Thermal transfer recording medium and printing apparatus

By introducing an intermediate layer of the thermoplastic elastomer into the thermal transfer recording medium, and finely controlling the energy and temperature of the thermal head, the problems of turbidity and reduction of the color tone in the prior art are solved, and clear multi-color recording is achieved and efficient continuous printing.

CN118973828APending Publication Date: 2024-11-15BROTHER KOGYO KK +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030980.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

When recording texts of various colors, existing thermal transfer recording media tend to have problems such as turbid tone and reduced clarity, especially when it is difficult to maintain clarity of text during low-temperature transfer.

Method used

Using an intermediate layer containing a thermoplastic elastomer, the adhesive force variation between the first and second thermal transfer layers is ensured by adjusting the energy and temperature control applied by the thermal head, thereby achieving a clear two-color recording.

Benefits of technology

It effectively avoids turbidity in color, ensures clarity and color separation of text, and maintains efficient recording performance during continuous thermal transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973828A_ABST
    Figure CN118973828A_ABST
Patent Text Reader

Abstract

The thermal transfer recording medium includes: a substrate layer having a first surface and a second surface; and a first heat transfer layer, an intermediate layer, and a second heat transfer layer which are sequentially laminated on the first surface of the base layer so as to be in direct contact with each other, the intermediate layer containing a thermoplastic elastomer. The thermal transfer recording medium is provided with an intermediate layer containing a thermoplastic elastomer, so that the thermal transfer recording medium can record characters with good clarity and at least two colors.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Application

[0002] This application corresponds to Japanese Patent Application No. 2022-075254 filed with the Japan Patent Office on April 28, 2022, and all disclosed contents of the application are incorporated herein by reference. Technical Field

[0003] The present invention relates to a thermal transfer recording medium capable of recording characters in different colors and a printing device for transferring the thermal transfer recording medium to a printed medium. Background Art

[0004] For example, Patent Documents 1 and 2 disclose thermal transfer recording media capable of recording text in different colors (e.g., black and red). Such thermal transfer recording media are installed in a dedicated printing device. By adjusting the energy applied to the thermal head of the printing device, text in different colors can be transferred to the printed medium.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2000-094843

[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 62-227788

[0009] Patent Document 3: Japanese Patent Application Laid-Open No. 63-214481 Summary of the invention

[0010] Problems to be solved by the invention

[0011] One embodiment of the present invention provides a thermal transfer recording medium capable of recording characters with good clarity and in at least two colors.

[0012] Solutions to Solve Problems

[0013] A thermal transfer recording medium according to one embodiment of the present invention comprises: a substrate layer having a first surface and a second surface; and a first thermal transfer layer, an intermediate layer and a second thermal transfer layer, which are sequentially stacked on the first surface of the substrate layer in direct contact with each other, and the intermediate layer comprises a thermoplastic elastomer.

[0014] Effects of the Invention

[0015] The thermal transfer recording medium according to one embodiment of the present invention includes an intermediate layer containing a thermoplastic elastomer, and therefore can record characters with good clarity and in at least two colors. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a diagram schematically showing the structure of a printing device according to an embodiment of the present invention.

[0017] Figure 2 is a block diagram showing the electrical structure of the printing device.

[0018] Figure 3 This is a schematic diagram for explaining a heating process and a cooling process of the printing apparatus.

[0019] Figure 4A as well as Figure 4B This is a schematic diagram for explaining a cooling process and a transfer process of the printing device.

[0020] Figure 5A as well as Figure 5B This is a diagram showing an example of a printing pattern by the printing device.

[0021] Figure 6 This is a schematic cross-sectional view showing a layer structure of an ink ribbon according to an embodiment of the present invention.

[0022] Figure 7 The figure shows the relationship between the elapsed time and the reaching temperature of the thermal transfer recording medium in the heating step and the cooling step.

[0023] Figure 8 This is a diagram showing the relationship between the elapsed time in the heating step and the cooling step and the interlayer adhesive force of the thermal transfer recording medium.

[0024] Fig. 9 This is a diagram showing the relationship between the elapsed time in the heating step and the cooling step and the interlayer adhesive force of the thermal transfer recording medium.

[0025] Fig.10 It is a diagram showing a state where the thermal transfer recording medium is peeled off.

[0026] Fig.11 It is a diagram showing a state where the thermal transfer recording medium is peeled off.

[0027] Fig.12 It is a diagram showing a state where the thermal transfer recording medium is peeled off.

[0028] Fig.13 It is a diagram showing a state where the thermal transfer recording medium is peeled off.

[0029] Fig.14 It is a diagram showing a state where the thermal transfer recording medium is peeled off.

[0030] Fig.15It is a diagram showing a state where the thermal transfer recording medium is peeled off.

[0031] Fig.16 This is a diagram for comparing the solubility parameters (SP values) of the constituent materials of the thermal transfer recording medium according to one embodiment of the present invention.

[0032] Fig.17 This is a diagram showing the relationship between the type of material constituting a part of the thermal transfer recording medium and the magnitude of the solubility parameter. DETAILED DESCRIPTION

[0033] Next, embodiments of the present invention will be described in detail with reference to the drawings.

[0034] [Overall Structure of Printing Device 1]

[0035] Figure 1 It is a diagram schematically showing the structure of a printing device 1 according to an embodiment of the present invention.

[0036] Reference Figure 1 The printing device 1 is a thermal transfer printer that transfers ink from an ink ribbon 3 to a printing tape 2 as an example of a printed medium. The printing tape 2 may include, for example, a strip-shaped film tape containing a base material for direct ink transfer, and a paper label tape formed by arranging a plurality of paper labels on a strip-shaped base film.

[0037] The characters recorded on the printing tape 2 may include typical characters, symbols such as barcodes and QR codes (registered trademarks), numbers, patterns, designs, etc. The printing device 1 of this embodiment can record characters of different colors (for example, black and red) on the printing tape 2 .

[0038] The printing device 1 mainly includes a housing 4 , a tape cassette 5 accommodated in the housing 4 , a thermal head 6 , a platen roller 7 , and a control substrate 8 .

[0039] The housing 4 may be a box-shaped member made of a plastic shell, for example. An outlet 9 for taking out the printed printing tape 2 is formed on the outer wall of the housing 4. A cutter (not shown) may be provided near the outlet 9. By cutting with the cutter, the printing tape 2 can be separated into labels of the size of each unit for use and taken out.

[0040] The tape cassette 5 may be a detachable cassette relative to the housing 4. The tape cassette 5 may be inserted in the tape feed direction D1 (in the direction of the tape feed direction D2). Figure 1The printing tape roll 10 (in other words, it may also be a label tape roll), the supply roll 11, the ink ribbon roll 12, the ink ribbon peeling member 13, and the ink ribbon winding roll 14 are sequentially accommodated from the upstream side to the downstream side (in the direction from the right side to the left side), respectively. In the present embodiment, the printing tape roll 10 and the ink ribbon roll 12 are of the type used in the state of being accommodated in the tape box 5, but may also be of the type directly mounted on the printing device 1 for use, for example.

[0041] The printing tape roll 10 is manufactured by winding the printing tape 2 into a cylindrical shape, and the printing tape roll 10 is rotatably held in the tape cassette 5, for example. A printing tape drive shaft 16 provided in the housing 4 is inserted into the supply roller 11. The rotational force R1 generated by the driving of the printing tape drive shaft 16 is transmitted to the supply roller 11, so that the supply roller 11 rotates.

[0042] The ink ribbon roller 12 is manufactured by winding the ink ribbon 3 into a cylindrical shape, and the ink ribbon roller 12 is rotatably held in the ribbon cassette 5, for example. The ink ribbon drive shaft 18 provided in the housing 4 is inserted into the ink ribbon winding roller 14. The rotational force R2 generated by the driving of the ink ribbon drive shaft 18 is transmitted to the ink ribbon winding roller 14, so that the ink ribbon winding roller 14 rotates.

[0043] The ink ribbon stripping member 13 may be a guide member that changes the feeding direction D2 of the ink ribbon 3. The ink ribbon stripping member 13 may have a shape that can abut against the ink ribbon 3 being transported, for example, it may have a roller shape or a blade shape. The ink ribbon 3 is partially thermally pressed against the printing tape 2 by the thermal head 6, and is transported toward the removal port 9 together with the printing tape 2. The ink ribbon stripping member 13 abuts against the ink ribbon 3 in the middle of being transported, and the feeding direction D2 of the ink ribbon 3 is suddenly changed relative to the feeding direction D1 of the printing tape 2. As a result, the printing tape 2 and the ink ribbon 3 are separated, and the ink ribbon 3 is stripped from the printing tape 2.

[0044] The thermal head 6 is disposed between the printing tape roller 10 and the ink ribbon roller 12 and the ink ribbon peeling member 13 in the feeding direction D1 of the printing tape 2. The thermal head 6 includes a substrate 19 and a heating element 20 (such as a heating resistor) formed on the substrate 19. The Joule heat generated by the conduction of electricity to the heating element 20 is used for thermal transfer of the ink of the ink ribbon 3.

[0045] The platen roller 7 is inserted with, for example, a platen drive shaft 21 provided in the housing 4. The rotational force R3 generated by the driving of the platen drive shaft 21 is transmitted to the platen roller 7, so that the platen roller 7 rotates. The control board 8 is an electronic device that performs electrical control of the printing device 1, and is provided inside the housing 4.

[0046] [Electrical Structure of Printing Device 1]

[0047] Figure 2 It is a block diagram showing the electrical structure of the printing device 1 .

[0048] Reference Figure 2 The control circuit 22 is provided on the control substrate 8 of the printing device 1. The control circuit 22 may include a CPU 23, a ROM 24, a memory 25, a RAM 26, and an input / output I / F 27 (interface). These are electrically connected via a data bus (not shown), for example.

[0049] The ROM 24 stores various programs for driving the printing device 1 (for example, Figure 3 as well as Figure 4A , B, etc.). The CPU 23 uses the temporary storage function of the RAM 26 and performs signal processing according to the program stored in the ROM 24, thereby controlling the printing device 1 as a whole. The memory 25 can be composed of, for example, a part of the storage area of ​​the ROM 24. The memory 25 can store in advance a table for displaying the remaining amount (consumption) of the ink ribbon 3 on the display unit (not shown) of the housing 4.

[0050] The first drive circuit 28 and the second drive circuit 29 are electrically connected to the input / output I / F 27. The first drive circuit 28 performs power supply control on the heating element 20 of the thermal head 6. The second drive circuit 29 performs drive control on the drive motor 30 that drives the supply roller 11, the ribbon winding roller 14, and the platen roller 7 to rotate so as to output drive pulses.

[0051] [Flow of Printing Process by Printing Device 1]

[0052] Figure 3 This is a schematic diagram for explaining a heating process and a cooling process of the printing apparatus 1 . Figure 4A as well as Figure 4B This is a schematic diagram for explaining a cooling process and a transfer process of the printing device 1 . Figure 4B is from Figure 4A An enlarged view of the main part when observing the transfer pattern in the direction of arrow 4B. Figure 5A as well as Figure 5B 1 is a diagram showing an example of a printed pattern 44 by the printing device 1. Figure 1 as well as Figure 3~Figure 5A as well as Figure 5B , the printing process performed by the printing device 1 is described in detail.

[0053] In order to print characters on the printing tape 2, the printing tape 2 is fed out from the printing tape roller 10 by the rotational drive of the supply roller 11, and the ink ribbon 3 is fed out from the ink ribbon roller 12 by the rotational drive of the ink ribbon winding roller 14. Figure 1 as well as Figure 3As shown, the printing ribbon 2 and the ink ribbon 3 are conveyed toward the downstream side in a state of overlapping each other. In the printing ribbon 2, the surface on the ink ribbon 3 side is a printing surface 31 (front surface), and the surface on the opposite side is a back surface 32. In the ink ribbon 3, the surface on the printing ribbon 2 side is an adhesive surface 33 (front surface), and the surface on the opposite side is a back surface 34.

[0054] Reference Figure 3 The ink ribbon 3 includes a base layer 35, a first ink layer 36 as an example of a first thermal transfer layer, and a second ink layer 37 as an example of a second thermal transfer layer. The first ink layer 36 and the second ink layer 37 are stacked in this order on a surface 38 as an example of a first surface of the base layer 35. The surface opposite to the surface 38 of the base layer 35 is a back surface 39 (back surface 34 of the ink ribbon 3). The first ink layer 36 and the second ink layer 37 contain colorants of different colors. For example, the first ink layer 36 may contain a black colorant as an example of a first ink, and the second ink layer 37 may contain a red colorant as an example of a second ink.

[0055] The ink ribbon 3 is conveyed toward the thermal head 6 in a state where the second ink layer 37 is in contact with the printing ribbon 2. In the thermal head 6, as shown in FIG. Figure 3 Specifically, the heating element 20, which generates heat due to power supply, is pressed against the ink ribbon 3, so that the heat is transferred to the first ink layer 36 and the second ink layer 37 via the base material layer 35. The stack of the ink ribbon 3 and the printing ribbon 2 is sandwiched between the thermal head 6 and the platen roller 7, and is transported to the downstream side while being heated by the thermal head 6.

[0056] The heating element 20 can be controlled to have the same temperature as a whole, or to have different temperatures in some parts. Figure 3 As shown, the first portion 40 of the heating element 20 may be controlled to a relatively low first heating temperature, and the second portion 41 of the heating element 20 may be controlled to a second heating temperature higher than the first heating temperature. Thus, the ink ribbon 3 may include a first portion 42 heated at the first heating temperature and a second portion 43 heated at the second heating temperature. In the first portion 42 and the second portion 43 of the ink ribbon 3, at least a portion or all of the first ink layer 36 and the second ink layer 37 are melted or softened, so as to be in close contact with the printing ribbon 2.

[0057] Reference Figure 3 as well as Figure 4A , B, a cooling process is performed in the area between the thermal head 6 and the ink ribbon stripping member 13. Specifically, the ink ribbon 3 that is thermally pressed to the printing ribbon 2 in the heating process is naturally cooled in the area from the thermal head 6 to the ink ribbon stripping member 13, and the temperature is reduced toward the use environment temperature of the printing device 1.

