Starch extrusion and papermaking method
Through extruded starch technology, the dry strength and mechanical properties of paper are improved in the papermaking process, the problems of low solubility of traditional starch and microbial corruption are solved, and the production of high-quality paper is achieved.
Patent Information
- Application Number
- CN202380032870.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-10
- Filing Date
- 2023-04-05
- Publication Date
- 2024-11-15
AI Technical Summary
In traditional papermaking processes, starch has low solubility in the production process, high risk of microbial corruption, and insufficient dry strength of paper, making it difficult to meet the mechanical properties of modern paper products.
Using extruded starch technology, the starch is mechanically processed in a twin-screw extruder to generate high solubility and modified starch, which increases the mechanical properties of the paper during the drying process, and improves the paper by adding cationic starch and enzyme modification treatment. strength.
It significantly improves the dry strength and mechanical properties of paper, reduces the risk of microbial corruption, improves the tensile strength and compression resistance of paper, and is suitable for the production of high-quality paper products.
Smart Images

Figure CN118974352A_ABST
Abstract
Description
[0001] Related applications
[0002] This application claims priority to and the benefit of U.S. Provisional Patent Application No. 63 / 329,114, filed on April 8, 2022, for "Production of Paper and Paperboard," and U.S. Provisional Patent Application No. 63 / 351,149, filed on June 10, 2022, for "Extrusion Starch and Papermaking Process," the contents of both of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to paper (including tissue, towels, card and board) and papermaking processes, starch-derived materials, and the use of starch-derived materials in paper production, for example as dry strength agents. Background Art
[0004] The following paragraphs are not an admission that anything discussed therein is prior art or part of the knowledge of a person skilled in the art.
[0005] Paper is typically made on a paper machine in a largely continuous process. Many modern paper machines are descended from older paper machines, such as the Fourdrinier machine developed in the early 19th century. A typical Fourdrinier machine has at least a forming section, a press section, and a drying section. Pulp is made by combining fibers (also called fiber slurry) with other materials (such as fillers), optionally refined or otherwise physically or chemically treated, and transferred to the paper machine's header tank (also called a headbox or blender box). From the paper machine's header tank, the slurry is transferred to the headbox and, from there, to a wire (usually a moving wire ring) in the forming section. Water from the slurry is filtered through the wire, typically with the aid of suction, to form a continuous sheet, also called a web. The sheet enters the press section, where more water is removed by pressing the sheet against absorbent felts. The pressed sheet then enters the drying section, where it is thermally dried, for example, by a series of steam-heated cylinders. In some examples, these sections are followed by one or more of the following: a size press, a calender, and a coating section. The reel section at the end of the machine winds the paper onto reels for storage, transport, or further processing. Other machines, such as cylinder paper machines or tissue paper machines, use different arrangements or designs of machine sections to accomplish similar steps. Paper can be formed into various thicknesses (i.e., 0.07-0.18 mm) or weights (i.e., 15-300 g / m 2 or 30-300g / m 2 ), optionally from lightweight or thin paper to ordinary multipurpose or printing paper (optionally 60-120g / m 2 ), then to the card (optionally 135g / m 2 or larger) or cardboard (optionally 250g / m 2 or larger), can be single-layer or multi-layer, and have various surface features or other properties.
[0006] In some cases, starch is added to paper pulp, for example as a dry strength agent. Traditionally, native starch granules are cooked in water at the papermaking site to form a dissolved starch solution before use. The most typical method for dissolving starch granules is jet cooking, in which an aqueous starch slurry is contacted with steam at a temperature of approximately 120-130°C and dissolved in a tube in a process that takes about 1-2 minutes. After the starch is dissolved, it is typically diluted to a solids content of less than 1% before adding it to the papermaking slurry to ensure uniform mixing with the paper pulp. The dissolved starch is used immediately after production to avoid microbial spoilage or retrogradation.
[0007] In other examples, a pregelatinized starch slurry or dry cold water-soluble starch is mixed with water and added to the papermaking slurry. For example, cold water-soluble starch can be prepared by the method described in U.S. Patent 5,037,929. Alternatively, Tate & Lyle's STA-LOK™ 280 contains pretreated cationic waxy corn starch and is provided as a 30% solids slurry. In other examples, a dispersion of regenerated starch particles can be used, such as described in European Patent Publication No. 1,176,254. Summary of the Invention
[0008] The following description is intended to introduce the reader to the present disclosure but does not define any invention. One or more inventions may reside in any combination or subcombination of the features described below, or elsewhere in the specification. The inventors do not waive or disclaim their rights to any one or more inventions disclosed in the specification simply because they do not recite such other one or more inventions in the claims.
[0009] This specification describes a papermaking method. The method includes providing a pulp, optionally referred to as pulp for simplicity, comprising a fibrous material, such as a fiber slurry, water, optionally one or more inorganic fillers, and extruded starch. Optionally, the pulp may have one or more additives or auxiliaries. The pulp is formed into a paper web. The paper web is pressed to at least a minimum solids content and dried. The minimum solids content (weight percentage) is 46+(x-10)*0.3, where x is the ash content of the dried paper. The extruded starch optionally has one or more properties. In some examples, the extruded starch is cationic. In some examples, the starch is chemically or enzymatically modified in the extruder, for example, the starch can be acid-lyzed. In some examples, the extruded starch is not cross-linked. In some instances, the solubility of the extruded starch is 40-99%, or 40-93%, or 40-92%, or less than 92%, for example, as determined by the amount of rapidly soluble starch (RSS). In some examples, the molecular weight of the extruded starch exceeds 300,000 Da. In some examples, the weight fraction of the extruded starch that exceeds 30,000,000 Da is 0.05 or less. In some examples, the extruded starch has an RVA viscosity of 15,000 cP or less at 20% S (solids content).
[0010] This specification also describes a composition comprising extruded starch. In some examples, the extruded starch is cationic. In some examples, the extruded starch is not cross-linked. In some examples, the solubility of the extruded starch is 40-99% or 40-93%. In some examples, the molecular weight of the extruded starch is 300,000 Da or greater, 500,000 Da or greater, 2,000,000 Da or greater, or 4,000,000 Da or greater. In some examples, the weight fraction of the extruded starch exceeding 30,000,000 Da is 0.05 or less. In some examples, the RVA viscosity of the extruded starch at 20% S (solids content) is 15,000 cP or less, or 5,000 cP or less.
[0011] This specification also describes a method for preparing a composition comprising extruded starch. Feed starch or starch-containing material is extruded together with water. Optionally, one or more processing aids, polyols, wetting agents or plasticizers (i.e., glycerol) can be added during or after the extrusion process. Optionally, starch is acidified or enzyme-modified during the extrusion process. Extrusion can be carried out in a twin-screw extruder, which optionally has one or more mixing and / or high shear sections. Optionally, the feed starch can be cationic, or starch can be cationized in the extruder.
[0012] In at least some examples, extruding starch and / or the methods described for making paper using extruded starch results in a final paper having a higher dry strength than paper made using conventional starch. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The dependence of the Short Span Compression Test (SCT) results on the cationic charge level of selected press sheets including starch samples Blank, 1, 15 and 16 at 5 kg / t and 10 kg / t is depicted in graphical form.
[0014] Figure 2 The dependence of the Short Span Compression Test (SCT) results on the molecular weight of selected press sheets, including starch samples 1, 10-11 at 5 kg / t and 10 kg / t, is depicted in graphical form.
