products.

[0011] As a preferred embodiment of the present invention, the initiator and the olefin ether monomer are mixed in the following manner: directly mixing the olefin ether monomer and the initiator, or adding the initiator into an organic solvent and then adding the olefin ether monomer, or adding the olefin ether monomer into an organic solvent and then adding the initiator; the organic solvent includes a halogenated hydrocarbon reagent, a benzene reagent, an ether reagent or dimethyl sulfoxide.

[0012] As a preferred embodiment of the present invention, the initiator, the ligand and the olefin ether monomer are mixed in the following manner: directly mixing the olefin ether monomer with the initiator and the ligand, or adding the initiator and the ligand into an organic solvent and then adding the olefin ether monomer, or adding the olefin ether monomer into an organic solvent and then adding the initiator and the ligand; the organic solvent includes a halogenated hydrocarbon reagent, a benzene reagent, an ether reagent or dimethyl sulfoxide.

[0013] As a preferred embodiment of the present invention, the reaction temperature is -78 to 30°C and the reaction time is 0.5 to 48 hours.

[0014] As a preferred embodiment of the present invention, the molar ratio of the initiator to the olefin ether monomer is (0.1-10):1000; and the molar ratio of the ligand to the initiator is 1:1.

[0015] As a preferred embodiment of the present invention, the ligand includes ethylene glycol dimethyl ether, ethylene glycol diethyl ether, dimethoxymethane, 4,4'-bispyridine, pentamethyldiethylenetriamine, 2,2'-dimethoxy-1,1'-binaphthyl, 2,3,5,6-tetrahydronaphtho[2,1-H:1,2-J][1,4,7]trioxacycloundecone, binaphthol diacetate, 2,2'-bis(methoxymethoxy)-1,1'-binaphthyl, 2,2' -dimethoxymethoxy-3,3'-dimethyl-1,1'-binaphthyl, 3,3'-dibromo-2,2'-di(methoxymethoxy)-1,1'-binaphthyl, 2,2'-bis(methoxymethoxy)-3,3'-diphenyl-1,1'-binaphthyl, 2,2'-dimethoxy-3,3'-diphenyl-1,1'-binaphthyl and one or more of piperidine; the inert solvent comprises one or more of methanol, ethanol and isopropanol.

[0016] The present invention also provides a polyolefin ether prepared according to the above-mentioned preparation method.

[0017] The present invention also provides a use of the polyolefin ether described above in thermoplastic plastics, rubber, elastomer, adhesive, coating or chemical additive.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The present invention aims to solve the shortcomings of the initiators or starters for the cationic polymerization of corresponding olefin ether monomers in literature and related patent reports, such as high preparation cost, difficulty in obtaining, difficulty in storage, and unsuitability for industrial-scale production of corresponding polymer materials. The present invention introduces a trifluoromethylsulfonate initiator / starter with low cost, simple structure, high activity and very convenient use. The initiator has a simple principle for initiating cationic polymerization of ether monomers and is easy to operate. The polymerization can be carried out at room temperature, and the molecular weight (200 to 500,000 Daltons) and molecular weight distribution (1.08 to 8) of the product can be controlled.

[0020] (2) The present invention can initiate polymerization in both bulk and solution states of the monomer. By directly adding a ligand in an equimolar amount to the above-mentioned initiator / starter, the chain transfer reaction can be effectively inhibited, thereby increasing the molecular weight of the product and effectively regulating the stereoregularity of the monomer unit (the isotacticity can reach more than 80%). Among them, in the bulk state, the amount of initiator used can be as low as 0.1% mole (relative to the molar amount of the monomer). These trifluoromethylsulfonate initiators / starters can initiate polymerization when exposed to air and can be stored in an atmosphere of non-inert gas (such as nitrogen, helium, etc.) (deterioration is less than 1% by weight after 6 months). In summary, the trifluoromethylsulfonate initiator / starter introduced by the present invention can efficiently initiate the polymerization of ether monomers and produce practical polyether polymer materials on a large scale. DETAILED DESCRIPTION

[0021] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0022] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0023] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0024] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0025] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0026] In the following examples, room temperature refers to 23° C., and the raw materials used are all commercially available conventional raw materials, without any special limitation. The following description will not be repeated.

[0027] Example 1

[0028] Weigh iron trifluoromethanesulfonate (50 mg, 0.1 mmol) and place it in a flask, and add a mechanical stirring paddle. Measure vinyl ethyl ether (7.2 g, 0.1 mol) and slowly drip it into the flask at room temperature, and then stir at room temperature for 3 hours. Add 20 μl of diethylamine to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate a polymer.

