Positive electrode material, preparation method thereof and electrochemical device
By forming a two-component coating of fast ion conductors and metal oxides on the surface of the ternary positive electrode material, gradient design and wet spray coating technology, the structural stability and cyclic performance problems of the ternary positive electrode material are solved, and a higher level of performance is achieved rate performance and long-term stability.
Patent Information
- Application Number
- CN202411003856.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
AI Technical Summary
During long-term use of ternary positive electrode materials, there are problems of poor structural stability, circulation performance and thermal stability, and existing surface modification methods cannot effectively solve these problems.
Using a two-component coating containing fast ion conductors and metal oxides, the concentration gradient of fast ion conductors gradually increases from outside to inside in the radial direction, and the concentration gradient of metal oxides gradually decreases from outside to inside, and is formed by wet spray coating technology. Composite coating improves lithium ion transmission rate and isolates electrolyte corrosion.
The surface structural stability and cyclic performance of the positive electrode material are improved, the hidden danger of coating stress concentration is reduced, and the rate performance and long-term cyclic stability are improved.
Smart Images

Figure CN118969982A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of new energy materials, and in particular to a positive electrode material and a preparation method thereof, and an electrochemical device. Background Art
[0002] Ternary cathode materials mainly refer to composite oxides containing nickel (Ni), cobalt (Co), manganese (Mn) or aluminum (Al), such as LiNiCoMnO2 or LiNiCoAlO2, which are important cathode materials in lithium-ion batteries. The above ternary cathode materials show good comprehensive performance in terms of energy density, cycle stability and safety, so they are widely used in electric vehicles, energy storage systems and other fields.
[0003] However, there are some key problems in the long-term use of ternary positive electrode materials, which limit their performance and lifespan, such as poor structural stability, cycle performance and thermal stability, as well as defects such as interfacial side reactions and metal dissolution. Summary of the invention
[0004] In view of this, in order to solve at least one of the above technical problems, an embodiment of the present application provides a positive electrode material.
[0005] In addition, the embodiments of the present application also provide a method for preparing the aforementioned positive electrode material, and an electrochemical device using the positive electrode material.
[0006] An embodiment of the present application provides a positive electrode material, comprising a core and a coating located on the surface of the core, wherein the core is a ternary positive electrode material, the coating contains a fast ion conductor and a metal oxide, and the concentration gradient of the fast ion conductor gradually increases radially from the outside to the inside of the coating, and the concentration gradient of the metal oxide gradually decreases radially from the outside to the inside of the coating.
[0007] In some possible embodiments, the fast ion conductor includes an M element, the M element includes at least one of Ge, La, Zr, Al, Ti, As, Nb, Ta and Ca, and the M element exists in the form of at least one of an oxide, a sulfide, a phosphate and a sulfide-phosphate complex.
[0008] In some possible embodiments, the fast ion conductor includes Li 10 GeP2S 12 、Li7La3Zr2O 12 and Li 1.3 Al 0.3 Ti 1.7 At least one of (PO4)3.
[0009] In some possible embodiments, the metal oxide includes at least one of ZrO2, La2O3, Al2O3 and TiO2.
[0010] The present application also provides a method for preparing a positive electrode material, comprising:
[0011] Spray coating the fast ion conductor slurry and the metal oxide slurry on the ternary positive electrode material matrix at the same time to obtain a positive electrode material precursor, wherein as the spray coating time increases, the spraying speed of the fast ion conductor slurry gradually decreases, and the spraying speed of the metal oxide slurry gradually increases; and
[0012] The positive electrode material precursor is sintered to obtain the positive electrode material.
[0013] In some possible embodiments, the injection speed is measured by the liquid inlet rotation speeds of the fast ion conductor slurry and the metal oxide slurry. The liquid inlet rotation speed of the fast ion conductor slurry is initially 60rpm~100rpm, and gradually decreases at a rate of change of 0.5rpm / min~2rpm / min. The liquid inlet rotation speed of the metal oxide slurry is initially 0~20rpm, and gradually increases at a rate of change of 0.5rpm / min~2rpm / min.