[0058] Then, if Figure 4A As shown in FIG. 2 and FIG. 3 , the feeding direction D2 of the ink ribbon 3 is selectively changed by the ink ribbon peeling member 13, so that an external force F1 is applied to the base layer 35 and the second ink layer 37 in a direction away from each other. As a result, the printing ribbon 2 and the ink ribbon 3 are separated, and the ink ribbon 3 is wound around the ink ribbon winding roller 14. At this time, the first portion 42 and the second portion 43 of the ink ribbon 3 that have been heated by the thermal head 6 selectively remain on the printing ribbon 2, thereby performing the transfer process. For example, in the first portion 42, peeling may occur between the base layer 35 and the laminated body including the first ink layer 36 and the second ink layer 37, thereby transferring the laminated body. On the other hand, in the second portion 43, peeling may occur between the first ink layer 36 and the second ink layer 37, thereby selectively transferring the second ink layer 37.

[0059] Thus, a printed pattern 44 of different colors (for example, black and red) is formed on the printing tape 2. Figure 5A As shown, the printed pattern 44 can have different colors for individual characters. Figure 5A In the example shown in FIG. 1 , when viewed from the printing surface 31 of the printing tape 2, a red pattern 45 based on the second ink layer 37 can be visually recognized on the outermost surfaces of letters “A” and “C”, and a black pattern 46 based on the first ink layer 36 can be visually recognized on the outermost surface of letter “B”. Figure 5B As shown, the printed pattern 44 can be visually recognized as both a red pattern 45 and a black pattern 46 for each character portion.

[0060] After the transfer of the ink ribbon 3 , the printing tape 2 on which the characters are recorded is taken out from the take-out port 9 of the printing device 1 .

[0061] [An example of a problem in two-color printing]

[0062] In a thermal transfer thermal printer (printing device 1), after the ink ribbon 3 is heated by the thermal head 6 according to the pattern of recording information, the ink ribbon 3 is peeled off from the printing tape 2. As a result, the ink layers 36 and 37 are selectively melted or softened according to the heating pattern and peeled off from the base material layer 35 and transferred to the printing surface 31 of the printing tape 2, so that the text is recorded on the printing surface 31. The above-mentioned two-color thermal transfer printing is also disclosed in the aforementioned patent documents 1 and 2, but there are the following problems.

[0063] For example, Patent Document 1 discloses a thermal transfer sheet for recording in two colors, comprising a substrate and a plurality of thermal transfer ink layers (e.g., a first thermal transfer ink layer and a second thermal transfer ink layer) with different tones stacked on the substrate. The two thermal transfer ink layers are respectively formed of thermoplastic resin, wax, or the like.

[0064] In Patent Document 1, for example, when a relatively low energy is applied to the thermal head and thermal transfer is performed at a low temperature, the first thermal transfer ink layer softens and the adhesion to the substrate is reduced, and the second thermal transfer ink layer softens and generates adhesion to the surface of the transferred body. However, the result of the two thermal transfer ink layers softening together and thus maintaining adhesion is that the entire thermal transfer ink layer, that is, the first thermal transfer ink layer and the second thermal transfer ink layer are thermally transferred to the surface of the transferred body as a whole. Therefore, the text recorded on the surface of the transferred body, for example, becomes the color tone of the first thermal transfer ink layer located on the outermost layer after transfer, such as black.

[0065] On the other hand, when a relatively high energy is applied to the thermal head and thermal transfer is performed at a higher temperature, the first thermal transfer ink layer further softens and the adhesion force relative to the substrate increases, and the second thermal transfer ink layer softens and generates adhesion force relative to the surface of the transfer body. During this thermal transfer, the so-called reverse transfer occurs in which the first thermal transfer ink layer remains on the substrate side. Therefore, only the second thermal transfer ink layer is selectively thermally transferred to the surface of the transfer body. As a result, the text recorded on the surface of the transfer body becomes the color tone of the second thermal transfer ink layer, for example, red.

[0066] However, sometimes between the range of transfer temperature (≈ the energy applied to the thermal head, the same below) when the two thermal transfer ink layers are thermally transferred as a whole (hereinafter sometimes referred to as the "low-temperature transfer range") and the range of transfer temperature when only the second thermal transfer ink layer is thermally transferred (hereinafter sometimes referred to as the "high-temperature transfer range"), there is a range of transfer temperature in which a portion of the first thermal transfer ink layer is transferred together with the second thermal transfer ink layer and the color tone of the text becomes turbid (hereinafter sometimes referred to as the "turbid transfer range").

[0067] Furthermore, in a thermal transfer sheet formed by directly stacking two thermal transfer ink layers, there is a tendency that the turbid transfer range is large and the low temperature transfer range and high temperature transfer range are narrow. In addition, there is a tendency that heat accumulates in the thermal head due to continuous thermal transfer printing, so that the temperature of the thermal head gradually rises. Therefore, it is particularly difficult to maintain the temperature of the thermal head in the low temperature transfer range, so that the color tone of the text is easily turbid during low temperature transfer.

[0068] The thermal transfer sheet of patent document 1 may further include a peeling layer formed between the first thermal transfer ink layer and the second thermal transfer ink layer. The peeling layer is composed of a colorless, transparent wax with low melting viscosity and high fluidity. The peeling layer melts or softens during thermal transfer, promoting the separation of the two thermal transfer ink layers. The high-temperature transfer range can be further expanded to the low-temperature side, thereby narrowing the turbid transfer range. However, there is a tendency that the low-temperature transfer range that can suppress the peeling of the peeling layer and transfer the two thermal transfer ink layers in one piece becomes narrower. In addition, wax is easy to affect the surroundings due to its low melting viscosity. Especially when recording fine images such as bar codes, there is a situation where excess peeling occurs and the clarity of the recording is reduced.

[0069] Patent document 2 discloses an ink ribbon including a substrate and a first ink layer and a second ink layer directly stacked on the substrate. In Patent document 2, the ink ribbon is first heated in a low temperature transfer range, and the two ink layers are thermally transferred integrally to the surface of the substrate. Then, the case where only the second ink layer remains and the ink ribbon is reheated when peeling off is studied, so that the first ink layer is reversely transferred to the substrate side. However, the thermal transfer printing of Patent document 2 requires a printer with a special thermal head that can be reheated after thermal transfer, and has a problem of low versatility.

[0070] The inventors of the present application have found multiple problems in view of the thermal transfer methods of Patent Documents 1 and 2. At least one of the multiple problems (first problem) is to provide a thermal transfer recording medium (ink ribbon) capable of simultaneously recording text with good clarity and in at least two colors.

[0071] Another of the above-mentioned problems (second problem) is to provide a thermal transfer recording medium (ink ribbon) that can clearly separate two colors without turbidity even when thermal transfer recording is continuously performed using a general-purpose thermal transfer printer that supports recording of two colors.

[0072] Another one of the multiple topics (the third topic) is to provide a thermal transfer recording medium (ink ribbon) that can record text with excellent clarity without causing turbidity in the color tone and clearly separating into two colors even when thermal transfer recording is continuously performed using a general thermal transfer printer corresponding to recording of two colors, and without causing unnecessary peeling.

[0073] [Introduction of the intermediate layer 51 comprising a thermoplastic elastomer]

[0074] In order to solve the above-mentioned problems, the inventors of the present application have studied and implemented the case of introducing an intermediate layer containing a thermoplastic elastomer into a thermal transfer recording medium (ink ribbon), which will be described in detail below.

[0075] Figure 62 is a schematic cross-sectional view showing a layer structure of a thermal transfer recording medium 47 according to an embodiment of the present invention. Figure 6 , a thermal transfer recording medium 47 is shown in a state of being adhered to a printing tape 2 as an example of a medium to be printed.

[0076] The thermal transfer recording medium 47 can be used as the ink ribbon 3 in Figure 1~Figure 4A , B. The thermal transfer recording medium 47 includes a substrate layer 48, a back layer 49, a first thermal transfer layer 50, an intermediate layer 51, and a second thermal transfer layer 52. The first thermal transfer layer 50, the intermediate layer 51, and the second thermal transfer layer 52 are stacked in this order on a surface 53 of the substrate layer 48 as an example of a first surface. The surface on the opposite side of the surface 53 of the substrate layer 48 may be a back surface 54. The back layer 49 is stacked on the back surface 54 of the substrate layer 48. The first thermal transfer layer 50 and the second thermal transfer layer 52 may be referred to as a first ink layer and a second ink layer, respectively.

[0077] The thermal transfer recording medium 47 of the present invention is characterized by comprising a substrate layer 48, and a first thermal transfer layer 50, an intermediate layer 51, and a second thermal transfer layer 52 sequentially laminated in direct contact with each other on a surface 53 of the substrate layer 48. The intermediate layer 51 contains a thermoplastic elastomer as a binder.

[0078] In the thermal transfer recording medium 47, for example, there is a thermal head 6 (refer to Figure 1 as well as Figure 3 ) The energy applied is set to be low and the thermal transfer is performed at a low temperature. In this case, the first thermal transfer layer 50 softens and the adhesion to the base layer 48 is reduced. On the other hand, the second thermal transfer layer 52 softens and generates adhesion to the printing surface 31 of the printing tape 2. In addition, the affinity between the two thermal transfer layers 50, 52 and the intermediate layer 51 is improved, and the adhesion of the two thermal transfer layers 50, 52 to the intermediate layer 51 is respectively improved. In addition, compared with wax or the like that forms a peeling layer as in Patent Document 1, the intermediate layer 51 containing a thermoplastic elastomer has a relatively high melt viscosity. The intermediate layer 51 maintains adhesion to the first thermal transfer layer 50 and the second thermal transfer layer 52 by means of its rubber-like elastic force. As a result, the entire thermal transfer layer, that is, the first thermal transfer layer 50, the intermediate layer 51 and the second thermal transfer layer 52 are thermally transferred to the printing surface 31 of the printing tape 2 as a whole. The characters recorded on the printing surface 31 of the printing tape 2 are in the color tone of the first thermal transfer layer 50 located on the outermost surface after the transfer, for example, black.

[0079] On the other hand, for the thermal transfer recording medium 47, there is a case where the energy applied to the thermal head 6 is set higher, so that thermal transfer is performed at a higher temperature. In this case, the first thermal transfer layer 50 is further softened and the adhesion force relative to the base layer 48 increases, and the second thermal transfer layer 52 generates adhesion force relative to the printing surface 31 of the printing tape 2. In addition, the adhesion force of the first thermal transfer layer 50 relative to the intermediate layer 51 increases, which is higher than the adhesion force between the second thermal transfer layer 52 and the intermediate layer 51. During thermal transfer, reverse transfer occurs in which the first thermal transfer layer 50 and the intermediate layer 51 remain on the side of the base layer 48, and only the second thermal transfer layer 52 is thermally transferred to the printing surface 31 of the printing tape 2. Therefore, the text recorded on the printing surface 31 of the printing tape 2 becomes the color tone of the second thermal transfer layer 52, for example, red. As a result, it is possible to record patterns of two colors, such as black and red, using a general thermal transfer printer corresponding to recording of two colors.

[0080] In addition, as described above, the thermoplastic elastomer included in the intermediate layer 51 has a higher melt viscosity than wax or the like, so that the low-temperature transfer range in which the two thermal transfer layers 50 and 52 can be transferred integrally can be expanded to the high-temperature side, thereby narrowing the turbid transfer range. In addition, the temperature dependence of the rubber-like elastic force, adhesion force and other characteristics of the intermediate layer 51 including the thermoplastic elastomer with high melt viscosity is low compared to the two thermal transfer layers 50 and 52 and the peeling layer. Therefore, even if the temperature of the thermal head 6 gradually rises while the thermal transfer recording is continuously performed, the turbidity of the color tone of the text can be suppressed.

[0081] Therefore, according to the present invention, even if thermal transfer recording is continuously performed using a general-purpose thermal transfer printer that supports recording in two colors, the color tone is not easily muddy and is clearly separated into two colors, and no unnecessary peeling occurs, so that text with excellent clarity can be recorded.

[0082] Hereinafter, specific compositions, physical properties, etc. of the base material layer 48 , the back layer 49 , the first thermal transfer layer 50 , the intermediate layer 51 , and the second thermal transfer layer 52 included in the thermal transfer recording medium 47 will be described in detail.

[0083] (1) Base material layer 48

[0084] As the substrate layer 48, for example, films of resins such as polysulfone, polystyrene, polyamide, polyimide, polycarbonate, polypropylene, polyester, triacetate, thin papers such as capacitor paper and glassine, and cellophane can be listed. Among them, films of polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate are preferred from the viewpoints of mechanical strength, dimensional stability, heat treatment resistance, price, etc. The thickness of the substrate layer 48 can be arbitrarily set according to the specifications of the thermal transfer printer, for example. For example, the thickness of the substrate layer 48 is 1 μm or more, preferably 2 μm or more. For example, the thickness of the substrate layer 48 is 10 μm or less, preferably 8 μm or less. For example, the thickness of the substrate layer 48 is 1 μm or more and 10 μm or less, preferably 2 μm or more and 8 μm or less.

[0085] (2) Back layer 49

[0086] The back layer 49 improves the heat resistance, sliding property, and abrasion resistance of the back surface 54 of the base material layer 48 in contact with the thermal head 6. Examples of the back layer 49 include silicone resin, fluororesin, silicone-fluoro copolymer resin, nitrocellulose resin, silicone-modified urethane resin, and silicone-modified acrylic resin. The back layer 49 may contain a lubricant as needed.

[0087] The back layer 49 can be formed, for example, by applying a coating obtained by dissolving or dispersing the above-mentioned resin or the like in an arbitrary solvent to the back surface 54 of the base layer 48 and then drying the coating. The thickness of the back layer 49 can be arbitrarily set according to the specifications of the thermal transfer printer, etc. The thickness of the back layer 49 can be adjusted by the coating amount of the back layer 49.

[0088] For example, the coating amount of the back surface layer 49 is 0.05 g / m 2 Above, preferably 0.1 g / m 2 For example, the coating amount of the back layer 49 is 0.5 g / m 2 Below, preferably 0.4g / m 2 For example, the coating amount of the back surface layer 49 is 0.05 g / m 2 Above and 0.5g / m 2 Below, preferably 0.1g / m 2 Above and 0.4g / m 2 The specific thickness of the back layer 49 is, for example, 0.05 μm or more, preferably 0.1 μm or more. The thickness of the back layer 49 is, for example, 0.5 μm or less, preferably 0.4 μm or less. The thickness of the back layer 49 can be, for example, 0.05 μm or more and 0.5 μm or less, preferably 0.1 μm or more and 0.4 μm or less.