[0029] Remove the solvent, dry the product, weigh 7 grams of the product, and the yield is more than 97%. Product structure information: H NMR spectrum,1 H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 64%. Gel permeation chromatography (GPC), weight average molecular weight 32,000 Daltons, number average molecular weight 16,000 Daltons, molecular weight distribution 2. Differential scanning calorimetry (DSC), glass transition temperature -33°C.

[0030] Example 2

[0031] Weigh iron trifluoromethanesulfonate (50 mg, 0.1 mmol) and place it in a flask, and add a mechanical stirring paddle. Measure vinyl ethyl ether (14.4 g, 0.2 mol) and slowly drip it into the flask at room temperature, and then stir at room temperature for 3 hours. Add 150 μL of diethylamine to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate a polymer.

[0032] The solvent was removed, the product was dried, and 13.9 g of the product was weighed, with a yield of more than 97%. Product structure information: H NMR spectrum, 1 H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 54%. Gel permeation chromatography (GPC), weight average molecular weight 60,000 Daltons, number average molecular weight 25,000 Daltons, molecular weight distribution 2.4. Differential scanning calorimetry (DSC), glass transition temperature -35°C.

[0033] Example 3

[0034] Weigh iron trifluoromethanesulfonate (ferric iron) (50 mg, 0.1 mmol), put it into a flask, and add a mechanical stirring paddle. Measure vinyl ethyl ether (3.6 g, 0.05 mol) and slowly drip it into the flask at room temperature, then stir at room temperature for 6 hours. Add 10 microliters of diethylamine to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate a polymer.

[0035] The solvent was removed, the product was dried, and 3.5 g of the product was weighed, with a yield of more than 97%. Product structure information: H NMR spectrum, 1H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 68%. Gel permeation chromatography (GPC), weight average molecular weight 18,000 Daltons, number average molecular weight 12,000 Daltons, molecular weight distribution 1.5. Differential scanning calorimetry (DSC), glass transition temperature -24°C.

[0036] Example 4

[0037] Weigh iron trifluoromethanesulfonate (50 mg, 0.1 mmol) and place it in a flask, add a mechanical stirring paddle. Place the flask in an ice-water bath and maintain it at 0°C. Measure vinyl ethyl ether (7.2 g, 0.1 mol) and slowly drip it into the flask, then stir at 0°C for 3 hours. Add 10 μL of ethanol to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate the polymer.

[0038] The solvent was removed, the product was dried, and 6.7 g of the product was weighed, with a yield of more than 93%. Product structure information: H NMR spectrum, 1 H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 57%. Gel permeation chromatography (GPC), weight average molecular weight 40,000 Daltons, number average molecular weight 25,000 Daltons, molecular weight distribution 1.6. Differential scanning calorimetry (DSC), glass transition temperature -36°C.

[0039] Example 5

[0040] Weigh iron trifluoromethanesulfonate (50 mg, 0.1 mmol), put it into a flask, and add a mechanical stirring paddle. Place the flask in a low-temperature bath and maintain it at -20°C. Measure vinyl ethyl ether (7.2 g, 0.1 mol) and slowly drip it into the flask at -20°C, then stir at -20°C for 6 hours. Add 50 microliters of diethylamine to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate the polymer. Remove the solvent, dry the product, and weigh 6.8 grams of the product, with a yield of more than 94%. Product structure information: H NMR spectrum, 1H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 68%. Gel permeation chromatography (GPC), weight average molecular weight 68,000 Daltons, number average molecular weight 52,000 Daltons, molecular weight distribution 1.3. Differential scanning calorimetry (DSC), glass transition temperature -28°C.

[0041] Example 6

[0042] Weigh iron trifluoromethanesulfonate (50 mg, 0.1 mmol), put it into the flask, inject 50 ml of dimethoxymethane, then add 0.1 mmol of ligand (2,2'-dimethoxy-1,1'-binaphthyl), and put in a mechanical stirring paddle. Place the flask in a low temperature bath and maintain it at -50°C. Measure vinyl ethyl ether (7.2 g, 0.1 mol) and slowly drip it into the flask at -50°C, then stir at -50°C for 6 hours. Add 40 microliters of water to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate the polymer.

[0043] The solvent was removed, the product was dried, and 7.1 g of the product was weighed, with a yield of more than 98%. Product structure information: H NMR spectrum, 1 H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 84%. Gel permeation chromatography (GPC), weight average molecular weight 80,000 Daltons, number average molecular weight 74,000 Daltons, molecular weight distribution 1.08. Differential scanning calorimetry (DSC), glass transition temperature -27°C, melting point 104°C.

[0044] Example 7

[0045] Iron trifluoromethanesulfonate (50 mg, 0.1 mmol) was weighed and placed in a flask containing vinyl ethyl ether (7.2 g, 0.1 mol) with a mechanical stirring paddle in advance. The mixture was stirred at room temperature for 3 hours. 10 μL of methanol was added to quench the reaction. The mixture was then poured into an inert solvent (methanol) to precipitate a polymer.