[0014] In some possible embodiments, the spray coating time is 0.5h to 1.5h, the spray coating temperature is 150°C to 300°C, and after the spray coating is completed, the temperature is kept at 150°C to 300°C for 10min to 60min.
[0015] In some possible embodiments, the method for preparing the positive electrode material satisfies at least one of the following conditions:
[0016] The fast ion conductor includes an M element, wherein the M element includes at least one of Ge, La, Zr, Al, Ti, As, Nb, Ta and Ca, and the M element exists in the form of at least one of an oxide, a sulfide, a phosphate and a sulfide-phosphate complex;
[0017] The fast ion conductor includes Li 10 GeP2S 12 、Li7La3Zr2O 12 and Li 1.3 Al 0.3 Ti 1.7 At least one of (PO4)3;
[0018] The metal oxide includes at least one of ZrO2, La2O3, Al2O3 and TiO2.
[0019] In addition, an embodiment of the present application further provides an electrochemical device, which includes a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the positive electrode plate includes a positive electrode active substance, and the positive electrode active substance is the aforementioned positive electrode material.
[0020] Compared with the prior art, the cathode material provided in the embodiment of the present application has a dual-phase coating with uniform thickness, which reduces the surface defects of the cathode material and improves the surface structural stability of the cathode material. The coating contains two phases, a fast ion conductor and a metal oxide, which are mixed to form an integrated composite coating structure. Compared with the dual coating structure in which the two substances are directly formed into coatings, the problem of sudden change in thermal expansion coefficient between the coatings is solved, and the hidden danger of stress concentration in the coating during long-term circulation is effectively reduced, and the long-term surface stability of the cathode material is improved.
[0021] Moreover, the concentration of each phase in the dual-phase component coating is gradient. The inner layer is designed with a high fast ion conductor concentration to increase the lithium ion transmission rate and improve the rate performance of the positive electrode material; the outer layer is designed with a high metal oxide concentration gradient to isolate the electrolyte corrosion function and improve the cycle performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A process flow chart of the method for preparing the positive electrode material provided in an embodiment of the present application.
[0023] Figure 2 This is a schematic diagram of the structure of the electrochemical device provided in an embodiment of the present application.
[0024] Figure 3 This is a scanning electron microscope image of the positive electrode material of Example 1 of the present application.
[0025] Figure 4 This is a scanning electron microscope image of the positive electrode material of comparative example 1 of the present application.
[0026] Figure 5 It is a comparison chart of the cycle capacity retention rate curves at 45°C of batteries prepared with the positive electrode materials in Example 1 of the present application and Comparative Examples 1-4. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0028] Ternary cathode materials show good comprehensive performance in terms of energy density, cycle stability and safety. However, ternary cathode materials have problems such as poor structural stability and poor cycle performance during long-term use. In order to overcome the above problems, it is common to form a coating on the surface of ternary materials through surface modification to improve the long-term performance and life of ternary cathode materials.
[0029] However, the inventors of the present application have found that the above-mentioned problems of ternary positive electrode materials cannot be effectively solved by adopting a single-phase coating modification method. For example, the coating modification of ternary positive electrode materials with metal oxides can isolate the infiltration of electrolyte, but also hinder the transmission path of lithium ions, forming interface impedance, causing the positive electrode material to lose its initial capacity and reducing the energy density of the positive electrode material. The use of a double coating system, such as a fast ion conductor-conductive polymer double coating, has both excellent cycle performance and good rate performance, but due to the difference in thermal expansion coefficients between the two coating layers, it will cause stress concentration between the coatings, resulting in cracks and damage or even peeling of the coating during long-term cycling, causing long-term performance failure of the positive electrode material.
[0030] To this end, the positive electrode material provided in the embodiment of the present application includes a core and a coating located on the surface of the core, wherein the core is a ternary positive electrode material, the coating contains a fast ion conductor and a metal oxide, and the concentration gradient of the fast ion conductor gradually increases from the outside to the inside of the coating along the radial direction, and the concentration gradient of the metal oxide gradually decreases from the outside to the inside of the coating along the radial direction. That is, the coating is a composite coating of a two-component phase containing a fast ion conductor and a metal oxide, and is structurally a single coating, which can effectively solve the problem of capacity attenuation and cycle performance deterioration of the ternary positive electrode material in high-voltage long-term cycle use scenarios.