[0089] (3) First thermal transfer layer 50

[0090] The first thermal transfer layer 50 can be formed, for example, by any thermoplastic resin. In order to improve the affinity and adhesion to the base layer 48 and the intermediate layer 51, the first thermal transfer layer 50 is preferably formed by using epoxy resin as the thermoplastic resin. Epoxy resin has excellent affinity and adhesion to the base layer 48 composed of a polyester film such as PET and the thermoplastic elastomer forming the intermediate layer 51. The first thermal transfer layer 50 can be formed by using epoxy resin as the thermoplastic resin in a state where the curing agent is not added (removed).

[0091] Examples of epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, alicyclic epoxy resins, hydrogenated bisphenol A epoxy resins, hydrogenated bisphenol AD ​​epoxy resins, propylene glycol glycoxyether, pentaerythritol polyglycidyl ether and other aliphatic epoxy resins, epoxy resins obtained from aliphatic or aromatic amines and epichlorohydrin, epoxy resins obtained from aliphatic or aromatic carboxylic acids and epichlorohydrin, heterocyclic epoxy resins, spiro-ring-containing epoxy resins, epoxy-modified resins, brominated epoxy resins, etc. Specific examples of epoxy resins are not particularly limited, and examples thereof include the following various epoxy resins. These epoxy resins can be used alone or in combination of two or more.

[0092] Among the substantially solid epoxy resins of the JER (registered trademark) series manufactured by Mitsubishi Chemical Corporation, 1001 [softening point (ring and ball method): 64°C, number average molecular weight Mn: about 900], 1002 [softening point (ring and ball method): 78°C, number average molecular weight Mn: about 1200], 1003 [softening point (ring and ball method): 89°C, number average molecular weight Mn: about 1300], 1055 [softening point (ring and ball method): 93°C, number average molecular weight Mn: about 1600], 1004 [softening point (ring and ball method): 97°C, number average molecular weight Mn: about 1650], 1004AF [softening point (ring and ball method): 97°C, number average molecular weight Mn: about 2900〕、1009〔softening point (ring and ball method): 144℃、number average molecular weight Mn: about 3800〕、1010〔number average molecular weight Mn: about 5500〕、1003F〔softening point (ring and ball method): 96℃〕、1004F〔softening point (ring and ball method): 103℃〕、1005F、1009F〔softening point (ring and ball method): 144℃〕、1004FS〔softening point (ring and ball method): 100℃〕、1006FS〔softening point (ring and ball method): 112℃〕、1007FS〔softening point (ring and ball method): 124℃〕。

[0093] The softening point of the epoxy resin used in the first thermal transfer layer 50 is, for example, 95° C. or higher, preferably 110° C. or higher, and more preferably 125° C. or higher. If the softening point is within this range, it is possible to suppress the occurrence of a high adhesive force between the first thermal transfer layer 50 and the base material layer 48 at a relatively low temperature during low-temperature transfer. Since the low-temperature transfer range of the first thermal transfer layer 50 can be sufficiently extended to the high-temperature side, even if thermal transfer recording is performed continuously, it is possible to suppress the occurrence of color turbidity.

[0094] The first thermal transfer layer 50 may contain an adhesive in addition to the epoxy resin. By containing an adhesive, the affinity and adhesion to the base layer 48 and the intermediate layer 51 can be further improved. Examples of the adhesive include rubber adhesives, acrylic adhesives, silicone adhesives, vinyl alkyl ether adhesives, polyvinyl alcohol adhesives, polyvinyl pyrrolidone adhesives, polyacrylamide adhesives, and cellulose adhesives.

[0095] In consideration of improving affinity and compatibility with epoxy resin and affinity and adhesion to substrate layer 48 and intermediate layer 51, acrylic adhesive is preferred as the adhesive. Specific examples of acrylic adhesive are not particularly limited, and the following acrylic adhesives can be cited, for example. These acrylic adhesives can be used alone or in combination of two or more.

[0096] BPS1109 (non-volatile content: 39.5% by mass), BPS3156D (non-volatile content: 34% by mass), BPS4429-4 (non-volatile content: 45% by mass), BPS4849-40 (non-volatile content: 40% by mass), BPS5160 (non-volatile content: 33% by mass), BPS5213K (non-volatile content: 35% by mass), BPS5160 (non-volatile content: 33% by mass), BPS5213K (non-volatile content: 35% by mass), BPS5156D (non-volatile content: 34 ...56D (non-volatile content: 34% by mass), BPS5156D (non-volatile content: 34% by mass), BPS5156D (non-volatile content: 34% by mass), %), BPS5215K (non-volatile content: 39 mass %), BPS5227-1 (non-volatile content: 41.5 mass %), BPS5296 (non-volatile content: 37 mass %), BPS5330 (non-volatile content: 40 mass %), BPS5375 (non-volatile content: 45 mass %), BPS5448 (non-volatile content: 40 mass %), BPS5513 (non-volatile content: 44.5 mass %), BPS5565 K (non-volatile content: 45 mass%), BPS5669K (non-volatile content: 46 mass%), BPS5762K (non-volatile content: 45.5 mass%), BPS5896 (non-volatile content: 37 mass%), BPS5978 (non-volatile content: 35 mass%), BPS6074HTF (non-volatile content: 52 mass%), BPS6080TFK (non-volatile content: 45 mass%), BPS6130 ... Component: 45.5 mass %), BPS6153K (non-volatile component: 25 mass %), BPS6163 (non-volatile component: 37 mass %), BPS6231 (non-volatile component: 56 mass %), BPS6421 (non-volatile component: 47 mass %), BPS6430 (non-volatile component: 33 mass %), BPS6574 (non-volatile component: 57 mass %), BPS8170 (non-volatile component: 36.5 mass %), BPS HS-1 (non-volatile component: 40 mass %).

[0097] Among the solvent-based adhesives (re-peelable type) manufactured by Lion Chemical Co., Ltd., AS-325 (solid content concentration: 45 mass %), AS-375 (solid content concentration: 45 mass %), AS-409 (solid content concentration: 45 mass %), AS-417 (solid content concentration: 45 mass %), AS-425 (solid content concentration: 45 mass %), AS-455 (solid content concentration: 45 mass %), AS-665 (solid content concentration: 40 mass %), AS-1107 (solid content concentration: 43 mass %), and AS-4005 (solid content concentration: 45 mass %).

[0098] The acrylic adhesive used in the first thermal transfer layer 50 may be used in combination with a tackifier. This is because, for example, the breakability of the first thermal transfer layer 50 can be improved, unnecessary peeling can be suppressed, and the clarity of the recorded text can be improved. Examples of the tackifier include ester gum, terpene phenol resin, rosin ester, etc. Specific examples of the tackifier are not particularly limited, and for example, the following various tackifiers can be listed. These tackifiers can be used alone or in combination of two or more.

[0099] Terpene-phenol resins of the YS Polyster series manufactured by Yasuhara Chemical Co., Ltd. include U130 (softening point: 130±5°C), U115 (softening point: 115±5°C), T160 (softening point: 160±5°C), T145 (softening point: 145±5°C), T130 (softening point: 130±5°C), T115 (softening point: 115±5°C), T100 (softening point: 100±5°C), T80 (softening point: 80±5°C), S145 (softening point: 145±5°C), G150 (softening point: 150±5°C), G125 (softening point: 125±5°C), N125 (softening point: 125±5°C), K125 (softening point: 125±5°C), and TH130 (softening point: 130±5°C).

[0100] Among Ester Gum manufactured by Arakawa Chemical Industries, Ltd., AA-G [softening point (ring and ball method): 82 to 88°C], AA-L [softening point (ring and ball method): 82 to 88°C], AA-V [softening point (ring and ball method): 82 to 95°C], 105 [softening point (ring and ball method): 100 to 110°C], AT [viscosity: 20,000 to 40,000 mPa·s], H [softening point (ring and ball method): 68 to 75°C], HP [softening point (ring and ball method): 80°C or more].

[0101] Among the Pensel (registered trademark) series of rosin esters manufactured by Arakawa Chemical Industries, Ltd., GA-100 [softening point (ring and ball method): 100 to 110°C], AZ [softening point (ring and ball method): 950 to 105°C], C [softening point (ring and ball method): 117 to 127°C], D-125 [softening point (ring and ball method): 120 to 130°C], D-135 [softening point (ring and ball method): 130 to 140°C], D-160 [softening point (ring and ball method): 150 to 165°C], and KK [softening point (ring and ball method): 165°C or more].

[0102] The softening point of the tackifier used in the first thermal transfer layer 50 is, for example, 60° C. or higher, preferably 120° C. or lower. If the softening point is within this range, the first thermal transfer layer 50 and the intermediate layer 51 can be well reversely transferred to the substrate layer 48 during high-temperature transfer. Since the high-temperature transfer range of the first thermal transfer layer 50 can be sufficiently extended to the low-temperature side, turbidity of the color tone can be suppressed.

[0103] The first thermal transfer layer 50 may contain any colorant. As the colorant, one or more various colorants corresponding to the color tone of the first thermal transfer layer 50 may be used. As the colorant, for example, a pigment may be used. Considering the improvement of the weather resistance of the text, etc., a pigment is preferably used as the colorant used in the first thermal transfer layer 50. For example, carbon black is preferably used as a pigment for coloring the first thermal transfer layer 50 in black. There is no particular limitation on specific examples of carbon black, and for example, the following various carbon blacks can be listed. These carbon blacks can be used alone or in combination of two or more.

[0104] MA77 powder made by Mitsubishi Chemical Corporation〔LFF, DBP absorption: 68cm 3 / 100g〕、MA7 powder〔LFF、DBP absorption: 66cm 3 / 100g〕、MA7 granular〔LFF、DBP absorption: 65cm 3 / 100g〕、MA8 powder〔LFF、DBP absorption: 57cm 3 / 100g〕、MA8 granular〔LFF、DBP absorption: 51cm 3 / 100g〕、MA11 powder〔LFF、DBP absorption: 64cm 3 / 100g〕、MA100 powder〔LFF、DBP absorption: 100cm 3 / 100g〕、MA100 granular〔LFF、DBP absorption: 95cm 3 / 100g〕、MA100R powder〔LFF、DBP absorption: 100cm 3 / 100g〕、MA100R granular〔LFF、DBP absorption: 95cm 3 / 100g〕、MA100S powder〔LFF、DBP absorption: 100cm 3 / 100g〕、MA230 powder〔LFF、DBP absorption: 113cm 3 / 100g〕、MA220 powder〔LFF、DBP absorption: 93cm 3 / 100g〕、MA14 powder〔LFF、DBP absorption: 73cm 3 / 100g〕.

[0105] Mitsubishi Chemical Corporation #3030B (furnace method, DBP absorption: 130 cm 3 / 100g)、#3040B(Furnace method, DBP absorption: 114cm 3 / 100g)、#3050B(Furnace method, DBP absorption: 175cm 3 / 100g), #3230B (furnace method, DBP absorption: 140cm 3 / 100g)、#3350B(Furnace method, DBP absorption: 164cm 3 / 100g), #3400B (furnace method, DBP absorption: 175cm 3 / 100g).

[0106] Tokablack (registered trademark) series manufactured by Tokai Carbon Co., Ltd., #5500 (furnace method, DBP absorption: 155 cm 3 / 100g)、#4500(Furnace method, DBP absorption: 168cm 3 / 100g)、#4400(Furnace method, DBP absorption: 135cm 3 / 100g)、#4300(Furnace method, DBP absorption: 142cm 3 / 100g).

[0107] ORION ENGINEERED CARBONS PRINTEX (Japanese: プリンテックス; registered trademark) series L (furnace method, DBP absorption: 120cm 3 / 100g), L6 (furnace method, DBP absorption: 126cm 3 / 100g).

[0108] Birla Carbon's CONDUCTEX (Japanese: コンダクテックス; registered trademark) series, 975 (furnace method, 170cm 3 / 100g), SC (furnace method, 115cm 3 / 100g).

[0109] CABOT's VULCAN series, XC72 (furnace method, DBP absorption: 174 cm 3 / 100g), 9A32 (furnace method, DBP absorption: 114cm 3 / 100g), 3700 (furnace method, DBP absorption: 111cm 3 / 100g).

[0110] DenkaBlack (registered trademark) series manufactured by Denka Co., Ltd., DenkaBlack granular product (acetylene method, DBP absorption: 160cm 3 / 100g), FX-35 (acetylene method, DBP absorption: 220cm 3 / 100g), HS-100 (acetylene method, DBP absorption: 140cm 3 / 100g).

[0111] EC300J (vaporization method, DBP absorption: 360cm) from the Ketjenblack (registered trademark) series produced by Lion Chemical Co., Ltd. 3 / 100g), EC600DJ (vaporization method, DBP absorption: 495cm 3 / 100g).

[0112] The ratio of each component in the first thermal transfer layer 50 is not particularly limited. The ratio of the acrylic adhesive to 100 parts by mass of the epoxy resin is, for example, 30 parts by mass or more, preferably 40 parts by mass or more. The ratio of the acrylic adhesive to 100 parts by mass of the epoxy resin is, for example, 150 parts by mass or less, preferably 100 parts by mass or less. The ratio of the acrylic adhesive to 100 parts by mass of the epoxy resin is, for example, 30 parts by mass or more and 150 parts by mass or less, preferably 40 parts by mass or more and 100 parts by mass or less.

[0113] The ratio of the tackifier to 100 parts by mass of the epoxy resin is, for example, 3 parts by mass or more, preferably 5 parts by mass or more. The ratio of the tackifier to 100 parts by mass of the epoxy resin is, for example, 150 parts by mass or less, preferably 100 parts by mass or less. The ratio of the tackifier to 100 parts by mass of the epoxy resin is, for example, 3 parts by mass or more and 150 parts by mass or less, preferably 5 parts by mass or more and 100 parts by mass or less.

[0114] The ratio of the colorant such as carbon black to 100 parts by mass of the epoxy resin is, for example, 100 parts by mass or more, preferably 130 parts by mass or more. The ratio of the colorant to 100 parts by mass of the epoxy resin is, for example, 230 parts by mass or less, preferably 200 parts by mass or less. The ratio of the colorant to 100 parts by mass of the epoxy resin is, for example, 100 parts by mass or more and 230 parts by mass or less, preferably 130 parts by mass or more and 200 parts by mass or less.