[0046] The solvent was removed, the product was dried, and 7.1 g of the product was weighed, with a yield of more than 97%. Product structure information: H NMR spectrum, 1H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 52%. Gel permeation chromatography (GPC), weight average molecular weight 48,000 Daltons, number average molecular weight 6,000 Daltons, molecular weight distribution 8. Differential scanning calorimetry (DSC), glass transition temperature -38°C.

[0047] Example 8

[0048] Weigh iron trifluoromethanesulfonate (50 mg, 0.1 mmol) and add it to a flask containing vinyl ethyl ether (7.2 g, 0.1 mol) and 0.1 mmol of ligand (2,2'-bis(methoxymethoxy)-3,3'-diphenyl-1,1'-binaphthyl). Place a mechanical stirring paddle in the flask in advance. Then stir at room temperature for 3 hours. Add 10 microliters of methanol to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate the polymer.

[0049] The solvent was removed, the product was dried, and 6.9 g of the product was weighed, with a yield of more than 95%. Product structure information: H NMR spectrum, 1 H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 82%. Gel permeation chromatography (GPC), weight average molecular weight 66,000 Daltons, number average molecular weight 60,000 Daltons, molecular weight distribution 1.1. Differential scanning calorimetry (DSC), melting point 100°C.

[0050] By comparing Example 7 and Example 8, it can be seen that after adding the ligand, the molecular weight of the product is significantly increased, and the stereoregularity of the product is also significantly improved.

[0051] Example 9

[0052] Weigh iron trifluoromethanesulfonate (50 mg, 0.1 mmol), put it into a flask, inject 50 ml of ethylene glycol diethyl ether (which can also act as a ligand), and put in a mechanical stirring paddle. Measure vinyl ethyl ether (7.2 g, 0.1 mol) and slowly drip it into the flask at 0°C, then stir at 0°C for 3 hours. Add 10 microliters of diethylamine to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate the polymer.

[0053] The solvent was removed, the product was dried, and 6.8 g of the product was weighed, with a yield of more than 95%. Product structure information: H NMR spectrum, 1H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 83%. Gel permeation chromatography (GPC), weight average molecular weight 45,000 Daltons, number average molecular weight 42,000 Daltons, molecular weight distribution 1.07. Differential scanning calorimetry (DSC), glass transition temperature -21°C, melting point 102°C.

[0054] Example 10

[0055] Weigh iron trifluoromethanesulfonate (50 mg, 0.1 mmol), put it into a flask, inject 50 ml of ether, and add a mechanical stirring paddle. Measure vinyl ethyl ether (7.2 g, 0.1 mol) and slowly drip it into the flask at 0°C, then stir at 0°C for 3 hours. Add 10 μl of diethylamine to quench the reaction. Then pour the mixture into an inert solvent (methanol) to precipitate the polymer.

[0056] The solvent was removed, the product was dried, and 6.9 g of the product was weighed, with a yield of more than 95%. Product structure information: H NMR spectrum, 1 H NMR (400MHz, Chloroform-d), δ = 3.82-3.21 (m, 3H), 1.98-1.38 (m, 2H), 1.18 (t, J = 7.0Hz, 3H). Stereotacticity (isotacticity) meso content 73%. Gel permeation chromatography (GPC), weight average molecular weight 34,000 Daltons, number average molecular weight 28,000 Daltons, molecular weight distribution 1.21. Differential scanning calorimetry (DSC), glass transition temperature -24°C, melting point 100°C.

[0057] Embodiment 11

[0058] The preparation steps of polyether elastomer are as follows:

[0059] Weigh iron trifluoromethanesulfonate (ferric iron) (50 mg, 0.1 mmol), put it into a flask, and add a mechanical stirring paddle. Measure tetrahydrofuran (7.2 g, 0.1 mol) and slowly drip it into the flask at room temperature (23°C), and then stir it at room temperature for 3 hours. Take the mixed solution and observe the monomer conversion using a chromatograph or nuclear magnetic resonance spectrometer. Then pour the mixed solution into an inert solvent methanol to precipitate a polymer.

[0060] The solvent was removed, the product was dried, and 7 grams of the product was weighed, with a yield of more than 96%. Product structure information: H NMR spectrum, 1H NMR (400 MHz, Chloroform-d), δ = 3.42 (h, J = 3.1 Hz, 4H), 1.62 (dq, J = 6.1, 3.0 Hz, 4H). Gel permeation chromatography (GPC), weight average molecular weight 105,000 Daltons, number average molecular weight 71,000 Daltons, molecular weight distribution 1.48.