[0031] On the one hand, the composite coating with uniform thickness reduces the surface defects of the positive electrode material and improves the surface structural stability of the positive electrode material; and the composite coating structure formed by mixing the two phases solves the problem of sudden change in thermal expansion coefficient between coatings compared to the double coating structure in which the two substances are directly formed into coatings separately, effectively reducing the hidden danger of stress concentration in the coating during the long-term cycle of the positive electrode material and improving the long-term surface stability of the positive electrode material.
[0032] On the other hand, the concentration gradient change of the two-phase components in the coating further improves the problem of thermal expansion coefficient mutation between the coatings, and forms a structure of inner layer high fast ion conductor concentration-outer layer high metal oxide concentration gradient: the inner layer high fast ion conductor concentration design can shorten the lithium ion transmission path, effectively improve the lithium ion transmission rate in the positive electrode material, thereby improving the rate performance of the positive electrode material. This is because the fast ion conductor is conducive to the rapid transport of Li + , the positive electrode material is modified to a certain extent, the surface structure of the positive electrode material is stabilized, and Li is formed near the inner core surface.+ The element gradient forms a thin transition interface area to make the coating more compatible with the core material; at the same time, the high metal oxide concentration gradient design of the outer layer can effectively isolate the electrolyte from erosion, thereby improving the cycle performance of the positive electrode material. This is because during long-term cyclic use, the solvents and additives in the electrolyte may react with the positive electrode material, resulting in deterioration of battery performance. The metal oxide passivation layer can effectively isolate the electrolyte from corroding the transition layer metal inside the positive electrode material and inhibit the side reaction between the electrolyte and the positive electrode material.
[0033] In some embodiments, the fast ion conductor may include an M element, which may include at least one of Ge, La, Zr, Al, Ti, As, Nb, Ta, and Ca, etc. The M element may exist in the form of at least one of oxides, sulfides, phosphates, and sulfide-phosphate complexes, etc., that is, the fast ion conductor may be an oxide, sulfide, phosphate, and sulfide-phosphate complex of the M element. The above fast ion conductors all have high ionic conductivity and high thermal stability.
[0034] In some embodiments, the fast ion conductor may include Li 10 GeP2S 12 (LGPS), Li7La3Zr2O 12 (LLZO) and Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP), etc. Selecting fast ion conductors such as LGPS, LLZO and LATP with high ionic conductivity and chemical stability as components of the ternary cathode material coating can significantly improve the performance and stability of the cathode material, including increasing the ion transfer rate, enhancing chemical and thermal stability, and reducing the capacity attenuation and safety hazards of the prepared battery.
[0035] In some embodiments, the metal oxide may include at least one of ZrO2, La2O3, Al2O3, and TiO2, etc. The above metal oxides are chemically inert and can effectively block direct contact between the positive electrode material and the electrolyte, avoid dissolution of the core metal, reduce the destruction of the crystal structure of the positive electrode material, and improve the thermal stability and cycle performance of the positive electrode material.
[0036] In some embodiments, the thickness of the coating can be 10nm to 200nm. Within the above range, it can avoid the situation where the coating is too thin (less than 10nm) and cannot effectively isolate the electrolyte or provide sufficient ionic conductivity; at the same time, it can also avoid the situation where the internal impedance of the positive electrode material increases due to the coating being too thick (greater than 200nm), thereby affecting the energy density and overall performance of the positive electrode material.
[0037] In some embodiments, the core of the ternary positive electrode material may include one of a nickel-cobalt-manganese ternary positive electrode material and a nickel-cobalt-aluminum ternary positive electrode material, and the ternary positive electrode material may further include LiNi x Co y Mn 1-x-y O2, wherein 0.5≤x≤0.8, 0≤y≤0.25, and illustratively may be LiNi 0.5 Co 0.25 Mn 0.25 O2、LiNi 0.62 Co 0.2 Mn 0.18 O2、LiNi 0.7 Co 0.1 Mn 0.2 O2 or LiNi 0.8 Co 0.1 Mn 0.1 O2, etc. It can be understood that the types of ternary positive electrode materials include but are not limited to the above range.