[0115] It should be noted that, among the components contained in the first thermal transfer layer 50 , the components provided in a liquid state dissolved or dispersed in an arbitrary solvent may be adjusted in amount so that the ratio of the effective component therein is within the above range (the same applies hereinafter).

[0116] The first thermal transfer layer 50 can be formed, for example, by applying a coating prepared by dissolving or dispersing the above-mentioned components in an arbitrary solvent directly or via an arbitrary release layer on the surface 53 of the substrate layer 48 and then drying the coating. Figure 5A as well as Figure 5B As shown, the text recorded on the printing tape 2 is color-separated. In order to perform the color separation, if the adjustment of the adhesion between the first thermal transfer layer 50 and the base layer 48 and other layers is taken into consideration, the first thermal transfer layer 50 is preferably formed directly on the surface 53 of the base layer 48 without the release layer.

[0117] The thickness of the first thermal transfer layer 50 can be arbitrarily set according to, for example, the specifications of the thermal transfer printer, etc. The thickness of the first thermal transfer layer 50 can be adjusted by the amount of the first thermal transfer layer 50 applied.

[0118] For example, the coating amount of the first thermal transfer layer 50 is 0.1 g / m 2 Above, preferably 0.5g / m 2 For example, the coating amount of the first thermal transfer layer 50 is 3.0 g / m 2 Below, preferably 2.5g / m 2 For example, the coating amount of the first thermal transfer layer 50 is expressed as 0.1 g / m 2 Above and 3.0g / m 2 Below, preferably 0.5g / m 2 Above and 2.5g / m 2 the following.

[0119] The specific thickness (before printing) of the first thermal transfer layer 50 is, for example, 0.05 μm or more, preferably 0.5 μm or more. The thickness of the first thermal transfer layer 50 is, for example, 3.0 μm or less, preferably 2.5 μm or less. The thickness of the first thermal transfer layer 50 can be, for example, 0.05 μm or more and 3.0 μm or less, preferably 0.5 μm or more and 2.5 μm or less. The thickness of the first thermal transfer layer 50 can be confirmed based on, for example, a SEM (Scanning Electron Microscope) image, a TEM (Transmission Electron Microscope) image, or the like of the thermal transfer recording medium 47.

[0120] (4) Middle layer 51

[0121] The intermediate layer 51 contains a thermoplastic elastomer as described above. In particular, the intermediate layer 51 is preferably formed only of a thermoplastic elastomer. The thermoplastic elastomer forming the intermediate layer 51 preferably contains at least one of a styrene-based thermoplastic elastomer and an acetate-based thermoplastic elastomer.

[0122] Examples of styrene-based thermoplastic elastomers include styrene-butadiene-styrene block copolymers (SBS), styrene-ethylene·butylene-styrene block copolymers (SEBS), styrene-ethylene·propylene-styrene block copolymers (SEPS), styrene-ethylene / ethylene·propylene-styrene block copolymers (SEEPS), and styrene-isoprene-styrene block copolymers (SIS). Examples of acetate-based thermoplastic elastomers include ethylene-vinyl acetate copolymers (EVA).

[0123] The content of styrene in the thermoplastic elastomer included in the intermediate layer 51 is, for example, 10% by mass or more and 70% by mass or less, preferably 15% by mass or more and 50% by mass or less. If the styrene content is too high, the rubber elasticity of the intermediate layer 51 is reduced, and there is a case where the adhesion to the first thermal transfer layer 50 and the second thermal transfer layer 52 cannot be maintained during low-temperature transfer, or the color of the text becomes turbid. If the styrene content is too low, the rubber elasticity of the intermediate layer 51 becomes too large, and there is a case where the second thermal transfer layer 52 cannot be peeled off during high-temperature transfer, and the color of the text becomes turbid.

[0124] The melt flow rate (hereinafter, sometimes abbreviated as "MFR") of the thermoplastic elastomer contained in the intermediate layer 51 is, for example, 1000 g / 10 min or less, preferably 400 g / 10 min or less. The MFR may be, for example, the MFR at a temperature of 190° C. and a load of 2.16 kg obtained by the measurement method specified in ISO 1133-1:2011. Hereinafter, the measurement conditions of the MFR are 190° C. and a load of 2.16 kg unless otherwise specified.

[0125] Thermoplastic elastomers with an MFR exceeding 400 g / 10 min tend to have an excessively strong affinity with the second thermal transfer layer 52. Therefore, there is a case where the second thermal transfer layer 52 cannot be peeled off during high-temperature transfer, and the color of the text becomes turbid. In addition, there is a case where the entire thermal transfer recording medium 47, that is, the base material layer 48, the first thermal transfer layer 50, the intermediate layer 51, and the second thermal transfer layer 52 are attached to the printing surface 31 of the printing tape 2. Thermoplastic elastomers with an MFR exceeding 400 g / 10 min have a low melt viscosity and high fluidity, so there is a case where the adhesion to the first thermal transfer layer 50 and the second thermal transfer layer 52 cannot be maintained during low-temperature transfer, or the color of the text becomes turbid.

[0126] On the other hand, if a thermoplastic elastomer having an MFR of 400 g / 10 min or less is used, the problems that may occur when a thermoplastic elastomer having an MFR exceeding 400 g / 10 min is used can be suppressed. Furthermore, even if thermal transfer recording is performed continuously, the color tone is not easily turbid on the printing surface 31 of the printing tape 2 and is clearly separated into two colors, and no unnecessary peeling occurs, and text with excellent clarity can be recorded. In order to further enhance these effects, the MFR of the thermoplastic elastomer is preferably 2.5 g / 10 min or less, and particularly preferably 2.3 g / 10 min or less in the above range.

[0127] There is no particular restriction on the lower limit of MFR, and the thermoplastic elastomer with a measurement result of "No Flow" at the temperature of 190°C and a load of 2.16 kg described above can also be used. There is no particular restriction on specific examples of the thermoplastic elastomer, and for example, the following various thermoplastic elastomers can be listed. These thermoplastic elastomers can be used alone or in combination of two or more.

[0128] Among the SEBS of the Tuftec (registered trademark) series manufactured by Asahi Kasei Corporation, H1521 [MFR: 2.3 g / 10 min], H1051 [MFR: less than 0.8 g / 10 min], H1052 [MFR: less than 13.0 g / 10 min], H1272 [MFR: no flow], P1083 [MFR: 3.0 g / 10 min], P1500 [MFR: 4.0 g / 10 min], P5051 [MFR: 3.0 g / 10 min], and P2000 [MFR: 3.0 g / 10 min].

[0129] Among the Tufprene (registered trademark) series of SBS manufactured by Asahi Kasei Corporation, A [MFR: 2.6 g / 10 min], 125 [MFR: 4.5 g / 10 min], and 126S [MFR: 4.5 g / 10 min].

[0130] Among Asaprene (registered trademark) T series SBS manufactured by Asahi Kasei Corporation, T-411 [MFR: no flow], T-432 [MFR: no flow], T-437 [MFR: no flow], T-438 [MFR: no flow], and T-439 [MFR: no flow].

[0131] Among the SEPS of the SEPTON (registered trademark) series manufactured by Kuraray Co., Ltd., 2002〔MFR: 70 g / 10 min〕, 2004F〔MFR: 5 g / 10 min〕, 2005〔MFR: no flow〕, 2006〔MFR: no flow〕, 2063〔MFR: 7 g / 10 min〕, and 2104〔MFR: 0.4 g / 10 min〕, the MFR of these SEPS was measured under the conditions of a temperature of 230°C and a load of 2.16 kg.

[0132] Among the SEEPS of the SEPTON (registered trademark) series manufactured by Kuraray Co., Ltd., 4033〔MFR: <0.1 g / 10 min〕, 4044〔MFR: no flow〕, 4055〔MFR: no flow〕, 4077〔MFR: no flow〕, and 4099〔MFR: no flow〕. The MFR of these SEEPS was measured under the conditions of a temperature of 230°C and a load of 2.16 kg.

[0133] Among the HYBRAR (registered trademark) series of vinyl SIS manufactured by Kuraray Co., Ltd., 5125 [MFR: 4 g / 10 min] and 5127 [MFR: 5 / 10 min].

[0134] Ultrathene (registered trademark) series EVA manufactured by Tosoh Corporation: 514R [MFR: 0.41 g / 10 min], 515 [MFR: 2.5 g / 10 min], 510 [MFR: 2.5 g / 10 min], 510F [MFR: 2.5 g / 10 min], 520F [MFR: 2.0 g / 10 min], 540 [MFR: 3.0 g / 10 min], 540F [MFR: 3.0 g / 10 min] in], 537 [MFR: 8.5g / 10min], 537L [MFR: 8.5g / 10min], 537S-2 [MFR: 8.5g / 10min], 541 [MFR: 9.0g / 10min] , 541L [MFR: 9.0g / 10min], 530 [MFR: 75g / 10min], 526 [MFR: 25g / 10min], 630 [MFR: 1.5g / 10min], 631 [MFR :1.5g / 10min], 636 [MFR: 2.5g / 10min], 625 [MFR: 14g / 10min], 626 [MFR: 3.0g / 10min], 627 [MFR: 0.8g / 1 0min], 633 [MFR: 20g / 10min], 635 [MFR: 2.4g / 10min], 640 [MFR: 2.8g / 10min], 634 [MFR: 4.3g / 10min], 68 0 [MFR: 160g / 10min], 681 [MFR: 350g / 10min], 751 [MFR: 5.7g / 10min], 710 [MFR: 18g / 10min], 720 [MFR: 15 0g / 10min], 722 [MFR: 400g / 10min], 750 [MFR: 30g / 10min], 752 [MFR: 60g / 10min], 760 [MFR: 70g / 10min].

[0135] The intermediate layer 51 can be formed, for example, by applying a coating obtained by dissolving or dispersing a material for forming the intermediate layer 51 including at least a thermoplastic elastomer in an arbitrary solvent onto the first thermal transfer layer 50 and then drying the coating.

[0136] The thickness of the intermediate layer 51 can be arbitrarily set according to the specifications of the thermal transfer printer, for example. The thickness of the intermediate layer 51 can be adjusted by the coating amount of the intermediate layer 51. For example, the coating amount of the intermediate layer 51 is expressed as 0.1 g / m 2 Above, preferably 0.2 g / m 2 For example, the coating amount of the intermediate layer 51 is 2.0 g / m 2Below, preferably 1.5g / m 2 For example, the coating amount of the intermediate layer 51 is expressed as 0.1 g / m 2 Above and 2.0g / m 2 Below, preferably 0.2g / m 2 Above and 1.5g / m 2 the following.

[0137] The specific thickness (before printing) of the intermediate layer 51 is, for example, 0.05 μm or more, preferably 0.2 μm or more. The thickness of the intermediate layer 51 is, for example, 2.0 μm or less, preferably 1.5 μm or less. The thickness of the intermediate layer 51 can be, for example, 0.05 μm or more and 2.0 μm or less, preferably 0.2 μm or more and 1.5 μm or less. The thickness of the intermediate layer 51 can be confirmed based on, for example, a SEM (Scanning Electron Microscope) image, a TEM (Transmission Electron Microscope) image, or the like of the thermal transfer recording medium 47.

[0138] It should be noted that due to the limitation of coating accuracy, the thickness of the intermediate layer 51 may sometimes have errors depending on the measurement position. The coating amount and thickness of the intermediate layer 51 may also include such errors. For example, 0.2 g / m 2 The intermediate layer 51 formed by the coating amount may include a coating amount of 0.1 g / m 2 The coating amount forms an area of ​​thickness of the case.

[0139] (5) Second thermal transfer layer 52

[0140] The second thermal transfer layer 52 can be formed of any thermoplastic resin, for example. Examples of the thermoplastic resin used in the second thermal transfer layer 52 include epoxy resin, polyester resin, polyolefin resin, etc. The thermoplastic resin can be appropriately selected according to the material of the printing tape 2. When the first thermal transfer layer 50 is formed of epoxy resin, it is preferred that the second thermal transfer layer 52 is also formed of epoxy resin.

[0141] By forming the second thermal transfer layer 52 with epoxy resin, the adhesion of the first thermal transfer layer 50 to the substrate layer 48 and the intermediate layer 51 can be balanced with the adhesion of the second thermal transfer layer 52 to the printing tape 2. As a result, the first thermal transfer layer 50 and the intermediate layer 51 can be well separated to the substrate layer 48 side, and the second thermal transfer layer 52 can be separated to the printing tape 2 side during high-temperature transfer. Since the high-temperature transfer range can be extended to the low-temperature side, the effect of suppressing color turbidity can be further improved. As the epoxy resin, various epoxy resins exemplified as the epoxy resin of the first thermal transfer layer 50 can be cited. These epoxy resins can be used alone or in combination of two or more.

[0142] The second thermal transfer layer 52 may contain wax in addition to the thermoplastic resin. By containing wax, the first thermal transfer layer 50 and the intermediate layer 51 can be separated to the substrate layer 48 side, and the second thermal transfer layer 52 can be separated to the printing tape 2 side during high-temperature transfer. Therefore, the high-temperature transfer range can be extended to the low-temperature side, thereby further improving the effect of suppressing color turbidity.

[0143] As the wax, any wax having affinity and compatibility with thermoplastic resins such as epoxy resins can be used. For example, natural waxes such as carnauba wax, paraffin wax, and microcrystalline wax, and synthetic waxes such as Fischer-Tropsch wax can be used. Specific examples of waxes are not particularly limited, and examples thereof include carnauba wax No. 1 flakes, No. 2 flakes, No. 3 flakes, No. 1 powder, and No. 2 powder (all of which have a melting point of 80 to 86°C) manufactured by Toyo Chemical Co., Ltd., paraffin waxes such as EMUSTAR-1155 (melting point: 69°C), EMUSTAR-0135 (melting point: 60°C), and EMUSTAR-0136 (melting point: 60°C) manufactured by Nippon Seiwa Co., Ltd., microcrystalline waxes such as EMUSTAR-0001 (melting point: 84°C) and EMUSTAR-042X (melting point: 84°C) manufactured by Nippon Seiwa Co., Ltd., and Fischer-Tropsch waxes such as FNP-0090 (freezing point: 90°C), SX80 (freezing point: 83°C), FT-0165 (melting point: 73°C), and FT-0070 (melting point: 72°C) manufactured by Nippon Seiwa Co., Ltd. These waxes can be used alone or in combination of two or more.