[0015] Figure 3 The dependence of the short span compression test (SCT) results on the cross-linking of selected press sheets, including starch samples 1, 3, 12, 13 at 5 kg / t and 10 kg / t, is depicted in graphical form.
[0016] Figure 4 The dependence of the burst test results on the cross-linking of selected press sheets, including starch samples 1, 3, 12, 13 at 5 kg / t and 10 kg / t, is depicted in graphical form.
[0017] Figure 5 The dependence of the Short Span Compression Test (SCT) results on the dry solids content (low DC, high DC) of selected press sheets including starch samples 1, 17, 18 at 5 and 10 kg / t is depicted in graphical form. DETAILED DESCRIPTION
[0018] As used in this specification and claims, the singular forms "a," "an," and "the" include plural referents unless the context dictates otherwise.
[0019] In a papermaking process, starch is optionally added to the slurry, for example upstream of or in the wet end, before, together with, or after the addition of fillers or additives. In some examples, starch is added to the fibrous material before any other additives or fillers are added. Starch can be added to either a thick or thin slurry. The addition of starch increases the strength of the final paper product. The starch can be, for example, regenerated starch granules. Starch regeneration refers to the destruction of the crystal structure of a native starch granule and the creation of a new granular structure. Each starch granule contains a plurality of starch molecules, which may optionally be cross-linked. For example, starch granules can be produced as described in, for example, European Patent Publication No. 1176254, which is incorporated herein by reference. In other examples, the starch is thermomechanically processed starch, in which the crystal structure of the native starch granule is destroyed, but a new supramolecular structure is not necessarily created, or different starch molecules may be present in combination with the supramolecular starch structure. Starch granules and other forms of thermomechanically processed starch can be produced in an extruder, and for brevity, the term "extruded starch" may be used herein to refer to them. However, other processes can also be used to produce similar materials. For example, some high shear static mixers can be used to generate similar mechanical energy. In contrast, some extruders generate very low mechanical energy and rely more on heat to cook the starch, which may not produce similar materials. Extruders that generate large amounts of mechanical energy include, for example, twin-screw co-rotating extruders.
[0020] As mentioned above, in some examples, extruded starch is not completely soluble. However, the insoluble structure can be very small, for example, 10-1000nm or 50-500nm, and mechanically behaves like a solution, although they may be more accurately described as a dispersion. In some examples, the mixture of extruded starch in water can include some dissolved starch molecules and some dispersed large starch molecules, supramolecular structures or particles. The terms "dispersion" or "solution" can be used herein to describe the mixture of extruded starch in water, but these two words are not used according to strict technical definitions.
[0021] In some examples, the extruded starch contains 99% or less, or 93% or less, or 92% or less rapidly soluble starch (RSS). A rapidly soluble starch is a starch that behaves to some extent as if it were in solution when mixed in room temperature water, whether or not it actually dissolves. RSS is determined by adding 4 g of dry extruded starch to 200 ml of deionized water; stirring at 600 RPM for 2 minutes; centrifuging at 3000 RPM for 15 minutes; removing 100 ml of supernatant by decantation or pipetting; drying the supernatant in an oven at 110°C; and measuring the remaining dry mass, which represents the mass of starch in the supernatant. The dry mass is divided by 2 g and converted to a percentage to determine the RSS. In an example described further below, an RSS of 92% was achieved in a twin-screw extruder without chemical or enzymatic modification of the starch. In another example, a starch with an RSS of 97% was chemically modified with acid in the extruder. The amount of acid used was less than the amount of acid used to produce the acid-hydrolyzed starch outside the extruder. It is contemplated that enzyme treatment in an extruder may alternatively or additionally be used to produce starches with RSS as high as 97% or 99%. The RSS of cross-linked starches produced in an extruder tends to be much lower. However, an RSS of 40 or higher may optionally be achieved by cross-linking.
[0022] As described below, the addition of extruded starch to the slurry can result in a finished paper having greater strength or other mechanical properties than paper made using conventionally cooked starch. Mechanical or other properties can be further improved by selecting an extruded starch having one or more optional properties. For example, the extruded starch is optionally not cross-linked. The RSS of the extruded starch is optionally 40-97% or 40-93%. The molecular weight of the extruded starch is optionally greater than 300,000 Da or greater, 500,000 Da or greater, 2,000,000 Da or greater, 4,000,000 Da or greater, or 5,000,000 Da or greater. The weight fraction of the extruded starch exceeding 30,000,000 Da is optionally 0.05 or less. The RVA viscosity of the extruded starch at 20% solids is optionally 15,000 cP or less, or 10,000 cP or less, or 5,000 cP or less. The extruded starch is optionally cationic. Cationicity is optionally measured as a percentage of nitrogen associated with the starch (excluding protein nitrogen) and ranges from about 0.1-1.6% or 0.1-0.8%.
[0023] Further improvements in mechanical properties can be achieved through manipulation of other steps in the papermaking process. As the papermaking process continues, the paper web or sheet formed from the slurry is pressed. In Fourdrinier papermaking machines, the paper web is transferred from the forming section to various press sections. In other papermaking machines, the web forming and pressing may be at least partially integrated, or other arrangements of similar machinery may be used. The paper web comprises fibrous material, extruded starch, optionally one or more inorganic fillers, and optionally one or more other additives. Typically, the pressed paper web is further dried in a thermal drying process.
[0024] The inventors have determined that pressing or otherwise dewatering a paper web to at least a minimum solids content can improve the strength or other mechanical properties of the final paper, particularly when extruded starch is present in the paper web. The minimum solids content may vary depending on the amount of inorganic filler also present in the paper web. In some examples, the slurry is pressed to a minimum solids content as defined by formula (I).
[0025] D(x)=46+(x-10)*0.3(I)
[0026] Where D(x) is the minimum solids content (weight %) of the finished paper, and (x) is the ash content (weight %). The minimum solids content refers to the solids content of the paper sheet after pressing and can be determined using the oven drying method of ISO 638:2008. The ash content x can be measured according to ISO 1762:2019. The ash content of the finished paper is related to the amount of inorganic filler added to the pulp.
[0027] In some examples, extruded starch is made by adding one or more starch-containing feeds (e.g., native starch or flour) to an extruder. Water is also added to the extruder. Optionally, processing aids, polyols, humectants, or plasticizers (e.g., glycerol) can be added to the extruder. When added to the extruder, the processing aids, polyols, humectants, or plasticizers can be added upstream or downstream of the mechanical processing area, where most of the mechanical work on the feed is performed. In other options, processing aids, polyols, humectants, or plasticizers (if any) can be added to the extrudate after extrusion. One or more starch-containing feeds preferably account for 80% or more of the solids (i.e., all materials except water) added to the extruder.
[0028] Mechanical energy can be used to process starch. Mechanical energy can be transferred to starch using a high shear mixer, a single screw extruder (under certain conditions) or a twin screw extruder having co-rotating or counter-rotating screws. A preferred extruder has two co-rotating screws. The extruder can have several, i.e. 5 or more, or 7 or more barrels. The extruder preferably includes one or more mixing and / or high shear sections. The mixing and / or high shear section can have reverse kneading elements, or forward and reverse kneading elements. The extruder or other high shear mixer can apply a specific mechanical energy (specific mechanical energy) of 100Wh or greater, or 150Wh or greater, or within the range of 175-300Wh to each kilogram of starch-containing feed. The extruder is preferably operated at a temperature lower than 180°C to reduce or avoid the presence of short-chain molecules (DP<6) in the extruded product. The maximum barrel temperature (temperature in the hottest barrel) in the extruder can be lower than 180°C, or 160°C or lower, or 120 to 160°C. The extruder may be as described in US Pat. No. 9,011,741, "Process for Producing Biopolymer Nanoparticles," which is incorporated herein by reference.