[0038] Compared with the prior art, the positive electrode material provided in the embodiment of the present application has the following beneficial effects:
[0039] 1. The composite coating design contains a dual-component phase of a fast ion conductor and a metal oxide. The coating is a structurally single integrated coating, which effectively reduces the hidden danger of stress concentration in the coating during long-term cycling and improves the surface structural stability of the positive electrode material.
[0040] 2. The inner layer high-fast ion conductor concentration gradient design shortens the lithium ion transmission path and improves the lithium ion transmission rate and rate performance of the positive electrode material.
[0041] 3. The outer layer has a high metal oxide concentration gradient design, which effectively isolates the electrolyte from corroding the core of the positive electrode material and improves the cycle performance of the positive electrode material.
[0042] See also Figure 1 As shown, the preparation method of the positive electrode material provided in the embodiment of the present application specifically includes the following steps:
[0043] Step S1, spray-coating the fast ion conductor slurry and the metal oxide slurry on the ternary positive electrode material matrix at the same time to obtain a positive electrode material precursor, wherein as the spray coating time increases, the spraying speed of the fast ion conductor slurry gradually decreases, and the spraying speed of the metal oxide slurry gradually increases.
[0044] Specifically, wet spray coating is adopted, and the spraying method can be to use a pump to extract the slurry and spray it evenly on the ternary material matrix. Compared with dry coating, the coating effect of wet spray is more uniform. During the wet spray coating process, the fast ion conductor slurry and the metal oxide slurry are sprayed separately. By adjusting the material injection speed and then adjusting the coating rate, the initial fast ion conductor slurry injection speed is controlled to be faster during the spray process, and the initial metal oxide slurry injection speed is slower. During the spray coating process, the fast ion conductor slurry injection speed gradually decreases, and the metal oxide slurry injection speed gradually increases. In this way, as the spray coating time increases, the concentration of the fast ion conductor in the coating gradually decreases, and the concentration of the metal oxide in the coating gradually increases, thereby realizing the change of the coating concentration gradient, and obtaining a composite coating with a gradient concentration of two components, constructing a high fast ion conductor concentration in the inner layer and a high metal oxide concentration gradient design in the outer layer, improving the coating structure stability, and improving the rate performance of the ternary positive electrode material and the stability during long-term cycling.
[0045] It is understood that the spray coating method includes but is not limited to the above method, and any method that can achieve spray coating of the ternary material matrix is acceptable. For example, a peristaltic pump can be used to extract the slurry, and a centrifugal rotating nozzle can be rotated at high speed to form physical droplets, so that the slurry is evenly dispersed on the ternary material matrix to be coated under the action of centrifugation.
[0046] In some embodiments, the injection rate of the fast ion conductor slurry and the injection rate of the metal oxide slurry can be measured by the liquid feeding speed of the slurry.
[0047] Among them, the initial liquid inlet speed of the fast ion conductor slurry can be 60rpm~100rpm, and can further be 60rpm~80rpm, and can be 60rpm, 70rpm, 80rpm, 90rpm or 100rpm, etc.; the speed can be gradually reduced at a rate of change of 0.5rpm / min~2rpm / min, and the rate of change can further be 1rpm / min~2rpm / min, and can be 0.5rpm / min, 1rpm / min, 1.5rpm / min or 2rpm / min, etc.
[0048] The liquid inlet speed of the metal oxide slurry can be initially 0-20rpm, and can further be 10rpm-20rpm, and can be exemplarily 0, 5rpm, 10rpm, 15rpm or 20rpm, etc.; the speed can be gradually increased at a rate of change of 0.5rpm / min-2rpm / min, and the rate of change can further be 1rpm / min-2rpm / min, and can be exemplarily 0.5rpm / min, 1rpm / min, 1.5rpm / min or 2rpm / min, etc.
[0049] Within the above-mentioned liquid inlet speed control parameter range, the wet spray process can effectively achieve uniform two-phase concentration gradient coating of the ternary positive electrode material matrix.
[0050] In some embodiments, the spray coating temperature is 150°C to 300°C, and may further be 200°C to 250°C, and may be 150°C, 200°C, 250°C or 300°C, etc. Within the above-defined range, it is beneficial for the auxiliary material droplets to dry quickly to form a gradual concentration gradient coating.