[0144] The second thermal transfer layer 52 may contain any colorant. As the colorant, one or more various colorants corresponding to the color tone of the second thermal transfer layer 52 may be used. As the colorant, for example, a pigment may be used. If the improvement of the weather resistance of the text is taken into consideration, a pigment is preferably used as the colorant used in the second thermal transfer layer 52. For example, as a pigment for coloring the second thermal transfer layer 52 in red, the following various red pigments may be listed. These red pigments may be used alone or in combination of two or more.

[0145] CI Pigment Red 5, 7, 9, 12, 48 (Ca), 48 (Mn), 49, 52, 53, 53:1, 57 (Ca), 57:1, 97, 112, 122, 123, 149, 168, 177, 178, 179, 184, 202, 206, 207, 209, 242, 254, 255.

[0146] The ratio of each component in the second thermal transfer layer 52 is not particularly limited. The ratio of the wax to 100 parts by mass of the epoxy resin is, for example, 3 parts by mass or more, preferably 5 parts by mass or more. The ratio of the wax to 100 parts by mass of the epoxy resin is, for example, 11 parts by mass or less, preferably 9 parts by mass or less. The ratio of the wax to 100 parts by mass of the epoxy resin is, for example, 3 parts by mass or more and 11 parts by mass or less, preferably 5 parts by mass or more and 9 parts by mass or less.

[0147] The ratio of the colorant such as the red pigment to 100 parts by mass of the epoxy resin is, for example, 70 parts by mass or more, preferably 80 parts by mass or more. The ratio of the colorant such as the red pigment to 100 parts by mass of the epoxy resin is, for example, 140 parts by mass or less, preferably 120 parts by mass or less. The ratio of the colorant such as the red pigment to 100 parts by mass of the epoxy resin is, for example, 70 parts by mass or more and 140 parts by mass or less, preferably 80 parts by mass or more and 120 parts by mass or less.

[0148] The second thermal transfer layer 52 can be formed, for example, by applying a coating agent obtained by dissolving or dispersing the above-mentioned components in an arbitrary solvent on the intermediate layer 51 and then drying the coating agent.

[0149] The thickness of the second thermal transfer layer 52 can be arbitrarily set according to the specifications of the thermal transfer printer, etc. The thickness of the second thermal transfer layer 52 can be adjusted by the coating amount of the second thermal transfer layer 52. For example, the coating amount of the second thermal transfer layer 52 is expressed as 0.2 g / m 2 Above, preferably 1.0 g / m 2 For example, the coating amount of the second thermal transfer layer 52 is 7.0 g / m 2 Below, preferably 5.0g / m 2 For example, the coating amount of the second thermal transfer layer 52 is 0.2 g / m 2 Above and 7.0g / m 2 Below, preferably 1.0g / m 2 Above and 5.0g / m 2 the following.

[0150] The specific thickness (before printing) of the second thermal transfer layer 52 is, for example, 0.05 μm or more, preferably 1.0 μm or more. The thickness of the second thermal transfer layer 52 is, for example, 7.0 μm or less, preferably 5.0 μm or less. The thickness of the second thermal transfer layer 52 can be, for example, 0.05 μm or more and 7.0 μm or less, preferably 1.0 μm or more and 5.0 μm or less. The thickness of the second thermal transfer layer 52 can be confirmed based on, for example, a SEM (Scanning Electron Microscope) image, a TEM (Transmission Electron Microscope) image, or the like of the thermal transfer recording medium 47.

[0151] [Introduction of the intermediate layer 51 based on irreversible change of force]

[0152] exist Figure 6 In the embodiment of the present invention, as an example of a thermal transfer recording medium (ink ribbon) capable of simultaneously recording text with good clarity and in at least two colors, a thermal transfer recording medium 47 having an intermediate layer 51 containing a thermoplastic elastomer is shown. The inventors of the present application have also studied and implemented thermal transfer recording media that exhibit the same effect from other viewpoints, and the following will describe them in detail. To put it bluntly, with respect to Figure 6 In the above, attention is paid to the chemical composition of the components of the intermediate layer 51 , and below, attention is paid to the irreversible change of the interlayer adhesive force caused by the control of the reaching temperature of the thermal transfer recording medium 47 .

[0153] Figure 7 It is shown Figure 1~Figure 4A , B is a diagram showing the relationship between the elapsed time and the reaching temperature of the thermal transfer recording medium 47 in the heating step and the cooling step.

[0154] Figure 7 The horizontal axis of represents the elapsed time of the printing process of the printing device 1. t0 represents the start time of printing, t1 represents the end time of heating by the thermal head 6, and t2 represents the arrival time of the ribbon peeling member 13. Figure 7 The vertical axis represents the arrival temperature of the thermal transfer recording medium 47. The arrival temperature of the thermal transfer recording medium 47 can be defined as the temperature of the thermal transfer recording medium 47 that changes due to external factors. The external factors may include, for example, heating by the thermal head 6, natural cooling of the thermal transfer recording medium 47 during transportation, and the like.

[0155] Reference Figure 7In the printing device 1, the temperature output (temperature energy) of the thermal head 6 is controlled by the control circuit 22, so that the reaching temperature of the thermal transfer recording medium 47 can be controlled. For example, a relatively low first energy is applied to the thermal head 6 in the heating process. In this case, the temperature of the thermal transfer recording medium 47 increases exponentially from the ambient temperature (e.g., room temperature) TE around the thermal transfer recording medium 47 as shown by the first temperature curve 55 of the single-point chain line and reaches T R1 .

[0156] Reach temperature T R1 It can be defined as a temperature that is higher than the first temperature T1 and lower than the second temperature T2. For example, the first temperature T1 is higher than 60°C and lower than 120°C, preferably higher than 70°C and lower than 90°C. For example, the second temperature T2 is higher than 80°C and lower than 180°C, preferably higher than 130°C and lower than 150°C. The reaching temperature T R1 The temperature can be set appropriately according to the output setting method of the thermal head 6 of the printing device 1 used. For example, the reaching temperature can be set in association with quantitative parameters such as the voltage, current, and power-on time supplied to the heating element 20 of the thermal head 6. In addition, the reaching temperature can also be set in association with a relative value relative to a predetermined reference value (for example, the value before power-on is 0 (zero)).

[0157] On the other hand, in the heating process, a second energy relatively higher than the first energy is applied to the thermal head 6. In this case, the temperature of the thermal transfer recording medium 47 increases exponentially from the ambient temperature TE to reach T TE as shown by the second temperature curve 56 of the solid line. R2 . Reach temperature T R2 It can be defined as a temperature exceeding the second temperature T2.

[0158] After the heating process, the thermal transfer recording medium 47 is naturally cooled in the section until it reaches the ink ribbon peeling member 13 (see also Figure 3 as well as Figure 4A , B). In the cooling process, the temperature of the thermal transfer recording medium 47 is reduced from the reaching temperature T R1 and T R2 decreases exponentially and reaches T P The reaching temperature at this time is T P It is the temperature at which a portion of the thermal transfer recording medium 47 is peeled off by the ribbon peeling member 13, and thus can be defined as the peeling temperature T P . Peeling temperature T PPreferably, it is below the third temperature T3. The third temperature T3 is lower than the first temperature T1 (i.e., the first temperature T1 is above the third temperature T3), for example, above 40°C and below 90°C, preferably above 60°C and below 80°C. Considering the chemical composition and physical properties of the ink of the thermal transfer recording medium 47, the first temperature T1, the second temperature T2, and the third temperature T3 can be appropriately set within the temperature range required for transfer to the printing tape 2.

[0159] Regardless of which heating control is performed in the heating process, the temperature curve (cooling curve) of the thermal transfer recording medium 47 in the cooling process will eventually converge to a constant temperature. Therefore, by ensuring a long cooling process time (t1→t2), the peeling temperature T of the first temperature curve 55 and the second temperature curve 56 can be made P In order to extend the cooling process time, for example, the distance between the thermal head 6 and the ink ribbon stripping member 13 is extended ( Figure 1 For example, the peeling distance L1 can be Figure 7 The state of the thermal transfer recording medium 47 after the heating process and the cooling process are performed according to the temperature change shown by the first temperature curve 55 is defined as the first state C1. Figure 7 The state of the thermal transfer recording medium 47 after the heating step and the cooling step are performed by the temperature change shown in the second temperature curve 56 is defined as a second state C2.

[0160] In this way, in the printing device 1, by controlling the temperature output (temperature energy) of the thermal head 6, the starting temperature (ambient temperature T E ) and the final temperature (peeling temperature T P ) is constant, and the arrival temperature of the thermal transfer recording medium 47 is varied. Considering this temperature control, for example, it is expected that Figure 6 The temperature output of the thermal head 6 is controlled by the physical properties of the base layer 48, the back layer 49, the first thermal transfer layer 50, the intermediate layer 51 and the second thermal transfer layer 52 of the thermal transfer recording medium 47, thereby controlling the adhesion between the layers of the thermal transfer recording medium 47.

[0161] Figure 8 as well as Fig. 9 This is a diagram showing the relationship between the elapsed time and the interlayer adhesive force of the thermal transfer recording medium 47 in the heating step and the cooling step. Figure 8 The temperature of the thermal transfer recording medium 47 is shown as follows: Figure 6 The changes in the adhesive forces F when the first temperature curve 55 changes. Fig. 9The temperature of the thermal transfer recording medium 47 is shown as follows: Figure 6 The changes in the respective adhesive forces F when the second temperature curve 56 changes.

[0162] Figure 8 as well as Fig. 9 The horizontal axis of represents the elapsed time of the printing process of the printing device 1. t0 represents the start time of printing, t1 represents the end time of heating by the thermal head 6, and t2 represents the arrival time of the ribbon peeling member 13. Figure 8 as well as Fig. 9 The vertical axis represents the magnitude of the adhesive force between the layers of the thermal transfer recording medium 47 .

[0163] exist Figure 8 as well as Fig. 9 , the first adhesive force F1 between the base material layer 48 of the thermal transfer recording medium 47 and the first thermal transfer layer 50 is represented by a solid line first adhesive force curve 57. In addition, the second adhesive force F2 between the first thermal transfer layer 50 and the second thermal transfer layer 52 is represented by a single-point dashed line second adhesive force curve 58. The first adhesive force F1 may include the force when the base material layer 48 and the first thermal transfer layer 50 are separated from each other, and the force when the first thermal transfer layer 50 is broken internally. The second adhesive force F2 may include the force when the intermediate layer 51 and the second thermal transfer layer 52 are separated from each other, and the force when the intermediate layer 51 is broken internally. In addition, in the case where the components of the first thermal transfer layer 50 and the intermediate layer 51 are mixed by melting to form a mixed layer, the force when the mixed layer and the second thermal transfer layer 52 are separated from each other may also be included.

[0164] Reference Figure 8 as well as Fig. 9 The first adhesive force F1 and the second adhesive force F2 both change over time as the heating process and the cooling process are performed, regardless of the energy applied to the thermal head 6 during the heating process. More specifically, the first adhesive force F1 and the second adhesive force F2 decrease together with the passage of the heating time, and the first adhesive force F1 and the second adhesive force F2 increase together with the passage of the cooling time after heating.

[0165] The magnitude relationship between the first adhesive force F1 and the second adhesive force F2 before heating and after cooling changes according to the energy applied to the thermal head 6. Figure 8As shown in FIG. 1 , when the energy applied to the thermal head 6 is relatively low, the second adhesive force F2 is greater than the first adhesive force F1 both before heating and after cooling (first state C1). Therefore, if peeling is performed in the first state C1, the first adhesive force F1 is less than the second adhesive force F2, so peeling occurs between the base layer 48 and the first thermal transfer layer 50, and the first thermal transfer layer 50 and the second thermal transfer layer 52 in the bonded state are transferred to the printing tape 2. On the other hand, in order to adjust the condition that the first adhesive force F1 is less than the second adhesive force F2 after cooling, it is preferable to at least Fig. 9 The cooling process is performed for a long time t3 corresponding to the intersection 59 of the first adhesive force curve 57 and the second adhesive force curve 58. This is because the thermal transfer recording medium 47 is sufficiently cooled, and cold peeling can be performed reliably.

[0166] In addition, for example Fig. 9 As shown, when the energy applied to the thermal head 6 is relatively high, the magnitude relationship between the first adhesive force F1 and the second adhesive force F2 is reversed before heating and after cooling (the second state C2). Before heating, the second adhesive force F2 is greater than the first adhesive force F1. On the other hand, after cooling (the second state C2), the second adhesive force F2 is less than the first adhesive force F1. In other words, the first adhesive force F1 undergoes an irreversible change. Therefore, if peeling is performed in the second state C2, the first adhesive force F1>the second adhesive force F2, so peeling occurs between the first thermal transfer layer 50 and the second thermal transfer layer 52, and the second thermal transfer layer 52 is transferred to the printing tape 2. On the other hand, in order to adjust to the condition where the first adhesive force F1>the second adhesive force F2 after cooling, it is preferably at least greater than Fig. 9 The cooling process is performed for a long time during the time t3 corresponding to the intersection 60 of the first adhesive force curve 57 and the second adhesive force curve 58. This is because the thermal transfer recording medium 47 is sufficiently cooled, and cold peeling can be performed reliably.

[0167] The time t3 may be appropriately set such that the first adhesive force F1 < the second adhesive force F2 after the thermal transfer recording medium 47 heated by low energy cools down, and the first adhesive force F1 > the second adhesive force F2 after the thermal transfer recording medium 47 heated by high energy cools down. For example, in either case of applying low energy or applying high energy, the time required to make the reaching temperature of the thermal transfer recording medium 47 lower than the third temperature T3 may be set. The peeling distance L1 (see FIG. 1 ) required to ensure the time t3 is Figure 1 ) is, for example, greater than 70 mm and less than 150 mm, preferably greater than 90 mm and less than 120 mm.

[0168] In this way, by utilizing the irreversible change of the first adhesive force F1 caused by the energy applied to the thermal head 6, the peeling position of the thermal transfer recording medium 47 can be freely controlled, thereby providing a thermal transfer recording medium 47 that can simultaneously record text with good clarity and in at least two colors.