[0061] Other embodiments are listed in table form:

[0062] Table 1 Preparation of polyolefin ethers using vinyl isobutyl ether monomer (0.1 mol) as an example

[0063]

[0064]

[0065] Table 2 Preparation of polyolefin ethers using vinyl octadecyl ether monomer (0.1 mol) as an example

[0066]

[0067]

[0068] Table 3 Preparation of polyolefin ethers using 1,3-dioxolane monomer (0.1 mol) as an example

[0069]

[0070]

[0071]

[0072] In addition to the homopolymerization of these ether monomers, the present invention also copolymerizes two or more ether monomers. The copolymerization of vinyl methyl ether and vinyl dodecyl ether is taken as an example below.

[0073] Table 4 Preparation of polyolefin ether by polymerization with a molar ratio of 1:4 of vinyl methyl ether (0.025 mol) and vinyl dodecyl ether

[0074]

[0075]

[0076] The above description is only a preferred specific implementation manner of the present invention, and the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, and they should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a polyolefin ether, characterized in that: The initiator is mixed with the olefin ether monomer, and after the reaction is completed, precipitation is performed using an inert solvent to obtain the polyolefin ether; The initiator includes triflate.

2. The method for preparing polyolefin ether according to claim 1, characterized in that: When the initiator is mixed with the olefin ether monomer, the ligand is also added.

3. The method for preparing polyolefin ether according to claim 1, characterized in that: The olefin ether monomers include one or more of vinyl methyl ether, vinyl ethyl ether, vinyl butyl ether, vinyl cyclohexane ether, ethyl propylene ether, ethyl propylene ether, vinyl n-octyl ether, vinyl dodecyl ether, vinyl octadecyl ether, 2,3-dihydrofuran, 3,4-dihydropyran, tetrahydrofuran and 1,3-dioxolane.

4. The method for preparing polyolefin ether according to claim 1, characterized in that: The trifluoromethanesulfonate includes one or more of lithium trifluoromethanesulfonate, sodium trifluoromethanesulfonate, potassium trifluoromethanesulfonate, magnesium trifluoromethanesulfonate, calcium trifluoromethanesulfonate, aluminum trifluoromethanesulfonate, barium trifluoromethanesulfonate, zinc trifluoromethanesulfonate, nickel trifluoromethanesulfonate, cobalt trifluoromethanesulfonate, ferrous trifluoromethanesulfonate, iron trifluoromethanesulfonate, tin trifluoromethanesulfonate, lead trifluoromethanesulfonate, copper trifluoromethanesulfonate, mercuric trifluoromethanesulfonate, gallium trifluoromethanesulfonate, boron trifluoromethanesulfonate, scandium trifluoromethanesulfonate, ammonium trifluoromethanesulfonate, manganese trifluoromethanesulfonate, silver trifluoromethanesulfonate and pyridine trifluoromethanesulfonate.

5. The method for preparing polyolefin ether according to claim 1, characterized in that: The reaction temperature is -78 to 30°C, and the reaction time is 0.5 to 48 hours.

6. The method for preparing polyolefin ether according to claim 1, characterized in that: The molar ratio of the initiator to the olefin ether monomer is (0.1-10):1000; the molar ratio of the ligand to the initiator is 1:

1.

7. The method for preparing polyolefin ether according to claim 1, characterized in that: The ligands include ethylene glycol dimethyl ether, ethylene glycol diethyl ether, dimethoxymethane, 4,4'-bispyridine, pentamethyldiethylenetriamine, 2,2'-dimethoxy-1,1'-binaphthyl, 2,3,5,6-tetrahydronaphtho[2,1-H:1,2-J][1,4,7]trioxacycloundecone, binaphthol diacetate, 2,2'-bis(methoxymethoxy)-1,1'-binaphthyl, 2,2'-dimethoxymethoxy One or more of oxy-3,3'-dimethyl-1,1'-binaphthyl, 3,3'-dibromo-2,2'-di(methoxymethoxy)-1,1'-binaphthyl, 2,2'-bis(methoxymethoxy)-3,3'-diphenyl-1,1'-binaphthyl, 2,2'-dimethoxy-3,3'-diphenyl-1,1'-binaphthyl and piperidine; the inert solvent includes one or more of methanol, ethanol and isopropanol.

8. A polyolefin ether prepared according to the preparation method according to any one of claims 1 to 7.

9. Use of the polyolefin ether according to claim 8 in thermoplastics, rubbers, elastomers, adhesives, coatings or chemical additives.

Citation Information

Patent Citations

  • Improvements in or relating to poly (vinyl ethers) and preparation thereof

    GB820469A

  • Production of polyvinyl ethereal compound

    JP1994234805A

  • Polyvinyl ether based high performance synthetic fluids prepared using cationic polymerizwation

    US20130165360A1

  • Polymerizing vinyl alkyl ethers

    US2457661A