[0051] In some embodiments, the spray coating time may be 0.5h to 1.5h, further may be 0.6h to 1h, illustratively may be 0.5h, 0.6h, 0.67h, 0.7h, 0.8h, 0.9h, 1h, 1.1h, 1.2h, 1.3h, 1.4h or 1.5h, etc. Within the above-defined range, the gradient coating of the ternary cathode material matrix can be completed.
[0052] In some embodiments, after the spray coating is completed, the temperature can be kept at 150° C. to 300° C. for 10 min to 60 min, which is beneficial for further drying the moisture in the auxiliary material.
[0053] In some embodiments, the spray coating process can be combined with a coating machine, and the coating machine can provide heating and heat preservation. For example, the coating machine can be a plow coater. During the spraying process, the plow always keeps the ternary cathode material substrate material in a stirring state. The plow coater jacket can be heated by oil temperature to maintain a certain spray coating temperature to achieve the effect of rapid drying of auxiliary material droplets. After the spraying is completed, the plow coater can continue to heat for a period of time to dry the moisture in the auxiliary material.
[0054] In some embodiments, the fast ion conductor includes an M element, wherein the M element includes at least one of Ge, La, Zr, Al, Ti, As, Nb, Ta, and Ca, and the M element exists in the form of at least one of an oxide, a sulfide, a phosphate, and a sulfide-phosphate complex. For example, the fast ion conductor may include Li 10 GeP2S 12 (LGPS), Li7La3Zr2O 12 (LLZO) and Li 1.3 Al 0.3 Ti 1.7 At least one of (PO4)3(LATP), etc. The above materials all have high ionic conductivity and chemical stability, which are beneficial to improving the electrochemical performance and stability of the positive electrode material.
[0055] In some embodiments, the metal oxide may include at least one of ZrO2, La2O3, Al2O3, and TiO2, etc. The above metal oxides are chemically inert and can effectively block direct contact between the positive electrode material and the electrolyte, thereby improving the thermal stability and cycle performance of the positive electrode material.
[0056] In some embodiments, the fast ion conductor slurry and the metal oxide slurry can be obtained by mixing a certain amount of fast ion conductor and metal oxide with a dispersant according to the coating process design. The dispersant can be water. Water as a dispersant is conducive to the implementation of the subsequent drying step, reduces impurities, and does not involve other high-cost or harmful solvents, which can reduce costs and simplify operations.
[0057] For example, the fast ion conductor and the metal oxide are mixed with the dispersant to obtain the fast ion conductor slurry and the metal oxide slurry respectively by stirring and dispersing in a mechanical stirring kettle, wherein the volume of the stirring kettle can be 1m 3 ~5m 3 The volume proportion of the fast ion conductor slurry and the metal oxide slurry can both be 1 / 3 to 2 / 3 of the container, so as to obtain a suspension system slurry with good solute dispersion, uniform composition, stable system and good fluidity.
[0058] In some embodiments, the solid content of the fast ion conductor slurry and the metal oxide slurry may be 5% to 20% by weight.
[0059] In some embodiments, the ternary cathode material matrix may include one of a nickel-cobalt-manganese ternary cathode material and a nickel-cobalt-aluminum ternary cathode material, and the ternary cathode material matrix may further include LiNi x Co y Mn 1-x-y O2, wherein 0.5≤x≤0.8, 0≤y≤0.25, and illustratively may be LiNi 0.5 Co 0.25 Mn 0.25 O2、LiNi 0.62 Co 0.2 Mn 0.18 O2、LiNi 0.7 Co 0.1 Mn 0.2 O2 or LiNi 0.8 Co 0.1 Mn 0.1 O2, etc. It can be understood that the types of ternary positive electrode materials include but are not limited to the above range.
[0060] Step S2, sintering the positive electrode material precursor to obtain the positive electrode material.
[0061] The coated ternary positive electrode material substrate (i.e., positive electrode material precursor) is placed in a sintering device (such as a roller kiln) for sintering, and a stable, uniform, and high-bonding-strength coating is formed after sintering.