[0029] Starch is contained in the feed.The feed can be a single type of native starch, or flour, or any combination of different types of starch, or a combination of starch and flour.In some examples, starch is not acid-decomposed substantially, but a small amount of acid can be added as a processing aid. Optionally, based on solid relative to feed, the addition of weak acid (pKa is 1 or larger) (if any) can be less than 1 weight % or less than 0.5 weight %. Optionally, based on solid relative to feed, the addition of strong acid (if any) can be less than 0.7 weight %, less than 0.5 weight % or less than 0.0001 weight %. Optionally, based on solid relative to feed, the addition of one or more enzymes (if any) can be less than 10%.The molecular weight of product can be at least 300000, at least 500000, at least 2 million, at least 3 million, at least 4 million or at least 5 million Da.In some examples, the polydispersity index (Mw / Mn) of extruded product is less than 2. The extruded product consists primarily (ie, 80% or more by dry weight) of one or more of the following: starch, protein, or other materials found naturally in starch or flour, or derivatives thereof.
[0030] Some examples of extruded starch prepared as described above were compared with commercially available pregelatinized starch. According to the above method, three feeds were used to prepare novel extruded starch products. The maximum barrel temperature was 120 to 160°C. The SME was 175-300Wh / kg of starch-containing feed. In sample A, the feed was dent corn starch. In sample B, the feed was corn flour. In sample C, the feed was waxy corn starch. The extruder was as described in U.S. Patent 9,011,741. The feed was introduced into the extruder together with glycerol (5 parts glycerol, 95 parts starch or flour, by weight) and water, but without a crosslinking agent or acid.
[0031] For comparison, a sample of Bunge PCF 1000, a commercially available pregelatinized corn flour, was tested. This product is made by processing corn flour in a single-screw extruder. While an extruder may be involved in preparing the pregelatinized starch, single-screw extruders are typically configured to provide low specific mechanical energy (SME) and to provide a thermal rather than a mechanical process. Extruders are used to provide a plug flow process to cook the starch rather than mechanically processing it. The SME in a single-screw extruder is typically well below 100 Wh / kg. In at least some cases, commercially available pregelatinized starches are also processed at very high temperatures, such as 180°C or higher. At high temperatures, more short-chain molecules can be produced.
[0032] Various samples were tested in dimethyl sulfoxide (DMSO) by gel permeation chromatography (GPC) to determine their molecular weight and molecular weight distribution. Gel permeation chromatography was performed using a Malvern Viscotek GPCmax equipped with a Malvern Viscotek TDA (triple detector assembly). The Viscotek TDA was equipped with refractive index (RI), intrinsic viscosity, and light scattering (LALLS, RALLS) detectors. For separation, a Polyanalytik (London, Ontario, Canada) PAA-206M size exclusion chromatography column was used, measuring 8 x 300 mm and filled with a polyhydroxymethacrylate-based gel with an estimated exclusion limit of 2 x 107 g / mol. Pullulan 50K (No. PATD-PUL50K, Mw: 46001 g / mol, PDI: 1.069) was used for calibration and confirmed with PolyCAL™ dextran Std-T73K (Mw: 71747 g / mol, Mn=53956 g / mol); both were purchased from Polyanalytik (London, Ontario, Canada). All samples were analyzed under the following experimental conditions: flow rate 0.6 ml / min; column temperature 70°C; mobile phase, DMSO (>99.9%) from Anachemia (Montreal, Quebec, Canada) and 0.05 M LiBr (99+%) from Sigma-Aldrich (Oakville, Ontario, Canada); sample concentration 2-3 mg / ml; injection volume 100 μl; number of replicates 4. Samples were diluted and filtered through a 0.2 μm filter before entering the GPC column. The results are shown in Table 1 below. "% Recovery" refers to the percentage of solids in the sample that passed through a 0.2 micron filter.
[0033] Table 1: GPC analysis results of various starch samples
[0034] sample Recovery rate (%) MW(Da) PCF 1000 70 <![CDATA[4*10 6 ]]> A 93 <![CDATA[6*10 6 ]]> B 78 <![CDATA[5*10 6 ]]> C 100 <![CDATA[6*10 6 ]]>
[0035] The molecular weight (MW) graphs of all samples show a peak molecular weight (peak MW) at 4*10 6 -6*10 6 However, the PCF 1000 sample has a lower peak in this range, as well as a 6 -2*10 6 The tail of the PCF 1000 distribution extends to 4*10 7 The molecular weight fraction (WF / dLogMW, where WF represents weight fraction and dLogMW represents the logarithm of molecular weight Mw) is 3*10 7 Da is 0.1. In contrast, samples A, B and C are7 The molecular weight fraction is 0.025 or less. In contrast, the molecular weight of commercially available acid-hydrolyzed starch is usually less than 2*10 6 .
[0036] The viscosity of the sample was tested using a Rapid Visco Analyzer (RVA, Perten Instruments) using the following operating procedure. The sample and analyte solution were dispensed into a new cartridge at a concentration of 20% solids, i.e., 7.0 g of dry product was added to the cartridge and the analyte was added to a total mass of 35.0 g. The sample weight was determined by correcting the sample moisture content to obtain a consistent dry weight. A new paddle was placed into the cartridge. The sample was pre-homogenized to ensure that any sample clumps adhering to the cartridge were transferred to the water and then immediately inserted into the RVA machine to begin the measurement. The analyte solution consisted of 16.0 g of sodium carbonate (Na2CO3) or 18.7 g of sodium carbonate monohydrate (Na2CO3·H2O) added and dissolved in 2 kg of demineralized water, and 0.4 ml of Acticide GA biocide (Thor Chemicals) was added. The RVA is designed to measure the viscosity profile of samples that have undergone thermal cycling. Thermal cycling causes the product to dissolve, accompanied by an increase in the viscosity of the sample. The behavior of viscosity as a function of temperature is characteristic of the material, and the measured value is a function of the temperature program. The procedure used is as follows:
[0037]
[0038] The output of the RVA is a viscosity-time curve. The RVA result for each sample is recorded as the final viscosity. This output depends on many factors, including starch type, amylose content, molecular weight, and molecular weight distribution. The results generated using the sample preparation method and RVA analysis protocol described above are shown in Table 2 below. cP stands for centipoise, a unit of measurement for viscosity.
[0039] Table 2: RVA analysis of various starch samples
[0040] sample RVA final viscosity (cP) PCF 1000 <![CDATA[23*10 3 ]]> A <![CDATA[7*10 3 ]]> B <![CDATA[7*10 3 ]]> C <![CDATA[1*10 3 ]]>
[0041] The viscosity of starch dispersions is influenced by the starch's botanical origin, as well as its molecular weight, and other factors. For example, dent corn starch retrogrades more readily in water than waxy corn starch. Starch retrogradation is a combination of recrystallization and hydrogen bonding, or gelatinization, typically accompanied by a series of physical changes, such as increased viscosity and turbidity of the retrograded starch solution. More specifically, for non-waxy starches, retrogradation results in the conversion of the starch paste into a firm gel composed of a three-dimensional network. Retrogradation may result in Sample A having a much higher viscosity than Sample C. Extruded starches made with waxy corn starch exhibited significantly lower viscosities than extruded starches made with other feed slurries.
