Overheating test method of sodium-nickel single battery
Through the overheating test method of sodium nickel single-body battery, the voltage-temperature curve is recorded by heating furnace temperature increase, which solves the problem of process abnormality not being recognized at room temperature, and realizes hot-pressing sealing, glass sealing and sealing of sodium nickel single-body battery Quick screening at nail welding ensures battery quality and reduces costs.
Patent Information
- Application Number
- CN202410987691.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art cannot identify abnormalities in sodium nickel single-body batteries at hot press seal, glass seal and sealing nail welding through open circuit voltage (OCV) detection at room temperature, resulting in the inability to effectively screen out batteries with abnormal processes.
The overheating test method of sodium-nickel single-body battery is used to judge the battery's qualification by heating the battery to 600°C in a heating furnace, recording the open circuit voltage and temperature changes, drawing the voltage-temperature curve, and reading the voltage sudden change temperature.
This method can quickly and conveniently identify abnormalities in the hot-press sealing, glass sealing and sealing nail welding of sodium nickel single-body batteries, ensuring the factory quality and low cost.
Smart Images

Figure CN118962472A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium-nickel battery detection, and in particular relates to an overheating test method for a sodium-nickel single battery. Background Art
[0002] The solid electrolyte inside the sodium-nickel single cell is a Na-β"-Al2O3 ceramic tube. During the battery production process, the ceramic tube needs to be hot-pressed, glass-sealed, and sealed with nails. When abnormalities occur at the hot-pressed seal, glass seal, and sealing nail welding (loose sealing, welding pinholes, etc.), the open circuit voltage has a significant mutation. At room temperature, the open circuit voltage (OCV) of batteries with abnormal sealing and welding is no different from that of normal batteries, and cannot be identified and screened through OCV testing. Therefore, it is very important to develop a sodium-nickel single cell detection method to feedback whether there are abnormalities in the three processes of hot-pressed sealing, glass sealing, and sealing nail welding. Summary of the invention
[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide an overheating test method for a sodium-nickel single cell battery, which can provide feedback on whether there are abnormalities in the three processes of hot pressing sealing, glass sealing and sealing pin welding of Na-β"-Al2O3 ceramic tubes, and the method has the advantages of being convenient, fast and low-cost.
[0004] To achieve the above objectives, the present invention provides the following technical solutions:
[0005] A method for overheating testing of a sodium-nickel single cell battery comprises the following steps:
[0006] (1) Place the sodium-nickel single battery to be tested in a heating furnace and heat it to 300°C for 4 hours, then heat it to 600°C at 100°C / h. During the heating process, record the open circuit voltage of the battery.
[0007] (2) Draw the open circuit voltage-temperature curve of the single cell according to the temperature change and the open circuit voltage change;
[0008] (3) Read the temperature Tm at which the battery open circuit suddenly changes according to the curve. If Tm>450°C, the single cell is qualified; if Tm<450°C, the single cell is unqualified.
[0009] Preferably, the sodium-nickel single battery is not formed.
[0010] Preferably, the maximum temperature of the heating furnace is greater than 600°C, and the heating rate is greater than 100°C / h.
[0011] Preferably, a temperature probe is provided at two positions in the middle and lower part of the same side of the sodium-nickel single battery to record the temperature.
[0012] Preferably, the battery voltage is collected by welding stainless steel wires to the positive and negative electrodes of the sodium-nickel single battery.
[0013] Preferably, the stainless steel wire is installed with a glass fiber sleeve to provide good insulation to prevent short circuit.
[0014] The beneficial effects of the present invention are:
[0015] At room temperature, abnormalities exist at the hot-pressing seal of the ceramic tube, the glass seal, and the sealing pin welding, making it impossible to use OCV detection to identify and screen the sodium-nickel single battery. The present invention performs overheat detection on the sodium-nickel single battery and obtains the sudden change temperature of the open circuit voltage according to the open circuit voltage versus temperature curve, thereby being able to quickly respond to whether there are abnormalities in the three processes of hot-pressing seal, glass seal, and sealing pin welding of the sodium-nickel single battery, and judge the factory quality of the sodium-nickel battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the sodium-nickel single battery heating device of the present invention, a left view (A) and a three-dimensional view (B).