[0062] In some embodiments, the sintering atmosphere can be oxygen or air, and the sintering atmosphere of oxygen or air is conducive to the formation of the metal oxide coating; the sintering temperature can be 300°C to 800°C, and can further be 400°C to 600°C, and can be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, etc., and the appropriate sintering temperature helps to form a uniform, stable and dense coating; the sintering time can be 5h to 15h, and can further be 8h to 12h, and can be 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h or 15h, etc., and the appropriate sintering time can ensure the full reaction of the coating, and further improve the uniformity, stability and density of the coating. Sintering under the above parameters is conducive to improving the comprehensive effect of coating, improving the quality of the coating, and thus improving the comprehensive performance of the positive electrode material.
[0063] Compared with the prior art, the method for preparing the positive electrode material provided in the embodiment of the present application has the following beneficial effects:
[0064] 1. Through the wet spray coating process, the effect of uniformly coating the above-mentioned coating on the surface of the ternary positive electrode material matrix can be achieved, and then the purpose of adjusting the coating rate can be achieved by accurately controlling the material injection speed, thereby realizing a gradual change in the concentration gradient of the two-component phase in the coating, and realizing a high fast ion conductor concentration in the inner layer and a high metal oxide concentration gradient in the outer layer of the coating, thereby improving the coating structure stability, improving the rate performance of the positive electrode material and the stability during long-term cycling.
[0065] 2. By controlling the temperature during and after the spraying process, the cathode material precursor can be quickly dried to dry out the moisture, which is beneficial to improving the coating effect and thus improving the performance of the cathode material.
[0066] 3. The preparation method is simple and efficient, which is conducive to the large-scale production of positive electrode materials and has excellent commercial prospects.
[0067] See also Figure 2 As shown, the embodiment of the present application also provides an electrochemical device (such as a battery), the electrochemical device 100 includes a positive electrode sheet 10, a negative electrode sheet 20, a separator 30 and an electrolyte 40, wherein the positive electrode sheet 10 includes a positive electrode active material, and the positive electrode active material is the positive electrode material as described above. The electrochemical device 100 prepared using the above-mentioned positive electrode material has the advantages of high capacity, high initial efficiency, long cycle life and excellent rate performance.
[0068] The above-mentioned positive electrode material and its preparation method and electrochemical device are further described below through specific examples.
[0069] Example 1
[0070] Step 1: 1.4 kg LLZO auxiliary material and pure water are mixed and stirred at a solid-liquid ratio of 1:10 to form slurry 1; 0.4 kg ZrO2 and pure water are mixed and stirred at a solid-liquid ratio of 1:10 to form slurry 2; the mechanical stirring kettle is kept stirring for 30 minutes until a stable suspension is formed.
[0071] Step 2: Select LiNi x Co y Mn 1-x-y The O2 ternary single crystal positive electrode material is coated on the ternary positive electrode material matrix, wherein x is 0.7 and y is 0.1, i.e., the molar percentage of Ni:Co:Mn in the ternary positive electrode material matrix is 7:1:2. It is put into a plowshare coating machine for continuous stirring, and the feeding weight is 300 kg. Heating oil is introduced into the outer sheath of the plowshare equipment, and the oil temperature is 200°C to continuously heat the material; the initial speed of the peristaltic pump for extracting slurry 1 is set to 60 rpm, and the initial speed of the peristaltic pump for extracting slurry 2 is set to 0 rpm, and spraying is performed. Thereafter, the speed of the peristaltic pump for extracting slurry 1 is reduced by 20 rpm every 10 minutes, and the speed of the peristaltic pump for extracting slurry 2 is increased by 20 rpm. The spray coating is stopped after 40 minutes; after stopping, the plowshare stirring is continuously maintained, and the sheath is continuously heated for 30 minutes to dry the moisture of the auxiliary material. After stopping the heating, the temperature is naturally cooled to room temperature to collect the material, and the positive electrode material precursor is obtained.
[0072] Step 3: Place the cathode material precursor in a roller kiln for sintering at a sintering temperature of 450° C. for 10 h to obtain the cathode material.