[0042] To compare samples of similar plant origin, PCF 1000 and Sample B were both made from corn flour. As shown in Table 2, despite the similar feedstock of Sample B and PCF 1000, its viscosity was much lower than that of PCF 1000. The inventors believe that the reduced viscosity of Sample B is due to the fact that Sample B is an extruded starch product as described herein, rather than a traditional pregelatinized starch. Without intending to be limited or bound by theory, the narrower MW distribution of Sample B relative to PCF 1000 (higher peak above 1.5 WF / dLogM in the molecular weight distribution plot) and the relative lack of a high molecular weight tail of PCF 1000 (i.e., a relative lack of MW greater than 3*10 in Sample B) contribute to the reduced viscosity of Sample B. 7 One or both of the molecular weight of Da) may be influencing factors.
[0043] Very high molecular weight starches will adhere to the fiber surface but, due to their large size, are more likely to desorb over time. Starches of very low molecular weight cannot bridge the fibers and cannot provide strength. Preferred molecular weights (unless otherwise stated, referring to the weight average molecular weight, also known as Mw, typically near the peak of the WF / dLog MW plot of the Log MW graph) can be 2,000,000 Da or greater, or 4,000,000 Da or greater; optionally, up to 12,000,000 Da, up to 10,000,000 Da or up to 8,000,000 Da. Jet cookers tend to produce starches of very high molecular weight, for example 27,000,000 to 390,000,000 Da for starches produced at 140°C-110°C, at least some of which may desorb from the pulp fibers during papermaking and not contribute to paper strength. Acid hydrolyzed and oxidized starch produced without the use of an extruder (compared to using small amounts of acid or enzymes as processing aids when making extruded starch) can have a lower molecular weight, but random chain scission tends to produce a large portion of very low molecular weight starch that does not contribute to paper strength. Extrusion preferentially breaks down starch molecules above a critical molecular weight, which is inversely related to the shear stress (i.e., specific mechanical energy or SME) applied by the extruder, and the possibility of further degradation of starch molecules below the critical molecular weight is minimized. For example, the cationic starch used in Example 1C below has a Mw of about 4,000,000 Da, with a weight fraction below 1,000,000 Da of 0%, a weight fraction above 10,000,000 Da of about 10%, and a weight fraction above about 25,000,000 Da of 0%. Other extruded starches may have a weight fraction below 1,000,000 Da of 0-8% or 0-1%, or a weight fraction below 100,000 Da in the range of 0-8% or 0-1%. In contrast, acid hydrolysis, oxidation, and enzyme treatment randomly break down starch molecules, resulting in some starch molecules with very low molecular weight. Starch that does not adhere to the fibers does not add strength to the paper and also increases the biological oxygen demand (BOD) of the wastewater generated during the papermaking process.
[0044] Typically, extruded starch is added to the slurry upstream of the papermaking machine. Alternatively, it can be added to the slurry in the papermaking machine, but upstream of the press section or similar section or device. The slurry can comprise a mixture of fibrous material, extruded starch, optionally one or more inorganic fillers, optionally paper auxiliaries or other additives, and water.
[0045] In some examples, a slurry is prepared by adding extruded starch to an aqueous suspension of fibrous material. The preparation of the slurry may include multiple steps, wherein the solids content of the slurry varies. For example, the thick stock may contain fibrous material at a concentration of approximately 0.5-40 g / L, 10-40 g / L, or 20-40 g / L. The thin stock may contain fibrous material at a concentration of approximately 0.5 g / L to approximately 15 g / L. In some examples, the extruded starch is added to the thick stock, or the extruded starch may be added to the thin stock. For example, paper pulp may be prepared by adding extruded starch to a thick stock having a fibrous material concentration of approximately 20 to approximately 40 g / L. Before the thick stock is transferred to the wet end, it is diluted to a fibrous material concentration of approximately 0.5 to approximately 15 g / L. In some examples, the extruded starch is added to the aqueous suspension of fibrous material before any fillers or additives are added.
[0046] The slurry may comprise extruded starch at a concentration of about 0.05% to about 5% by weight solids. The slurry may comprise about 0% to about 40% by weight of an inorganic filler (hereinafter referred to as x), expressed as ash content. The slurry may optionally comprise one or more other additives (also referred to as paper aids).
[0047] The fibrous material in the slurry can include virgin fiber, recycled fiber, softwood fiber, hardwood fiber, non-wood fiber or its combination. The fibrous material can include dried commodity pulp, paper machine broke, recycled fiber or its combination. Any softwood or hardwood fiber commonly used in the paper industry can be used for the fibrous material. For example, the fibrous material can include mechanical pulp, bleached and unbleached chemical pulp and / or fibrous material (also referred to as non-wood fiber material) from any annual plant.
[0048] If the fiber material comprises bleached and / or unbleached chemical pulp, the fiber material may have a pulp filterability of 20 to 30 SR. Pulp filterability can be measured in SR units (standing for Schopper Riegler units) according to ISO 5267-1:1999. A fiber material with a filterability of approximately 30 SR can be achieved by refining during pulping. The fiber material may have a filterability of 30 SR or less.
[0049] Extruded starch can be added to the slurry in the form of a powder, dispersion or mixture. Extruded starch preferably has a cationic charge, but can also have an anionic charge, a zwitterionic charge or a neutral charge. Extruded starch can include one or more chemical or enzymatic modifications. In some examples, cationic starch is used. Extruded starch can include corn starch, wheat starch, rice starch, pea starch, potato starch, tapioca starch, barley starch and all variants or cultivars, such as waxy corn starch or a combination thereof. Extruded starch can include a mixture of starch and a biopolymer, wherein the starch is optionally present in a weight % of at least 50% or 80%, and the biopolymer is optionally other polysaccharides, such as cellulose or glue, proteins, such as soy protein or gelatin or whey protein, or a combination thereof.
[0050] Extruded starch can be dried after leaving forcing machine, forms dry starch extrudate.Dry starch extrudate can be pulverized and / or ground to form extruded starch powder.Pulling and / or grinding of dry starch extrudate can comprise with hammer mill fragmentation and / or grind by cryogenic grinding process.
[0051] Optionally, the extruded starch powder is added to water to form a dispersion of extruded starch.The dispersion of extruded starch may have a solids content of about 0.1 wt % to about 50 wt % or about 1 wt % to about 10 wt %.
[0052] The amount of inorganic filler (ash content) added to the slurry can be adjusted according to any inorganic filler (ash content) that may already be present, for example due to the use of waste paper and / or coating scraps as a source of fibrous material. The inorganic filler can be an inorganic pigment, such as a metal oxide, carbonate, silicate, or a combination thereof. The inorganic filler can include calcium carbonate, talc, kaolin, bentonite, satin white, calcium sulfate, barium sulfate, titanium dioxide, ground lime, chalk, marble (GCC), precipitated calcium carbonate (PCC), or a combination thereof.
[0053] Optionally, after the extruded starch is added, an inorganic filler can be added to the slurry. The filler can be added at a stage when the slurry is in a thick slurry form (e.g., a fiber concentration of 0.5-40 g / L, 10-40 g / L, or 20-40 g / L). The filler can be added at a stage when the slurry is in a thin slurry form (e.g., a fiber concentration of 5 to 15 g / L). The filler can be added at two stages, when the slurry is a thick slurry and a thin slurry, wherein the ratio of thick slurry addition to thin slurry addition is about 5 / 1 to about 1 / 5.