[0017] Figure 2 This is the open circuit voltage-temperature curve of the sodium-nickel single battery in Example 1.
[0018] Figure 3 This is the open circuit voltage-temperature curve of the sodium-nickel single battery in Example 2. DETAILED DESCRIPTION
[0019] In order to make the technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0020] Example 1
[0021] A method for overheating testing of a sodium-nickel single cell battery comprises the following steps:
[0022] The unformed sodium-nickel single battery is placed in a heating furnace 1 for heating. Figure 1 As shown, the sodium-nickel single battery 2 is placed in the heating furnace from the top of the heating furnace, heaters 3 are evenly distributed around the battery, the heating furnace is sealed by a top cover 4, and the heating furnace also includes a control box 5.
[0023] The control box sets the heating furnace to heat up to 300°C in 4 hours, and then to 600°C at 100°C / h. During the heating process, the open circuit voltage of the battery is recorded. A temperature probe is set at the middle and lower positions on the same side of the sodium-nickel single battery to record the temperature. The open circuit voltage is collected by welding stainless steel wires to the positive and negative electrodes of the battery, and the stainless steel wires are insulated with glass fiber sleeves to prevent short circuits.
[0024] Draw the open circuit voltage-temperature curve of the single cell according to the temperature change and open circuit voltage change. The result is as follows: Figure 2 As shown, from Figure 2 The curve shows that the temperature Tm at which the battery open circuit mutation occurs is around 570°C, so the sodium-nickel single battery tested is qualified.
[0025] Example 2
[0026] A method for overheating testing of a sodium-nickel single cell battery comprises the following steps:
[0027] The unformed sodium-nickel single battery is placed in a heating furnace 1 for heating. Figure 1 As shown, the sodium-nickel single battery 2 is placed in the heating furnace from the top of the heating furnace, heaters 3 are evenly distributed around the battery, the heating furnace is sealed by a top cover 4, and the heating furnace also includes a control box 5.
[0028] The control box sets the heating furnace to heat up to 300°C in 4 hours, and then to 600°C at 100°C / h. During the heating process, the open circuit voltage of the battery is recorded. A temperature probe is set at the middle and lower positions on the same side of the sodium-nickel single battery to record the temperature. The open circuit voltage is collected by welding stainless steel wires to the positive and negative electrodes of the battery, and the stainless steel wires are insulated with glass fiber sleeves to prevent short circuits.
[0029] Draw the open circuit voltage-temperature curve of the single cell according to the temperature change and open circuit voltage change. The result is as follows: Figure 3 As shown, from Figure 3 The curve shows that the temperature Tm at which the battery open circuit mutation occurs is 400°C, so the sodium-nickel single battery tested is unqualified.
[0030] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for overheating test of sodium nickel single battery, characterized in that: The steps include: (1) Place the sodium-nickel single battery to be tested in a heating furnace and heat it to 300°C for 4 hours, then heat it to 600°C at 100°C / h. During the heating process, record the open circuit voltage of the battery. (2) Draw the open circuit voltage-temperature curve of the single cell according to the temperature change and the open circuit voltage change; (3) Read the temperature Tm at which the battery open circuit suddenly changes according to the curve. If Tm>450°C, the single cell is qualified; if Tm<450°C, the single cell is unqualified.
2. The overheating test method of a sodium-nickel single battery according to claim 1, characterized in that: The sodium-nickel single cell was not formed.
3. The overheating test method of a sodium-nickel single battery according to claim 1, characterized in that: The maximum temperature of the heating furnace is greater than 600° C., and the heating rate is greater than 100° C. / h.
4. The overheating test method of a sodium-nickel single battery according to claim 1, characterized in that: A temperature probe is respectively arranged at two positions on the same side of the sodium-nickel single battery to record the temperature.
5. The overheating test method of a sodium-nickel single battery according to claim 1, characterized in that: Stainless steel wires are welded to the positive and negative electrodes of the sodium-nickel single battery to collect the battery voltage.
6. The overheating test method of a sodium-nickel single battery according to claim 5, characterized in that: The stainless steel wire is installed with a glass fiber casing to ensure good insulation to prevent short circuit.