[0073] Comparative Example 1
[0074] Step 1: Put 1.4kg LLZO auxiliary material, 0.4kg ZrO2 and 300kg ternary cathode material matrix into a plowshare coating machine and stir continuously for 40min until the materials are evenly mixed, and then dry coat to obtain cathode material precursor. x Co y Mn 1-x-y O2 ternary single crystal positive electrode material, x is 0.7, y is 0.1, that is, the molar percentage of Ni:Co:Mn in the ternary positive electrode material matrix is 7:1:2.
[0075] Step 2: Place the cathode material precursor in a roller kiln for sintering at a sintering temperature of 450° C. for 10 h to obtain the cathode material.
[0076] Comparative Example 2
[0077] The specific process of the preparation process refers to Example 1, the difference is that in step 2, LLZO and ZrO2 auxiliary materials are coated step by step, the peristaltic pump speed is kept constant at 30 rpm, and the preparation method of the remaining positive electrode materials is basically the same as in Example 1, which will not be described in detail here.
[0078] Comparative Example 3
[0079] The specific process of the preparation process refers to Example 1, the difference is that in step 2, only ZrO2 auxiliary material coating is performed, the peristaltic pump speed is kept constant at 30 rpm, and the preparation method of the remaining positive electrode materials is basically the same as in Example 1, which will not be described in detail here.
[0080] Comparative Example 4
[0081] The specific process of the preparation process refers to Example 1, except that in step 2, only LLZO auxiliary material coating is performed, the peristaltic pump speed is kept constant at 30 rpm, and the preparation method of the remaining positive electrode materials is basically the same as in Example 1, which will not be described in detail here.
[0082] 1. The main parameters for preparing the positive electrode materials of Example 1 and Comparative Examples 1-4 are shown in Table 1.
[0083] Table 1
[0084]
[0085] 2. The following tests were performed on the positive electrode materials obtained in Example 1 and Comparative Examples 1-4.
[0086] The positive electrode material prepared in Example 1 was subjected to an X-ray diffraction test, and the results were as follows: Figure 3 As shown; the positive electrode material prepared in Comparative Example 1 was subjected to an X-ray diffraction test, and the results are as follows Figure 4 shown.
[0087] The electrical performance test conditions are as follows: the prepared positive electrode material, conductive carbon and binder polyvinylidene fluoride are mixed evenly in a mass ratio of 90:5:5 to form a button battery. The LAND battery test system is used for constant current charge and discharge test. During the test, the working voltage range of the first discharge capacity test is 2.8V~4.4V, the charge and discharge rate is +0.1C / -0.1C, and the CV cut-off current is 0.01C; the working voltage range of the 45°C cycle test is 2.8V~4.4V, the charge and discharge rate is +1C / 1C, and the CV cut-off current is 0.01C. The first coulomb efficiency at 0.1C, the first discharge capacity, and the capacity retention rate after 200 cycles at 45°C of the batteries prepared with the positive electrode materials obtained in Example 1 and Comparative Examples 1-4 are measured. The results are shown in Table 2; Figure 5It is a comparison chart of the 45°C cycle capacity retention rate curves of the corresponding batteries of Example 1 and Comparative Examples 1-4.
[0088] Table 2
[0089]
[0090] The above results show that:
[0091] The surface morphology of the positive electrode materials after coating and sintering of Example 1 and Comparative Example 1 is compared. After dry coating of Comparative Example 1, the auxiliary material particles are attached to the surface of the substrate, showing a significantly rough morphology, while the surface of the particles after spray sintering is relatively smooth, which indicates that the wet coating effect is more uniform. In addition, the battery capacity and initial efficiency prepared by the positive electrode material after spray coating in Example 1 are significantly higher than those in Comparative Example 1, and due to better coating uniformity, the capacity retention rate after 200 cycles is 3.17% higher than that of Comparative Example 1, and the long-term performance is greatly improved.
[0092] Comparative Example 2 is a method of inner layer LLZO fast ion conductor coating and outer layer inert ZrO2 coating. Since the ZrO2 outer coating blocks ion conduction, the discharge capacity and first efficiency are significantly reduced, and due to the stress concentration between the coatings caused by the difference in thermal expansion coefficients between the coatings, the long-term cycle performance of the positive electrode material is reduced.