[0054] The filler content (x) of formula (I) expressed as the ash content of the paper may be from about 0 wt % to about 40 wt %, or from about 0 wt % to about 20 wt %, based on the total dry weight of the finished paper.
[0055] The paper aids may include sizing agents, wet strength agents, retention aids, drainage aids, dry strength enhancers, fluorescent brighteners, defoamers, biocides, paper dyes, or combinations thereof. The paper aids may be added to the slurry when the fibrous material concentration of the slurry is about 5 g / L to about 15 g / L.
[0056] The extruded starch may be added in an amount of about 0.5 kg to about 50 kg, for example, about 0.6 kg to about 20 kg, of at least one extruded starch per metric ton of dry fibrous material. The amount of extruded starch added may be about 0.05% to about 5% by weight based on the dry weight of the fibrous material. The extruded starch may be applied to the slurry for a period of time from about 0.5 seconds to about 2 hours, or any time range from about 0.5 seconds to about 2 hours, from the time of addition to the sheet forming step. Preferably, the time range may be about 2 seconds to about 20 seconds.
[0057] The process can include slurry treatment (e.g., thick stock and thin stock) in the wet end of the papermaking process. The treatment of slurry with extruded starch can begin early in the papermaking process, during pulp preparation, where dry commercial pulp, paper machine broke, or recycled fiber material (such as OCC) can be reslushed before passing through other devices (such as deflakers and / or refiners). Thus, extruded starch can be reslushed with the dry fiber material in the pulper, or it can be added to the deflaker and / or refiner unit. The added extruded starch can be in the form of a dry powder or in the form of a liquid dispersion.
[0058] After leaving the press section, the solids content of a paper web can be as high as or exceeding 55% by weight, depending on the design and operation of the forming section, the design and operation of the press section, the web speed, the type and age of the felt used, and the composition and temperature of the slurry. As the web passes through the press section, its solids content increases with the pressure applied by the press section. The pressure, and thus the solids content of the web, can vary within a relatively wide range among different papermaking machines.
[0059] After leaving the press section, the paper web can be transferred to the dryer section of the paper machine. For graphic or packaging paper grades, the web can be transferred to a series of drying cylinders, where the solids content of the web can gradually increase from one drying cylinder to the next. For tissue and hygiene papers, the sheet can be transferred to a Yankee dryer, where it can undergo final drying and creping. The final dry content of the finished paper can be around 95% by weight.
[0060] Cationic extruded starch can be used as a dry strength agent, for example to improve one or more mechanical properties of paper, such as tensile strength, burst strength, short span compressive strength, and Scott bond strength. Cationic extruded starch can also be used to increase production speeds to avoid paper breaks that cause production line downtime. In addition, cationic extruded starch can be used to maintain strength at an appropriate level while making other changes that reduce cost or energy consumption but generally reduce strength. For example, reducing the basis weight of the paper; using shorter fibers; using mechanically treated, recycled, or non-wood fibers with lower performance; reducing the level of fiber refining; and increasing the ash content may all be desirable changes, but generally reduce paper strength. The addition of cationic extruded starch can offset (i.e., reduce or eliminate) the strength loss caused by one or more of the above changes.
[0061] In order to better understand the invention described herein, the following examples are given. It should be understood that these examples are for illustrative purposes only. Therefore, they should not limit the scope of the invention in any way. In these examples, the inventors have demonstrated that for a range of final paper weights, paper strength is improved compared to paper made with conventional starch and / or with a solids content lower than D(x). In Example 1B, a 100 g / m² weight was selected for consistency between samples. 2 However, starch similar to Starch Sample 1 was made on a commercial scale twin screw extruder using the same starting material (cationic waxy corn starch) and specific mechanical energy (SME), which was subsequently tested on commercial scale tissue, fourdrinier, and linerboard machines to produce final paper weights ranging from 16 to 205 g / m 2 , some of which are described in Example 1C. It is expected that starch sample 1 and other samples described below will be 2 ) will produce similar results. The samples described below are not numbered consecutively because other samples were produced according to the protocol described below but were not tested.
[0062] Example
[0063] Example 1A - Preparation and Characterization of Extruded Starch Products and Reference Samples
[0064] Starch sample 1
[0065] 100 parts by weight of cationic waxy corn starch ( 180, purchased from Tate & Lyle) was fed into a Buhler twin-screw extruder at a rate of 300 kg / h and a screw speed of 600 RPM. 15 parts by weight of water were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-135-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 175 Wh / kg. The bulk density of the extrudate was adjusted by adding 3-4 parts of water in barrel 12. The extrudate was discharged through two 29-hole dies, each with a diameter of 2 mm, and cut by a die-face cutter box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0066] Starch sample 3
[0067] 100 parts by weight of cationic waxy corn starch ( 180, purchased from Tate & Lyle) was fed into a Buhler twin-screw extruder at a rate of 300 kg / h and a screw speed of 650 RPM. 12 parts by weight of water, 1 part by weight of a 10% aqueous solution of sodium hydroxide, and 4 parts by weight of a 10% aqueous solution of sodium trimetaphosphate were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-130-135-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 244 Wh / kg. The extrudate was discharged through two 29-hole dies, each with a diameter of 2 mm, and cut by a die face cutting box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0068] Starch sample 4
[0069] 100 parts by weight of wet cationic waxy corn starch (Interbond TMC, purchased from Tate & Lyle) was fed into a Buhler twin-screw extruder at a rate of 300 kg / h and a screw speed of 600 RPM. 12 parts by weight of water were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-135-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 214 Wh / kg. The bulk density of the extrudate was adjusted by adding 3-4 parts of water in barrel 12. The extrudate was discharged through two 29-hole dies, each with a diameter of 2 mm, and cut by a die face cutting box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0070] Starch sample 5
[0071] 100 parts by weight of cationic potato starch (SolBond PC 80, available from Solam) with a nitrogen content of 0.64% and a moisture content of 11 to 13% was introduced into a Bühler twin-screw extruder at a rate of 300 kg / h and a screw speed of 600 RPM. Six parts by weight of water and 4.5 parts by weight of glycerol were added to the first barrel of the extruder. The extruder had 12 barrels and an adjusted temperature profile of 45-45-45-40-130-130-130-130-135-135-135-135-135°C. During extrusion, the specific mechanical energy applied to the starch was equal to 206 Wh / kg. The extrudate was discharged through two 29-hole dies, each with a diameter of 2 mm, and cut by a die-face cutting box at 3000 RPM. The chopped extrudate was further dried during air conveying and then passed into a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0072] Starch sample 10
[0073] 100 parts by weight of cationic waxy corn starch ( 180, purchased from Tate & Lyle) was fed into a Buhler twin-screw extruder at a rate of 200 kg / h and a screw speed of 550 RPM. 6 parts by weight of water and 0.6 parts by weight of a 10% aqueous phosphoric acid solution were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-135-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 239 Wh / kg. The extrudate was discharged through two 29-hole dies, each with a diameter of 2 mm, and was cut by a die face cutting box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0074] Starch sample 11