[0169] (1) Peeling Mode of Thermal Transfer Recording Medium 47

[0170] Figure 10~Figure 15 47 is a diagram showing a peeled state of the thermal transfer recording medium 47. Figure 10~Figure 15 , how the thermal transfer recording medium 47 is peeled off is described based on the magnitude relationship between the first adhesive force F1 and the second adhesive force F2. Figure 10~Figure 15 , a plurality of peeling modes are listed for the thermal transfer recording medium 47. Figure 10~Figure 15 The peeling modes are referred to as the first to sixth peeling modes in sequence. From the perspective of the energy supplied to the thermal head 6, the following can be distinguished: Fig.10 as well as Fig.11 The low energy peeling mode and Figure 12~Figure 15 High energy peeling mode shown.

[0171] Fig.10 as well as Fig.11 is through Figure 7 The peeling mode is performed in the first state C1 when the peeling (thermal transfer) is performed by heating control (low energy application) of the first temperature curve 55. Fig.10 In the first peeling mode, in the first state C1, the breaking strength (first adhesive force F1) between the base material layer 48 and the first thermal transfer layer 50 is the smallest in the thermal transfer recording medium 47, and peeling occurs at their interface. Fig.11 In the second peeling mode, in the first state C1 , the breaking strength (first adhesive force F1 ) in the first thermal transfer layer 50 is the smallest in the thermal transfer recording medium 47 , and peeling occurs inside the first thermal transfer layer 50 . Fig.10 The first peeling mode is interface failure. Fig.11 The second peeling mode is cohesive failure. Fig.10 as well as Fig.11 In any of the peeling modes, the first thermal transfer layer 50 and the second thermal transfer layer 52 in an adhered state are transferred to the printing tape 2 .

[0172] Figure 12~Figure 15 is through Figure 7 The peeling mode when peeling (thermal transfer) is performed in the second state C2 is performed by heating control (high energy application) of the second temperature curve 56 . Figure 12~Figure 15 The peeling mode can also be divided into at least two types, namely, interface failure and cohesive failure, similarly to the first and second peeling modes.

[0173] exist Fig.12 In the third peeling mode, in the second state C2, the breaking strength (second adhesive force F2) between the first thermal transfer layer 50 and the second thermal transfer layer 52 is the smallest in the thermal transfer recording medium 47, and peeling (interface failure) occurs at their interface. Fig.13 In the fourth peeling mode, in the second state C2 , the breaking strength (second adhesive force F2 ) in the second thermal transfer layer 52 is minimum in the thermal transfer recording medium 47 , and peeling (cohesive failure) occurs inside the second thermal transfer layer 52 .

[0174] exist Fig.14 In the fifth peeling mode, in the second state C2, the breaking strength (second adhesive force F2) in the intermediate layer 51 is the smallest in the thermal transfer recording medium 47, and peeling (cohesive failure) occurs inside the intermediate layer 51. Fig.15 In the sixth peeling mode, in the second state C2, the layer in contact with the second thermal transfer layer 52 is the mixed layer 61 formed by melting and mixing the components of the first thermal transfer layer 50 and the intermediate layer 51. In addition, the breaking strength (second adhesive force F2) between the mixed layer 61 and the second thermal transfer layer 52 is the smallest in the thermal transfer recording medium 47, and peeling (interface failure) occurs at their interface.

[0175] exist Figure 12~Figure 15 In any of the peeling modes, the second thermal transfer layer 52 is selectively transferred to the printing tape 2 in a manner that the first thermal transfer layer 50 does not remain.

[0176] Whether the thermal transfer recording medium 47 is Figure 10~Figure 15 Whether any of the peeling modes is broken can be confirmed by, for example, observing a cross section of the broken thermal transfer recording medium 47. For example, it can be confirmed based on a SEM (Scanning Electron Microscope) image or a TEM (Transmission Electron Microscope) image of the broken thermal transfer recording medium 47.

[0177] As described above, in the first to second peeling modes, the text recorded on the printing surface 31 of the printing tape 2 becomes the color tone of the first thermal transfer layer 50, such as black. In the third to sixth peeling modes, the text recorded on the printing surface 31 of the printing tape 2 becomes the color tone of the second thermal transfer layer 52, such as red.

[0178] Therefore, in order to provide a thermal transfer recording medium 47 capable of simultaneously recording text with good clarity and in at least two colors, at least one of the first to second peeling modes is achieved during the heating control (low energy application) of the first temperature curve 55, and at least one of the third to sixth peeling modes is achieved during the heating control (high energy application) of the second temperature curve 56. In order to achieve these peeling modes, the conditions of each layer of the thermal transfer recording medium 47 were studied from the following multiple viewpoints.

[0179] (2) Chemical composition of each layer of thermal transfer recording medium 47

[0180] From the viewpoint of the chemical composition of each layer of the thermal transfer recording medium 47, the chemical composition of each layer of the base layer 48, the back layer 49, the first thermal transfer layer 50, the intermediate layer 51, and the second thermal transfer layer 52 shown in the above-mentioned "[Introduction of the intermediate layer 51 containing the thermoplastic elastomer]" is preferred. Of course, the thermal transfer recording medium 47 having this chemical composition is different from the intermediate layer 51 containing the thermoplastic elastomer. Figure 7 Regardless of the temperature control shown, it is possible to simultaneously record text with good clarity and in at least two colors using a general-purpose thermal transfer printer by controlling the temperature under normal conditions.

[0181] In Figure 7 In the case of performing thermal transfer in the printing device 1 by temperature control as shown, in addition to the aforementioned thermoplastic elastomer, other compositions can be used as the intermediate layer 51. For example, the intermediate layer 51 can contain at least one of a polyolefin resin and a long-chain alkyl resin. These resins have low polarity. Figure 7 When peeling (thermal transfer) is performed in the second state C2 by heating control (high energy application) of the second temperature profile 56, cohesive failure can be caused inside the intermediate layer 51. Thus, peeling between the first thermal transfer layer 50 and the second thermal transfer layer 52 can be performed well.

[0182] Examples of the polyolefin-based resin include Surflen (registered trademark) P-1000 manufactured by Mitsubishi Chemical Corporation.

[0183] Examples of the long-chain alkyl resin include PEROYL (registered trademark) series manufactured by Lion Chemical Industries, Ltd., 1010, 1010S, 1050, 1070, and 406.

[0184] By providing the intermediate layer 51 including the resin exemplified above, it is also possible to provide a thermal transfer recording medium 47 on which characters in at least two colors can be recorded simultaneously with good clarity.

[0185] (3) Solubility parameter (SP value) of each layer of the thermal transfer recording medium 47

[0186] From the perspective of the physical properties of each layer of the thermal transfer recording medium 47, the relative relationship of the solubility parameters (SP values) of the constituents of each layer is focused on. By adjusting the SP values ​​of the constituents of each layer, the interlayer adhesion and internal peeling of the thermal transfer recording medium 47 can be controlled. The closer the SP values ​​of the constituents in contact with each other are, the easier it is to adhere (higher affinity), and the more separated the SP values ​​are, the easier it is to peel off (lower affinity). Therefore, by adjusting the balance of the SP values ​​and content rates of the constituents of each layer of the thermal transfer recording medium 47, the peeling position in the thermal transfer recording medium 47 can be flexibly controlled. As a result, a thermal transfer recording medium 47 that can simultaneously record text with good clarity and at least two colors is provided.

[0187] In the following, when the relative relationship (size relationship) of the SP values ​​is shown, as long as the calculation conditions of the SP values ​​of the comparison objects are the same, for example, the SP value may be either the HSP value (Hansen solubility parameter) or the SP value (Hildebrand solubility parameter). In addition, the calculation method of the SP value is not particularly limited, and it may be any of the methods of calculating the SP value, such as the method of obtaining the SP value based on the latent heat of evaporation, the method based on the Hildebrand Rule, the method based on the surface tension, and the method of calculating the SP value based on the molecular structure, such as the Small calculation method, the Fedors calculation method, the Hansen calculation method, and the Hoy calculation method. It should be noted that, unless otherwise specified, the SP value in the present invention showing the range of the SP value and the specific numerical value is the SP value (Hildebrand solubility parameter).

[0188] Fig.16 This is a diagram for comparing the solubility parameters (SP values) of the constituent materials of the thermal transfer recording medium 47 according to one embodiment of the present invention.

[0189] Reference Fig.16 The first thermal transfer layer 50 is composed of at least a first material 62 and a second material 63. The first material 62 is a material having a relatively lower SP value than the second material 63. The SP value of the first material 62 is, for example, 7.5 to 9.5, preferably 8.0 to 9.0. As the first material 62, the adhesive and tackifier exemplified as the components of the first thermal transfer layer 50 described above in “[Introduction of the intermediate layer 51 including the thermoplastic elastomer]” can be cited.

[0190] The second material 63 is a material having a relatively higher SP value than the first material 62. The SP value of the second material 63 is, for example, 9.0 to 12.0, preferably 10.0 to 11.0. As the second material 63, the thermoplastic resin exemplified as a component of the first thermal transfer layer 50 in the aforementioned “[Introduction of the intermediate layer 51 including the thermoplastic elastomer]” can be cited.

[0191] Regarding the weight ratio of the first material 62 and the second material 63 in the first thermal transfer layer 50, for example, the first material 62 is 30 parts by mass or more, preferably 45 parts by mass or more, relative to 100 parts by mass of the second material 63. For example, relative to 100 parts by mass of the second material 63, the first material 62 is 300 parts by mass or less, preferably 200 parts by mass or less. For example, relative to 100 parts by mass of the second material 63, the first material 62 is 30 parts by mass or more and 300 parts by mass or less, preferably 45 parts by mass or more and 200 parts by mass or less.

[0192] The intermediate layer 51 is composed of at least a third material 64. The third material 64 is a material having a relatively low SP value compared to the second material 63 and the fifth material 66 (described later). The SP value of the third material 64 is, for example, 7.5 to 10.0, preferably 8.0 to 9.0. As the third material 64, in addition to the thermoplastic elastomers exemplified in the aforementioned "[Introduction of the intermediate layer 51 containing the thermoplastic elastomer]", polyolefin resins and long-chain alkyl resins can also be cited.

[0193] The second thermal transfer layer 52 is composed of at least a fourth material 65 and a fifth material 66. The fourth material 65 is a material having a relatively higher SP value than the fifth material 66. The SP value of the fourth material 65 is, for example, 9.0 to 12.0, preferably 10.0 to 11.0. As the fourth material 65, the thermoplastic resins exemplified as the components of the second thermal transfer layer 52 in the aforementioned “[Introduction of the intermediate layer 51 including the thermoplastic elastomer]” can be cited.

[0194] The fifth material 66 is a material having a relatively lower SP value than the fourth material 65. The SP value of the fifth material 66 is, for example, 7.5 to 9.5, preferably 8.0 to 9.0. The fifth material 66 may include wax or the like exemplified as a component of the second thermal transfer layer 52 in the aforementioned “[Introduction of the intermediate layer 51 including the thermoplastic elastomer]”.

[0195] Regarding the weight ratio of the fourth material 65 and the fifth material 66 in the second thermal transfer layer 52, for example, the fifth material 66 is 3 parts by mass or more, preferably 5 parts by mass or more, relative to 100 parts by mass of the fourth material 65. For example, relative to 100 parts by mass of the fourth material 65, the fifth material 66 is 11 parts by mass or less, preferably 9 parts by mass or less. For example, relative to 100 parts by mass of the fourth material 65, the fifth material 66 is 3 parts by mass or more and 11 parts by mass or less, preferably 5 parts by mass or more and 9 parts by mass or less.

[0196] Fig.17 This is a diagram showing the relationship between the type of material constituting a part of the thermal transfer recording medium 47 and the magnitude of the solubility parameter.

[0197] As described above, the names of materials that can be used as the first to fifth materials 62 to 66 are exemplified, but as long as the relative relationship (size relationship) of the SP values ​​in the thermal transfer recording medium 47 is as described above, the materials used are not particularly limited. Fig.17 The size relationship shown is used as a reference to select the appropriate material. At this time, it is considered that the closer the SP values ​​between the materials are, the easier it is to adhere, and the farther the SP values ​​are, the easier it is to peel.

[0198] For example, regarding the first thermal transfer layer 50, terpene phenol resin may be selected as the first material 62, and epoxy resin may be selected as the second material 63. For example, regarding the intermediate layer 51, thermoplastic elastomer, polyolefin, etc. may be selected as the third material 64. For example, regarding the second thermal transfer layer 52, wax may be selected as the fourth material 65, and epoxy resin may be selected as the fifth material 66.

[0199] If the SP values ​​are combined as described above, it is possible to Figure 7 At least one of the first to second peeling modes can be achieved when the heating control (low energy application) of the first temperature curve 55 is performed, and at least one of the third to sixth peeling modes can be achieved when the heating control (high energy application) of the second temperature curve 56 is performed. As a result, it is possible to provide a thermal transfer recording medium 47 that can simultaneously record text with good clarity and at least two colors.

[0200] Example

[0201] Hereinafter, the present invention will be further described based on a plurality of samples, but the structure of the present invention is not limited to these examples.

[0202] [Coating agent for first thermal transfer layer (I)]

[0203] The components shown in Table 1 below were dissolved in a mixed solvent of toluene and methyl ethyl ketone (MEK) at a mass ratio of 1 / 4 to prepare a first thermal transfer layer coating (I) having a solid content concentration of 22.5 mass %. The ratio of the active ingredient in the acrylic adhesive was 80 mass parts per 100 mass parts of the epoxy resin.

[0204]

Table 1

[0205]

[0206] The components in the table are as follows.

[0207] Epoxy resin: JER1007 manufactured by Mitsubishi Chemical Corporation〔basically solid type, softening point (ring and ball method): 128°C, number average molecular weight Mn: about 2900, SP value: 9.5~11.5〕

[0208] Acrylic adhesive: AS-665 manufactured by Lion Chemical Co., Ltd. [Solid content concentration: 40% by mass, SP value: 8.0 to 9.0]

[0209] Tackifier: terpene phenol resin, YS Polyster T80 manufactured by Yasuhara Chemical Co., Ltd. (softening point: 80±5°C, SP value: 8.0~9.5)

[0210] Carbon black: MA100 powder manufactured by Mitsubishi Chemical Corporation〔LFF, DBP absorption: 100 cm 3 / 100g〕

[0211] [Coating agent for first thermal transfer layer (II)]

[0212] The first thermal transfer layer coating (II) was prepared in the same manner as the first thermal transfer layer coating (I), except that an equal amount of JER1004 manufactured by Mitsubishi Chemical Corporation (basically solid type, softening point (ring and ball method): 97°C, number average molecular weight Mn: about 1650, SP value: 9.5 to 11.5) was added as the epoxy resin. The solid content concentration was 22.5% by mass, and the ratio of the active ingredient in the acrylic adhesive was 80 parts by mass per 100 parts by mass of the epoxy resin.