[0093] Comparative Example 3 is coated with a single LLZO coating. Although LLZO itself has a certain effect of isolating the electrolyte, it lacks the modification of the inert oxide coating, and its long-term performance has obviously declined compared with Example 1.
[0094] Comparative Example 4 is coated with a single ZrO2 coating. The ZrO2 outer coating blocks ion conduction and lacks a fast ion conductor coating. The discharge capacity and first efficiency are significantly reduced, and the 200-cycle capacity retention rate is also reduced.
[0095] It can be seen that compared with comparative examples 1-4, the positive electrode material obtained in Example 1 has excellent performance and electrochemical test results due to wet spray coating and the formation of a dual-component gradient coating, indicating that the rate performance and stability of the positive electrode material in the examples of the present application during long-term cycling are improved.
[0096] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A positive electrode material, characterized in that: It includes a core and a coating located on the surface of the core, wherein the core is a ternary positive electrode material, the coating contains a fast ion conductor and a metal oxide, and the concentration gradient of the fast ion conductor gradually increases radially from the outside to the inside of the coating, and the concentration gradient of the metal oxide gradually decreases radially from the outside to the inside of the coating.
2. The positive electrode material according to claim 1, characterized in that The fast ion conductor includes an M element, and the M element includes at least one of Ge, La, Zr, Al, Ti, As, Nb, Ta and Ca. The M element exists in the form of at least one of an oxide, a sulfide, a phosphate and a sulfide-phosphate complex.
3. The positive electrode material according to claim 1, characterized in that The fast ion conductor includes Li 10 GeP2S 12 、Li7La3Zr2O 12 and Li 1.3 Al 0.3 Ti 1.7 At least one of (PO4)3.
4. The positive electrode material according to claim 1, characterized in that The metal oxide includes at least one of ZrO2, La2O3, Al2O3 and TiO2.
5. A method for preparing a positive electrode material, characterized in that: include: Spray coating the fast ion conductor slurry and the metal oxide slurry on the ternary positive electrode material matrix at the same time to obtain a positive electrode material precursor, wherein as the spray coating time increases, the spraying speed of the fast ion conductor slurry gradually decreases, and the spraying speed of the metal oxide slurry gradually increases; and The positive electrode material precursor is sintered to obtain the positive electrode material.
6. The method for preparing the positive electrode material according to claim 5, characterized in that: The injection speed is measured by the liquid inlet rotation speeds of the fast ion conductor slurry and the metal oxide slurry. The liquid inlet rotation speed of the fast ion conductor slurry is initially 60rpm~100rpm, and gradually decreases at a rate of change of 0.5rpm / min~2rpm / min. The liquid inlet rotation speed of the metal oxide slurry is initially 0~20rpm, and gradually increases at a rate of change of 0.5rpm / min~2rpm / min.
7. The method for preparing the positive electrode material according to claim 5, characterized in that: The temperature of the spray coating is 150° C. to 300° C., the time of the spray coating is 0.5 h to 1.5 h, and after the spray coating is completed, the temperature is kept at 150° C. to 300° C. for 10 min to 60 min.
8. The method for preparing the positive electrode material according to claim 5, characterized in that: The sintering temperature is 300° C. to 800° C., and the sintering time is 5 h to 15 h.
9. The method for preparing the positive electrode material according to claim 5, characterized in that: The method for preparing the positive electrode material satisfies at least one of the following conditions: The fast ion conductor includes an M element, wherein the M element includes at least one of Ge, La, Zr, Al, Ti, As, Nb, Ta and Ca, and the M element exists in the form of at least one of an oxide, a sulfide, a phosphate and a sulfide-phosphate complex; The fast ion conductor includes Li 10 GeP2S 12 、Li7La3Zr2O 12 and Li 1.3 Al 0.3 Ti 1.7 At least one of (PO4)3; The metal oxide includes at least one of ZrO2, La2O3, Al2O3 and TiO2.
10. An electrochemical device, characterized in that: The electrochemical device comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode active material, and the positive electrode active material is a positive electrode material as described in any one of claims 1 to 4 or a positive electrode material prepared by the preparation method of a positive electrode material as described in any one of claims 5 to 9.