[0075] 100 parts by weight of cationic waxy corn starch ( 180, purchased from Tate & Lyle) was fed into a Buhler twin-screw extruder at a rate of 200 kg / h and a screw speed of 550 RPM. 24 parts by weight of water were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-135-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 180 Wh / kg. The extrudate was discharged through two 29-hole dies, each with a diameter of 2 mm, and cut by a die face cutting box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0076] Starch sample 12
[0077] 100 parts by weight of cationic waxy corn starch ( 180, purchased from Tate & Lyle) was fed into a Buhler twin-screw extruder at a rate of 200 kg / h and a screw speed of 550 RPM. 12 parts by weight of water, 4 parts by weight of a 10% aqueous solution of sodium hydroxide, and 1.5 parts by weight of a 5% aqueous solution of sodium trimetaphosphate were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-130-135-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 261 Wh / kg. The extrudate was discharged through two 29-hole dies, each with a diameter of 2 mm, and cut by a die face cutting box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0078] Starch sample 13
[0079] 100 parts by weight of cationic waxy corn starch ( 180, purchased from Tate & Lyle) was fed into a Buhler twin-screw extruder at a rate of 200 kg / h and a screw speed of 550 RPM. 12 parts by weight of water, 4 parts by weight of a 10% aqueous solution of sodium hydroxide, and 1 part by weight of a 5% aqueous solution of sodium trimetaphosphate were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-130-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 269 Wh / kg. The extrudate was discharged through two 29-hole dies, each with a diameter of 2 mm, and cut by a die face cutting box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0080] Starch sample 15
[0081] 100 parts by weight of cationic waxy corn starch ( 235, purchased from Ingredion) was added to a Buhler twin-screw extruder at a rate of 200 kg / h and a screw speed of 350 RPM. 18 parts of water were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-135-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 139 Wh / kg. The bulk density of the extrudate was adjusted by adding 1.5 parts by weight of water to barrel 12. The extrudate was discharged through two 29-hole die heads, each with a diameter of 2 mm, and was cut by a die face cutting box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0082] Starch sample 16
[0083] 100 parts by weight of cationic waxy corn starch ( 650, purchased from Ingredion) was added to a Buhler twin-screw extruder at a rate of 200 kg / h and a screw speed of 350 RPM. 15 parts by weight of water were added to the first barrel of the extruder. The extruder had 12 barrels and the adjusted temperature profile was 45-45-45-40-130-130-130-135-135-135-135-135°C. During the extrusion process, the specific mechanical energy applied to the starch was equal to 180 Wh / kg. The bulk density of the extrudate was adjusted by adding 1.5 parts of water to barrel 12. The extrudate was discharged through two 29-hole die heads, each with a diameter of 2 mm, and was cut by a die face cutting box at 3000 RPM. The chopped extrudate was further dried during air suction conveying and then entered a hammer mill with a 3 mm screen. After grinding, the residual moisture content of the extruded starch powder was 7%.
[0084] Reference starch sample
[0085] Starch sample 17
[0086] Starch sample 17 is waxy corn starch with a nitrogen content of 0.35% and a moisture content of 11 to 13% ( 180, available from Tate & Lyle). Sample 17 is a granular starch used as the feed starch in the extrusion process to prepare Samples 1, 3, 11, 12, and 13.
[0087] Starch sample 18
[0088] Starch sample 18 is a cold water soluble starch ( 280), made from cationic waxy corn starch with a nitrogen content of 0.35%, available from Tate & Lyle. This starch sample was included in the testing procedure to demonstrate the differences between the extrusion process and existing starch gelatinization processes.
[0089] Fibraffin K
[0090] Fibraffin K is a commercially available Cationic potato starch from Fibraffin Co., Ltd., typically used for dry strength applications in the paper industry. Fibraffin K is supplied as starch granules and is cooked as a starch suspension in a jet cooker or heated under atmospheric conditions.
[0091] The composition and physical properties of the starch samples are shown in Table 3.
[0092] Table 3: Composition and physical properties of prepared starch samples
[0093]
[0094] Notes to Table 3:
[0095] NA: Not obtained
[0096] (*) Viscosity (Brookfield viscometer, 100 RPM, 25% solids, 25° C., suspension prepared with 0.8% sodium carbonate (Na 2 CO 3 ) solution).
[0097] (**) Instant starch: (Add 4 g of dry starch to 200 ml of deionized water; stir at 600 RPM for 2 minutes; centrifuge at 3000 RPM for 15 minutes; decant or pipette 100 ml of the supernatant to a dish and dry in an oven at 110°C to determine soluble starch).
[0098] (***) In the case of sample 17 (reference), a starch granule suspension having a solids content of 25% was prepared using a 0.8% Na2CO3 (sodium carbonate) solution. The suspension was heated on a 90°C hot plate for 30 minutes, resulting in a gel that could not be analyzed for viscosity and molecular weight.
[0099] (****) The amount of crosslinker used during extrusion affects the level of starch rapid solubility (RSS) (for the same feed starch). The higher the degree of crosslinking, the lower the RSS level.
[0100] Example 1B - Handsheet Preparation and Testing
[0101] Slurry preparation
[0102] The raw material (stock) for producing handsheets was obtained by beating paper sheets in a pulper. The paper sheets were packaging paper of the specification "Testliner 2" with a basis weight of 100 g / m 2 The pulping process is achieved by dissolving the paper sheet in tap water to a solids content of approximately 3.5% and subsequent mechanical treatment in a pulper. At the end of the pulping process, the pulp has a drainage rate of approximately 43° SR. Pulp drainage is measured in SR units (standing for Schopper Riegler units) according to standard ISO 5267-1:1999.
[0103] Preparation of starch dispersion
[0104] In a glass beaker, starch samples 1, 3, 4, 5, 10, 11, 12, 13, 15 and 16 were used to prepare dispersions of extruded starch powder with a solid content of 10% by mixing 50g of extruded starch powder with 450g of tap water (temperature of approximately 20°C) at 1000RPM using a propeller mixer (ER10). Before processing the slurry, the dispersion of the extruded starch powder underwent a two-step dilution process. 50ml of the 10% solid content dispersion was transferred to a separate glass beaker. The separate dispersion was then diluted to 1% solid content by adding 450g of tap water. The dilution process was repeated again by mixing 50ml of the diluted dispersion (with a solid content of 1%) with 450g of tap water to obtain a highly diluted dispersion with a solid content of 0.1%. The highly diluted extruded starch powder dispersion was then ready to be added to the slurry.
[0105] In the case of reference sample, sample 17 and Fibraffin K, in a glass beaker, 5g starch powder was mixed with 495g tap water (temperature was about 20°C) at 500RPM for 15 minutes to prepare a reference starch suspension with a solid content of 1%. The glass beaker containing the reference starch suspension was then transferred to a heated water bath maintained at 92°C to 95°C. The beaker was kept in the water bath for 30 minutes while continuing to stir at a speed of 500RPM. Before processing the slurry, 50ml of the cooked reference starch solution (solid content was 1%) was diluted with 450g tap water to obtain a starch solution with a solid content of 0.1%. The highly diluted reference starch solution was then added to the slurry and used.
[0106] In the case of Sample 18 (a starch dispersion with a solid content of 30%), a reference starch dispersion with a solid content of 10% was prepared by mixing 166.7 g of the original 30% solids reference starch dispersion with 332.3 g of tap water (temperature of approximately 20° C.) in a glass beaker using a propeller mixer (ER10) at 1000 RPM for 30 minutes. Prior to processing the slurry, the starch dispersion underwent a two-step dilution process. 50 ml of the 10% solids starch dispersion was transferred to a separate glass beaker. The separate dispersion was then diluted to 1% solids by adding 450 g of tap water. The dilution process was repeated by mixing 50 ml of the diluted reference starch dispersion (with a solid content of 1%) with 450 g of tap water to obtain a highly diluted reference starch dispersion with a solid content of 0.1%. The highly diluted reference starch dispersion was then ready for addition to the slurry.