[0213] [Coating agent for first thermal transfer layer (III)]

[0214] The first thermal transfer layer coating (III) was prepared in the same manner as the first thermal transfer layer coating (I) except that the tackifier was not added and the amount of the acrylic adhesive was 271 parts by mass. The solid content concentration was 22.5% by mass, and the ratio of the active ingredient in the acrylic adhesive was 108.4 parts by mass per 100 parts by mass of the epoxy resin.

[0215] [Intermediate layer coating (1)]

[0216] A thermoplastic elastomer [Tuftec H1521 manufactured by Asahi Kasei Corporation, SEBS, MFR: 12.3 g / 10 min, styrene content 18% by mass, SP value: 7.5 to 9.0] was dissolved in a mixed solvent of toluene and hexane in a mass ratio of 1:1 to prepare an intermediate layer coating (1) having a solid content concentration of 10% by mass.

[0217] [Intermediate layer coating (2)]

[0218] An intermediate layer coating (2) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Tuftec H1517 manufactured by Asahi Kasei Corporation [SEBS, MFR: less than 3.0 g / 10 min, styrene content 43% by mass, SP value: 7.5 to 9.0] was added as a thermoplastic elastomer. The solid content concentration was 10% by mass.

[0219] [Intermediate layer coating (3)]

[0220] An intermediate layer coating (3) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Tuftec H1272 manufactured by Asahi Kasei Corporation [SEBS, MFR: non-flowing, styrene content 35% by mass, SP value: 7.5 to 9.0] was added as a thermoplastic elastomer. The solid content concentration was 10% by mass.

[0221] [Intermediate layer coating (4)]

[0222] An intermediate layer coating (4) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Tuftec H1221 manufactured by Asahi Kasei Corporation [SEBS, MFR: less than 4.5 g / 10 min, styrene content 12% by mass, SP value: 7.5 to 9.0] was added as the thermoplastic elastomer. The solid content concentration was 10% by mass.

[0223] [Intermediate layer coating (5)]

[0224] An intermediate layer coating (5) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Tuftec H1043 manufactured by Asahi Kasei Corporation [SEBS, MFR: less than 2.0 g / 10 min, styrene content 67% by mass, SP value: 7.5 to 9.0] was added as the thermoplastic elastomer. The solid content concentration was 10% by mass.

[0225] [Intermediate layer coating (6)]

[0226] An intermediate layer coating (6) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Tufprene A (SBS, MFR: 2.6 g / 10 min, styrene content 40% by mass, SP value: 7.5 to 9.0) manufactured by Asahi Kasei Corporation was added as a thermoplastic elastomer. The solid content concentration was 10% by mass.

[0227] [Intermediate layer coating (7)]

[0228] An intermediate layer coating (7) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Ultrathene 634 (EVA, MFR: 4.3 g / 10 min, SP value: 7.5 to 9.0) manufactured by Tosoh Corporation was added as the thermoplastic elastomer. The solid content concentration was 10% by mass.

[0229] [Intermediate layer coating (8)]

[0230] An intermediate layer coating (8) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Ultrathene 722 (EVA, MFR: 400 g / 10 min, SP value: 7.5 to 9.0) manufactured by Tosoh Corporation was added as a thermoplastic elastomer. The solid content concentration was 10% by mass.

[0231] [Intermediate layer coating (9)]

[0232] An intermediate layer coating (9) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Ultrathene 725 (EVA, MFR: 1000 g / 10 min, SP value: 7.5 to 9.0) manufactured by Tosoh Corporation was added as a thermoplastic elastomer. The solid content concentration was 10% by mass.

[0233] [Intermediate layer coating (10)]

[0234] An intermediate layer coating (10) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of Ultrathene 684 (EVA, MFR: 2000 g / 10 min, SP value: 7.5 to 9.0) manufactured by Tosoh Corporation was added as a thermoplastic elastomer. The solid content concentration was 10% by mass.

[0235] [Intermediate layer coating (11)]

[0236] An intermediate layer coating (11) was prepared in the same manner as the intermediate layer coating (1) except that an equal amount of amorphous polyester resin (VYLON (registered trademark) 200 manufactured by Toyobo Co., Ltd., SP value: 9.5 to 11.0) was added as a thermoplastic resin instead of the thermoplastic elastomer. The solid content concentration was 10% by mass.

[0237] [Intermediate layer coating (12)]

[0238] An intermediate layer coating (12) was prepared in the same manner as the intermediate layer coating (1), except that an equal amount of wax [Carnauba wax No. 2 flakes (melting point: 80-86°C), SP value: 7.0-9.0, manufactured by Toyochem Co., Ltd.] was added instead of the thermoplastic elastomer. The solid content concentration was 10% by mass.

[0239] [Intermediate layer coating (13)]

[0240] An intermediate layer coating (13) was prepared in the same manner as the intermediate layer coating (1), except that an equal amount of a modified polyolefin resin (Surflen (registered trademark) P-1000 manufactured by Mitsubishi Chemical Corporation, SP value: 7.5 to 8.5) was added instead of the thermoplastic elastomer. The solid content concentration was 10% by mass.

[0241] The material names, MFRs, and styrene contents of the intermediate layer coatings (1) to (13) are summarized in Table 2. The proportions of the constituent components are omitted because the solid content / toluene / hexane ratios of the intermediate layer coatings (1) to (13) are 10 / 45 / 45.

[0242]

Table 2

[0243]

[0244] [Coating agent for second thermal transfer layer (I)]

[0245] The components shown in Table 3 below were dissolved in a mixed solvent of toluene and MEK at a mass ratio of 1 / 4 to prepare a second thermal transfer layer coating agent (I) having a solid content concentration of 28% by mass.

[0246]

Table 3

[0247]

[0248] The components in the table are as follows.

[0249] Epoxy resin: JER1004 manufactured by Mitsubishi Chemical Corporation〔Basically solid type, softening point (ring and ball method): 97°C, number average molecular weight Mn: about 1650, SP value: 9.5~11.5〕

[0250] Wax: Carnauba wax No. 2 powder manufactured by Toyochem Co., Ltd. (melting point: 80~86℃, SP value: 7.0~9.0)

[0251] Red pigment: CI Pigment Red 53:1 [SYMULER (registered trademark) Lake Red C-102 manufactured by DIC Corporation]

[0252] [Sample 1~15]

[0253] (1) Manufacturing of thermal transfer recording media

[0254] First, a PET film with a thickness of 4.5 μm was prepared as a base layer. Next, a silicone resin having a solid content of 0.1 g / m2 per unit area was formed on the opposite side (back side) of the base layer on which the thermal transfer layer was formed. 2 Next, any of the first thermal transfer layer coating agents prepared previously is applied to the surface of the substrate layer and then dried to form a solid content per unit area of ​​1.5 g / m 2 Next, any intermediate layer coating agent prepared previously is applied on the first thermal transfer layer and then dried to form a solid content per unit area of ​​1 g / m 2 Next, the second thermal transfer layer coating agent (I) prepared previously was applied on the intermediate layer and then dried to form a solid content per unit area of ​​2.5 g / m 2 The second thermal transfer layer was formed to produce a thermal transfer recording medium. The composition of each layer of the thermal transfer recording medium obtained from Samples 1 to 15 is shown in Tables 4 to 6 below. In the table, NF in the column of the adhesive of the intermediate layer means no flow.

[0255] (2) Evaluation

[0256] (2-1) Continuous Record Evaluation

[0257] The thermal transfer recording medium produced by each sample was cut into a strip of a specified width and wound into a roll, and installed in a thermal transfer printer [ZEBRA110Xi4 printer manufactured by Zebra Corporation]. Next, under an external temperature of 25°C, the energy value pre-set in the thermal transfer printer and applied to the thermal head was set to 16 (low temperature, black) or 24 (high temperature, red), and a solid image of 70 mm square was continuously recorded 20 times on the surface of a variable information printing label material [polyester film (white·smooth), FR1415-50 manufactured by LINTEC Corporation] at a printing speed of 5 inches / sec. If some turbidity was observed in the middle of the recording, the continuous printing was terminated at that point, and the number of times printed in black or red was recorded as the number of continuous printings. During the evaluation, it was considered that the sample with black printed even at the 20th time had excellent continuous printing performance of more than 20 times, and the sample with turbidity below the 3rd time was not practical enough. The results are shown in Tables 4 to 6.

[0258] (2-2) Evaluation of the clarity of records

[0259] The thermal transfer recording medium produced from each sample was cut into a strip of a predetermined width and wound into a roll, and then installed in a thermal transfer printer [ZEBRA110Xi4 printer manufactured by ZEBRA Co., Ltd.]. Next, in an environment with an outside temperature of 25°C, the energy value pre-set in the thermal transfer printer to be applied to the thermal head was set to 16 (low temperature, black) or 24 (high temperature, red), and a barcode was recorded on the surface of a variable information printing label material [polyester film (white and smooth), FR1415-50 manufactured by LINTEC Co., Ltd.] at a printing speed of 5 inches / sec. The recorded barcode was then read using a barcode verification machine (Laser Examiner Elite IS manufactured by MUNAZOWO Co., Ltd.), and the decodability level specified in the American National Standards Institute standard ANSI X3.182-1990 was determined based on the reading results. The clarity of the recording was evaluated according to the following criteria.

[0260] 0: Decodability level is A [Excellent] or B [Excellent] for both black and red.

[0261] △: For either black or red, the decodability level is C [Good], and the other is C [Good] or higher.

[0262] ×: For at least one of black and red, the decodability level is D [OK] or F [NOT].

[0263] The results are shown in Tables 4 to 6. It should be noted that among Samples 1 to 15, Samples 1 to 12 may be Examples, and Samples 13 to 15 may be Comparative Examples.

[0264]

Table 4

[0265]

[0266]

Table 5

[0267]

[0268]

Table 6

[0269]

[0270] According to the comparison between Samples 1 to 12 and Samples 13 to 15 in Tables 4 to 6, it can be seen that by providing an intermediate layer composed of a thermoplastic elastomer between the first thermal transfer layer and the second thermal transfer layer, the following thermal transfer recording medium is obtained: even if thermal transfer recording is performed continuously, the color tone is not easily turbid and is clearly divided into two colors, and no unnecessary peeling occurs, so that text with excellent clarity can be recorded.

[0271] In addition, according to the results of samples 1 to 12, EVA, SBS, SEBS, etc. are preferred as thermoplastic elastomers for forming the intermediate layer. Furthermore, considering further improvement of continuous recording performance, it is known that as thermoplastic elastomers, preferably, a thermoplastic elastomer having an MFR of 1000 g / 10 min or less at a temperature of 190° C. and a load of 2.16 kg is preferred, a thermoplastic elastomer having an MFR of 400 g / 10 min or less is further preferred, a thermoplastic elastomer having an MFR of 2.5 g / 10 min or less is particularly preferred, and a thermoplastic elastomer having an MFR of 2.3 g / 10 min or less is most preferred.

[0272] Comparison between Sample 1 and Sample 11 shows that, as the epoxy resin forming the first thermal transfer layer, an epoxy resin having a softening point of 95° C. or higher is preferred, an epoxy resin having a softening point of 110° C. or higher is further preferred, and an epoxy resin having a softening point of 125° C. or higher is particularly preferred. Furthermore, comparison between Sample 1 and Sample 12 shows that, it is preferred to mix a tackifier with the epoxy resin forming the first thermal transfer layer together with the acrylic adhesive.

[0273] [Samples 16~33]

[0274] (1) Manufacturing of thermal transfer recording media

[0275] First, a PET film with a thickness of 4.5 μm was prepared as a base layer. Next, a silicone resin having a solid content of 0.1 g / m2 per unit area was formed on the opposite side (back side) of the base layer on which the thermal transfer layer was formed.2 Next, any of the first thermal transfer layer coating agents prepared previously is applied to the surface of the substrate layer and then dried to form a solid content per unit area of ​​1.7 g / m 2 Next, any intermediate layer coating agent prepared previously was applied on the first thermal transfer layer and then dried to form an intermediate layer. Regarding the coating amount of the intermediate layer coating agent, in samples 16 to 29, the solid content per unit area was 1 g / m 2 , in samples 30 to 33, respectively, as shown in the following Table 10. Next, the second thermal transfer layer coating agent (I) prepared previously was applied on the intermediate layer and then dried to form a solid content per unit area of ​​2.5 g / m 2 The second thermal transfer layer was formed to produce a thermal transfer recording medium. The composition of each layer of the thermal transfer recording medium obtained from Samples 16 to 33 is shown in Tables 7 to 10 below. In the table, NF in the column of the adhesive of the intermediate layer means no flow.

[0276] (2) Evaluation

[0277] (2-1) Continuous Record Evaluation

[0278] The thermal transfer recording medium produced by each sample was cut into a strip of a predetermined width, wound into a roll, and installed in a thermal transfer printer (a prototype printer manufactured by Brother Industries, Ltd.). The main specifications of the thermal transfer printer are as follows.

[0279] <Resolution> 300dpi line thermal head

[0280] <Resistance of heating element> 1830Ω

[0281] <Transfer load> 30N / 2inch

[0282] <Transport speed> 20mm / sec

[0283] <Peeling distance> 110mm

[0284] Next, in an environment with an outside temperature of 25°C, the energy value pre-set in the thermal transfer printer and applied to the thermal head was set to low energy (0.25mJ / dot: 25V (0.34W / dot) / 750μsec, black) or high energy (0.34mJ / dot: 25V (0.34W / dot) / 1000μsec, red), and a 70mm square solid image was recorded 20 times continuously on the surface of the variable information printing label material [polyester film (white·smooth), FR1415-50 manufactured by LINTEC Co., Ltd.]. If some turbidity was observed in the middle of the recording, the continuous printing was terminated at that point, and the number of times the black or red was printed was recorded as the number of continuous printings. During the evaluation, it was considered that the sample that printed black even at the 20th time had excellent continuous printing performance of more than 20 times, and the sample that produced turbidity after the third time was not practical enough. The results are shown in Tables 7 to 10.