[0107] Slurry treatment
[0108] Separate glass beakers were prepared for treatment, each containing 500 g of a 3.5% solids pulp suspension containing each starch sample, including extruded starch and a reference starch. Two different starch addition levels were used. The lower starch addition level was 5 g dry starch per kg dry pulp, equivalent to 87.5 g of a 0.1% solids starch dispersion or solution. The higher starch addition level was 10 g dry starch per kg dry pulp, equivalent to 175 g of a 0.1% solids starch suspension or solution.
[0109] After starch (extruded starch powder dispersion or reference starch solution / dispersion) was added to the slurry according to the respective addition amount, the components were mixed using a propeller mixer at 100 RPM for 30 minutes. No retention aid was added.
[0110] Hand-made paper
[0111] Just before making handsheets, a portion of the slurry treated with the corresponding type of starch and the corresponding addition amount was taken out from the glass beaker and further diluted to a solid content of 0.25% (see Table 4, test numbers 3 to 54). Handsheet former Handsheets were made (ISO 5269-2:2004). The amount of pulp slurry added to the handsheet former was adjusted to give a 100 g / m 2 The handsheets were of a basis weight of 200 mm in diameter.
[0112] Blank reference
[0113] To provide blank references for the starch-treated cases above, additional handsheets were made without any starch addition (see Table 4, Trial Nos. 1 and 2). For the blank references, a cationic polyacrylamide solution (Solenis supplied) was added to the pulp suspension. 292) as a retention aid. The addition rate was 0.5 g per kilogram of dry pulp (polymer solution, used as is). This treatment maintained solids retention in the blank sheets at the same level as that of the starch-treated sheets. After addition of the retention aid, the pulp suspension was subjected to the dilution and handsheet making processes described above.
[0114] Pressing and drying
[0115] Leave quickly After the handsheet former, the wet handsheets (starch-treated and blank samples) were processed using a hydraulic press to achieve a higher dry content. To do this, the sheets were sandwiched between two sheets of blotting paper and pressed in a hydraulic press at 6 bar for 30 seconds. After the first pressing step, a dry content of 42% to 44% was typically found. For test points targeting a higher dry content, the pressing process was repeated after removing the wet blotting paper from the pressed handsheet and replacing it with a new pair of dry blotting papers. After the second pressing step, the dry content was typically 47% to 48%. After pressing, the handsheets were dried at 93°C for 6 minutes using a standard lightweight handsheet dryer. After drying, the handsheets were stored in a climate chamber at 23°C and 50% relative humidity under controlled environmental conditions for at least 12 hours.
[0116] The mechanical properties of the handsheets were characterized by the following standard methods:
[0117] Short span compression test
[0118] To measure short-span compressive strength (SCT), dry handsheets were cut into 15 mm wide and 125 mm long strips. Six strips were taken from each handsheet. SCT was tested according to ISO 9895:2008. A statistical average of 18 strips from three handsheets was used to determine a single data point.
[0119] Burst strength
[0120] The burst strength was measured according to ISO 2759:2014. A single handsheet was cut into four pieces. Twelve pieces from three handsheets were used to determine the statistical mean of one data point.
[0121] Basis weight -According to ISO536:2019 standard.
[0122] Ash content -According to ISO1762:2019 standard.
[0123] result
[0124] Table 4 summarizes the test results of 54 test points, including starch treatment samples at two addition levels (5 g / kg and 10 g / kg), pressed handsheets at two dry content levels (see test numbers 3-54), and blank controls at two dry content levels. Since the ash content varied little between the different test numbers, the minimum solids content D(x) (according to formula (1)) was found to be approximately 45.3%. As shown in Table 4, test numbers 3, 4, 7, 8, 11, 12, 15, 16, 19, 20, 23, 24, 27, 28, 31, 32, 35, 36, 39 and 40 correspond to a solid content level of D(x) = 45.3% or more; test numbers 5, 6, 9, 10, 13, 14, 17, 18, 21, 22, 25, 26, 29, 30, 33, 34, 37, 38, 41 and 42 correspond to a dry content level below D(x) = 45.3%. Test numbers 23, 24, 25, 26, 47, 48, 49, 50, 51, 52, 53 and 54 did not use extruded starch.
[0125] Analysis and Conclusion
[0126] The test results show that the solids content after pressing is below (-1.3% to -3%) the minimum solids content defined by "D(x)" or above (1.4% to 2.6%) the minimum solids content defined by "D(x)". Deviations of 1.3% to 3% below the minimum solids content of 45.3% or 1.4% to 2.6% above the minimum solids content of 45.3% are considered significant. The blank tests (Test Nos. 1 and 2) did not show a significant response in the strength parameters (SCT and Burst) when the solids content was increased from "below" to "above" the minimum solids content defined by "D(x)" of the test sample.
[0127] Tests on the cooked starch reference samples (see Table 4, Test Nos. 23-26 and 47-50) showed that the strength parameters increased when the starch addition increased from 5 g / kg dry pulp to 10 g / kg dry pulp. However, these tests did not show a significant response in the strength parameters (SCT and burst) when the solids content increased from "below" to "above" the minimum solids content defined by "D(x)" for the test sample.
[0128] For the tests involving extruded starch treated samples (see Table 4, Test Nos. 3-22 and 27-46), a significant response in strength parameters (SCT and burst) was observed when the solids content was increased from "below" to "above" the minimum solids content defined for the test sample "D(x)", regardless of whether the starch addition level was low (5 g / kg) or high (10 g / kg). According to Table 4, the strength increase averaged 6% to 8%. This response was significantly higher than the expected results for the reference samples using cooked granular starch (see Table 4, Test Nos. 23-26 and 47-50).
[0129] Cationic corn starch granules (Sample 17) prepared by cooking for Test Nos. 47-50 were also used as the base starch (Sample 1) for treatment in the extruder and were further used to run Test Nos. 3-6. When the starch is used as a dry strength additive in papermaking, the test results concluded that treating the starch in the extruder significantly improves paper strength compared to treating the starch using conventional cooking methods.
[0130] Furthermore, it was found that industrial gelatinized starches prepared from cationic corn starch having the same cationic charge density (see Table 4, Sample 18, Run Nos. 51-54) did not show a similar increase in paper strength compared to handsheets prepared using extruded starch treated samples when the solids content of the test samples was varied from "below" to "above" the minimum solids content defined by "D(x)." Based on these results, it is believed that processing starch to make it soluble in cold water (e.g., the gelatinization process) is likely not the step in the extrusion process that affects the dry strength properties of extruded starch in paper.
[0131] It was observed that the handsheets tested comprising extruded starch Sample 1 showed superior strength properties compared to reference cooked granular starch and reference precooked starch based on the same starch type and cationicity. Figure 5 It was also observed that the strength properties of the handsheets comprising extruded starch sample 1 (no cross-linking) and sample 12 (cross-linking) were not significantly different. Figure 3 and Figure 4 In addition, for all tests, the strength properties seem to level off when going from 5 kg / t to 10 kg / t. Based on these results, it is suggested that the properties of paper products containing extruded starch may not be strongly dependent on (i) cationicity, as the product with the highest charge has slightly lower strength properties, see Figure 1 (ii) maximizing molecular weight (MW), since products with the highest molecular weight have lower strength properties, see Figure 2 ; (iii) cross-linking changes, as cross-linking does not seem to significantly improve strength properties.