[0285] (2-2) Evaluation of the clarity of records

[0286] The thermal transfer recording medium produced by each sample was cut into a strip of a predetermined width and wound into a roll, and then installed in a thermal transfer printer (prototype printer manufactured by Brother Industries, Ltd.) of the same specification as (2-1). Next, in an environment with an outside temperature of 25°C, the energy value pre-set in the thermal transfer printer to be applied to the thermal head was set to low energy (0.25 mJ / dot: 25 V (0.34 W / dot) / 750 μsec, black) or high energy (0.34 mJ / dot: 25 V (0.34 W / dot) / 1000 μsec, red), and a bar code was recorded on the surface of a variable information printing label material (polyester film (white and smooth), FR1415-50 manufactured by LINTEC Co., Ltd.). The recorded barcode was then read using a barcode verification machine (Laser Examiner Elite IS manufactured by MUNAZOWO Co., Ltd.), and the decodability level specified in the American National Standards Institute standard ANSI X3.182-1990) was determined based on the reading result. The clarity of the record was evaluated according to the following criteria.

[0287] 0: Decodability level is A [Excellent] or B [Excellent] for both black and red.

[0288] △: For either black or red, the decodability level is C [Good], and the other is C [Good] or higher.

[0289] ×: For at least one of black and red, the decodability level is D [OK] or F [NOT].

[0290] The results are shown in Tables 7 to 10. It should be noted that among Samples 16 to 33, Samples 16 to 28 and Samples 30 to 33 may be Examples, and Sample 29 may be a Comparative Example.

[0291] (2-3) Observation of fracture position

[0292] The thermal transfer recording medium produced by each sample was cut into strips of a predetermined width and wound into a roll, and then installed in a thermal transfer printer (prototype printer manufactured by Brother Industries, Ltd.) with the same specifications as (2-1). Next, the energy values ​​pre-set in the thermal transfer printer to be applied to the thermal head were set to low energy (0.25 mJ / dot: 25 V (0.34 W / dot) / 750 μsec, reaching temperature T R1 : 80℃, black) and high energy (0.34mJ / dot: 25V (0.34W / dot) / 1000μsec, reaching temperature T R2 : 140°C, red), a solid image of 70 mm square was recorded on the surface of a variable information printing label material [polyester film (white and smooth), FR1415-50 manufactured by LINTEC Co., Ltd.]. In either case, the peeling distance of the thermal transfer printer was ensured to be 110 mm, so the peeling process was performed after being fully cooled (below 60°C). The cross-section of the obtained solid image was observed using a transmission electron microscope (TEM: HT7820 manufactured by Hitachi High-Tech Co., Ltd., accelerating voltage 100 kV). It was confirmed at which position of the thermal transfer recording medium the break occurred in each of the black transfer and the red transfer. The break position was distinguished according to the peeling mode as follows.

[0293] First peeling mode: between the substrate layer and the first thermal transfer layer (interface damage reference Fig.10 )

[0294] Second peeling mode: Inside the first thermal transfer layer (cohesive failure reference Fig.11 )

[0295] The third peeling mode: between the middle layer and the second thermal transfer layer (interface damage reference Fig.12 )

[0296] Fourth peeling mode: the inside of the second thermal transfer layer (cohesive failure reference Fig.13 )

[0297] Fifth peeling mode: inside the middle layer (cohesive failure Fig.14 )

[0298] The sixth peeling mode: between the mixed layer and the second thermal transfer layer (interface damage refers to Fig.15 )

[0299] The results are shown in Tables 7 to 10. In Tables 7 to 10, only the numbers enclosed in circles represent the first to sixth peeling modes, respectively. In addition, in Tables 7 to 10, when multiple peeling modes are shown, different peeling modes occur in the in-plane direction of the thermal transfer recording medium. In addition, since Sample 29 has a layer structure without an intermediate layer, the peeling modes in the lower part of Table 7 strictly speaking occur from Fig.13 as well as Fig.15 The cohesive failure and interface failure in the state of the intermediate layer 51 are omitted.

[0300]

Table 7

[0301]

[0302]

Table 8

[0303]

[0304]

Table 9

[0305]

[0306]

Table 10

[0307]

[0308] According to the comparison between samples 16 to 28 and sample 29 in Tables 7 to 9, for example, by referring to Fig.17 The balance of the SP values ​​of the constituent components of the first thermal transfer layer, the second thermal transfer layer, and the intermediate layer is adjusted to achieve a desired peeling pattern. As a result, it is known that a thermal transfer recording medium is obtained in which the color tone is not easily turbid and is clearly separated into two colors even when thermal transfer recording is performed continuously, and text with excellent clarity can be recorded without unnecessary peeling.

[0309] Comparison between Samples 16 to 27 and Sample 28 shows that, in order to further improve the continuous recording performance, it is preferable to use a thermoplastic elastomer as the intermediate layer.

[0310] Comparison between Sample 16 and Sample 26 shows that, as the epoxy resin forming the first thermal transfer layer, an epoxy resin having a softening point of 95° C. or higher is preferred, an epoxy resin having a softening point of 110° C. or higher is further preferred, and an epoxy resin having a softening point of 125° C. or higher is particularly preferred. Furthermore, comparison between Sample 16 and Sample 27 shows that, it is preferred to mix a tackifier with the epoxy resin forming the first thermal transfer layer together with the acrylic adhesive.

[0311] According to Sample 16 and Samples 30 to 33, even if the coating amount of the intermediate layer is changed, sufficient continuous recording performance and clarity can be achieved in practical use. It can be seen that among Sample 16 and Samples 30 to 33, Samples 16, 31 and 32 have particularly excellent continuous recording performance and clarity. Samples 16, 31 and 32 have the thinnest intermediate layer (less coating amount) among the layers constituting the thermal transfer recording medium, and the thickness (coating amount) of the intermediate layer can fully reflect the effect brought about by the introduction of the intermediate layer.

[0312] In other words, in sample 33, the middle layer of the layers constituting the thermal transfer recording medium is not the thinnest but relatively thick, so the transfer area (excess peeling) becomes larger and the clarity decreases. Generally, it is believed that if the thickness of the layer on the side close to the heat source increases as in sample 33, the reaching temperature at the interface between the layer on one side and the layer on the other side decreases, so the transfer area decreases. However, at the interface between the middle layer and the second thermal transfer layer, when the reaching temperature of the interface decreases, the (intermediate layer-second thermal transfer layer) Figure 6 The phenomenon that the adhesion between "51" and "52" is maintained low. As a result, it is believed that in the area around the barcode, the adhesion between the label material and the second thermal transfer layer ( Figure 6 Compared with the bonding force between "2" and "52"), the bonding force between the intermediate layer and the second thermal transfer layer is relatively low, and a break occurs between the intermediate layer and the second thermal transfer layer, and the excess peeling becomes larger.

[0313] On the other hand, in Sample 30, although the intermediate layer is the thinnest among the layers constituting the thermal transfer recording medium, the coating amount is 0.1 g / m 2 Such a small amount prevented the original function of the intermediate layer from being fully exerted, and it was confirmed that both the continuous recording performance and the clarity were reduced.

[0314] Description of Reference Numerals

[0315] 1 printing device; 2 printing ribbon; 3 ink ribbon; 6 thermal head; 20 heating element; 31 printing surface; 32 back surface; 35 substrate layer; 36 first ink layer; 37 second ink layer; 42 first part; 43 second part; 44 printing pattern; 45 red pattern; 46 black pattern; 47 thermal transfer recording medium; 48 substrate layer; 50 first thermal transfer layer; 51 intermediate layer; 52 second thermal transfer layer; 61 mixed layer; 62 first material; 63 second material; 64 third material; 65 fourth material; 66 fifth material; F1 external force; T1 first temperature; T2 second temperature; T3 third temperature; T R1 Reach temperature; T R2 Arrival temperature.

Claims

1. A thermal transfer recording medium, wherein: The thermal transfer recording medium comprises: a substrate layer having a first surface and a second surface; and A first thermal transfer layer, an intermediate layer and a second thermal transfer layer are sequentially stacked on the first surface of the substrate layer in direct contact with each other, The intermediate layer comprises a thermoplastic elastomer.

2. The thermal transfer recording medium according to claim 1, wherein The thermoplastic elastomer has a melt flow rate (MFR) of 1000 g / 10 min or less at a temperature of 190° C. and a load of 2.16 kg, as measured by the measurement method specified in ISO 1133-1:2011.

3. The thermal transfer recording medium according to claim 1 or 2, wherein: The thermoplastic elastomer includes at least one of a styrene-based thermoplastic elastomer and an acetate-based thermoplastic elastomer.

4. The thermal transfer recording medium according to claim 3, wherein The thermoplastic elastomer includes at least one selected from the group consisting of styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene·butylene-styrene block copolymer (SEBS), and ethylene-vinyl acetate copolymer (EVA).

5. The thermal transfer recording medium according to claim 3, wherein The thermoplastic elastomer includes a styrene-based thermoplastic elastomer, and the styrene-based thermoplastic elastomer contains styrene at a content of 10% by mass or more and 70% by mass or less.

6. The thermal transfer recording medium according to claim 1 or 2, wherein: The first thermal transfer layer contains epoxy resin and acrylic adhesive.

7. The thermal transfer recording medium according to claim 1 or 2, wherein: The second heat transfer layer includes thermoplastic resin and wax.

8. A thermal transfer recording medium, comprising a substrate layer, a first ink layer containing a first ink, an intermediate layer, and a second ink layer containing a second ink, which are sequentially stacked, and at least a portion of the first ink layer and the second ink layer are thermally transferred to a printed medium, wherein: In a first state where the thermal transfer recording medium is heated to a temperature not lower than a first temperature and not higher than a second temperature and then cooled to a temperature not higher than a third temperature, when an external force is applied to the substrate layer and the second ink layer in a direction away from each other, a rupture occurs between the first ink layer and the substrate layer or in the first ink layer, In the second state where the thermal transfer recording medium is heated to a temperature exceeding the second temperature and then cooled to a temperature not higher than the third temperature, when the external force is applied, rupture occurs between the first ink layer and the second ink layer or in the second ink layer.

9. The thermal transfer recording medium according to claim 8, wherein When the external force is applied in the first state, the breaking strength between the first ink layer and the base layer or within the first ink layer is the smallest in the thermal transfer recording medium. When the external force is applied in the second state, the breaking strength between the first ink layer and the second ink layer or within the second ink layer is minimum in the thermal transfer recording medium.

10. The thermal transfer recording medium according to claim 8 or 9, wherein: When the external force is applied in the second state, rupture occurs between the intermediate layer and the second ink layer.

11. The thermal transfer recording medium according to claim 10, wherein When the external force is applied in the second state, the breaking strength between the intermediate layer and the second ink layer is minimum in the thermal transfer recording medium.

12. The thermal transfer recording medium according to claim 10, wherein The intermediate layer includes a styrene-based thermoplastic elastomer.

13. The thermal transfer recording medium according to claim 12, wherein: The styrene-based thermoplastic elastomer includes at least one of a styrene-butadiene-styrene block copolymer (SBS) and a styrene-ethylene·butylene-styrene block copolymer (SEBS).

14. The thermal transfer recording medium according to claim 13, wherein The content of styrene in the styrene-based thermoplastic elastomer is 10% by mass to 70% by mass.

15. The thermal transfer recording medium according to claim 10, wherein The intermediate layer includes an acetate-based thermoplastic elastomer.

16. The thermal transfer recording medium according to claim 15, wherein The acetate-based thermoplastic elastomer includes ethylene-vinyl acetate copolymer (EVA).

17. The thermal transfer recording medium according to claim 10, wherein In the second state, the first ink layer is mixed with the intermediate layer.

18. The thermal transfer recording medium according to claim 8 or 9, wherein: When the external force is applied in the second state, fracture occurs in the intermediate layer.

19. The thermal transfer recording medium according to claim 18, wherein When the external force is applied in the second state, the breaking strength in the intermediate layer is minimum in the thermal transfer recording medium.

20. The thermal transfer recording medium according to claim 18, wherein The intermediate layer contains at least one of a polyolefin-based resin and a long-chain alkyl-based resin.

21. The thermal transfer recording medium according to claim 8 or 9, wherein: The first ink layer includes at least a first material and a second material having a solubility parameter (SP value) higher than that of the first material. The intermediate layer comprises at least a third material, The second ink layer includes at least a fourth material and a fifth material having a solubility parameter (SP value) lower than that of the fourth material.

22. The thermal transfer recording medium according to claim 8 or 9, wherein: The first temperature is equal to or higher than the third temperature.

23. The thermal transfer recording medium according to claim 8 or 9, wherein: The first state is a state in which the base material layer of the thermal transfer recording medium is heated to a temperature higher than the first temperature and lower than the second temperature and then cooled to a temperature lower than the third temperature. The second state is a state in which the base material layer of the thermal transfer recording medium is heated to a temperature exceeding the second temperature and then cooled to a temperature not higher than the third temperature.

24. The thermal transfer recording medium according to claim 1 or 8, wherein: Among the layers constituting the thermal transfer recording medium, the intermediate layer is the thinnest.

25. A printing device, wherein: The printing device performs the following steps: A heating step of heating the thermal transfer recording medium in a state where the thermal transfer recording medium, which is formed by sequentially stacking a base layer, a first ink layer containing a first ink, an intermediate layer, and a second ink layer containing a second ink, is in contact with a medium to be printed; a cooling step of cooling the thermal transfer recording medium heated by the heating step; as well as a transfer step of applying an external force in a direction away from each other to the base layer and the second ink layer of the thermal transfer recording medium cooled by the cooling step, thereby transferring at least a portion of the first ink and the second ink to the printed medium; In the heating step and the cooling step, The first portion of the thermal transfer recording medium is heated to a temperature higher than a first temperature and lower than a second temperature and then cooled to a third temperature or lower to form a first state, and the second portion of the thermal transfer recording medium is heated to a temperature higher than the second temperature and then cooled to a temperature lower than the third temperature to form a second state, In the transfer process, By applying the external force, the thermal transfer recording medium is broken at the first portion of the thermal transfer recording medium, between the first ink layer and the base layer or within the first ink layer, and the first ink and the second ink are transferred to the printed medium. By applying the external force, the thermal transfer recording medium is broken at the second portion of the thermal transfer recording medium between the first ink layer and the second ink layer or within the second ink layer, and the second ink is transferred to the printing medium.

26. A box, wherein The box contains: The thermal transfer recording medium according to claim 1 or 8; and A printed medium to which a portion of the thermal transfer recording medium is thermally transferred.