[0132] It was observed that the tests on handsheets comprising extruded starch samples 1 and 12 showed that for both starch addition levels (5 kg / t and 10 kg / t) a significant improvement in strength properties was observed from low dry content (<44%) to high dry content (>46%). Very little improvement in strength properties was observed for the reference starches - cooked granular starch (sample 17) and cold water soluble starch (sample 18). Figure 5 .
[0133] Table 4 - Composition and mechanical properties of prepared handsheets
[0134]
[0135]
[0136]
[0137] Example 1C - Machine-produced paper
[0138] Paper sample 1
[0139] Made of 100% RCP (recycled paper) fiber with a basis weight of 15.5-16.5 g / m 2 In the extrusion of GSM tissue paper, cationic starch addition levels of 2, 4, and 6 kg / T were used. With increasing cationic starch addition, the zeta potential increased from -12.4 mV to 2.4 mV, and the cation demand decreased from 78 uEq / L to 3 Eq / L. Retention increased from 75.2% to 88.9%. Cationic starch effectively neutralizes the surface charge of the fiber. The improved retention also helps reduce the BOD in the wet-end system.
[0140] Paper sample 2
[0141] In one example, standard waxy corn starch (Interstarch) was modified and extruded to have a nitrogen content of 0.35% by weight, a molecular weight of 4 x 10^6 Daltons, and an RSS value of 92%. This cationic extruded starch was added to a tissue paper machine made from virgin fiber consisting of 40% softwood kraft pulp (long fibers), 40% hardwood kraft pulp (short fibers), and 20% bleached chemithermomechanical pulp (BCTMP fibers).
[0142] The machine produces 17.5g / m at a speed of 1650m / min 2 This tissue machine has a double headbox. A double headbox is a system where two headboxes simultaneously add pulp slurry to the web. In this example, one headbox applies primarily long fibers, while the second applies primarily short fibers.
[0143] Additionally, cationic polyacrylamide (cPAM) and polyethyleneimine polymers (PEI) are added to comprise what is known in the papermaking art as a retention system or retention aid system.
[0144] Extruded starch is added only to the long fiber system. It is added before entering the long fiber machine chest, thus before the refiner, refiner chest, and header tank. Ten (10) kilograms of extruded starch are added per ton of dry long fiber pulp in the long fiber line, resulting in a total of five (5) kilograms of extruded starch per ton of finished tissue paper. The extruded starch is added over a 23-hour period.
[0145] No inorganic fillers were added. During the addition of extruded starch, the solids content (also called dryness) measured immediately after the press section was 44% to 46%. The ash content was essentially 0%. The press solids exceeded the minimum press solids content D = 46 + (0-10) * 0.3 = 43%.
[0146] The tensile strength of the tissue paper was measured multiple times over a period of time before and during the addition of the extruded starch. The tensile strength of the tissue paper was measured in the machine direction (the direction of the moving web) and the cross-machine direction (perpendicular to the web). The tensile strength measurements were averaged over a period of time before and during the addition of the extruded starch.
[0147] The average tensile strength of the tissue paper without extruded starch measured in the machine direction was 129 N / m (Newtons per meter).
[0148] The average tensile strength of the tissue without extruded starch measured in the cross-machine direction was 65 N / m.
[0149] The average tensile strength of tissue made from extruded starch, measured in the machine direction, was 159 N / m (Newtons per meter).
[0150] The average tensile strength of tissue made from extruded starch was 86 N / m measured in the cross-machine direction.
[0151] The addition of extruded starch increased tensile strength in the machine direction by 23% and in the cross-machine direction by 32%.
[0152] The dusting tendency of tissue paper during the period of addition of extruded starch was also tested and compared to tissue paper during the period of no extruded starch addition. Dust generation is a measure of the amount of fines and fibers that can be removed from the tissue paper. Increasing the incorporation of fines and fibers into the tissue paper matrix can reduce dusting during the tissue manufacturing process and in the end-use. Dust generation is assessed by measuring the dusting tendency of the tissue paper from an 81 cm 2The fine powder and fibers are removed and collected from the tissue paper sample while maintaining a constant air flow for a fixed time. 2 A tissue paper sample is weighed and placed in a dust collection chamber. The sample is then subjected to a constant airflow through the chamber. The airflow exiting the chamber is filtered, removing loose fines and fibers from the air. The collected fines and fibers are weighed and reported as the amount of fines and fibers removed as a percentage of the original tissue paper.
[0153] The average dust percentage of tissue paper produced without extruding the starch was 1.3%.
[0154] The average dust percentage of tissue paper produced with extruded starch was 1.1%.
[0155] Tissue softness is a desired characteristic of tissue end users. Those skilled in the papermaking field understand that there is generally an inverse relationship between tissue strength and softness; that is, increasing the tensile strength of tissue results in decreased softness. Softness is measured using a Tissue Softness Analyzer manufactured by Emtec Electronic, LLC. The Tissue Softness Analyzer measures microsurface variation, macrosurface variation, and stiffness. These parameters are extensively evaluated in panel tests to develop an algorithm that correlates these characteristics with human perception of softness and creates a quantitative value as an indicator of softness, also known as "hand." The higher the "hand" value, the softer the tissue.
[0156] The average softness measurement for tissue produced without extruded starch was 74.
[0157] The average softness measurement for tissue produced using the extruded starch was 75.
[0158] Surprisingly, the application of extruded starch showed a significant increase in tensile strength without any loss in tissue softness.
[0159] Paper sample 3
[0160] In another example, standard waxy corn starch (Interstarch) was modified and extruded to a nitrogen content of 0.35% by weight, a molecular weight of 4 x 10^6 Daltons, and an RSS value of 92%. This cationic extruded starch was then added to a paper towel machine that uses either 70% hardwood fiber and 30% softwood fiber, or 60-70% hardwood fiber, 30% softwood fiber, and up to 10% BCTMP fiber. BCTMP fiber has a shorter length and lower cost, but the final product has lower tensile strength.
[0161] The machine uses a double-layer headbox to produce 18g / m 2 of paper towels.
[0162] Additionally, cationic polyacrylamide (cPAM) and polyethyleneimine polymers (PEI) are added as part of the retention system as well as wet strength additives.
[0163] Extruded starch is added to the long fiber system, with a total of 5 kg of extruded starch added per ton of finished paper towels. It is added before entering the long fiber machine pulp chest, so before the refiner, refiner pulp chest and header tank.
[0164] No inorganic fillers were added. During the addition of extruded starch, the solids content of the paper web (also known as web dryness), measured immediately after the press section, was 44% to 46%. The ash content was measured to be essentially 0%. The press solids exceeded the minimum press solids content D = 46 + (0-10) * 0.3 = 43%.
[0165] Before adding extruded starch (called "control"), the 18g / m 2 The tensile strength of paper towels was measured for 1 year and then at multiple times during which extruded starch was added (referred to as "tests"). The tensile strength of the paper towels was measured in the machine direction (the direction of the moving web) and the cross-machine direction (perpendicular to the web).
[0166] For a paper towel made with a furnish of 70% hardwood fiber and 30% softwood fiber, the tensile strength is:
[0167]
[0168] For a paper towel made of 60% hardwood fiber, 30% softwood fiber, and 10% BCTMP, the tensile strength is:
[0169]
[0170] The addition of extruded starch increased both the machine and cross-machine direction tensile strength. Furthermore, these results indicate that the tensile strength properties of tissue without BCTMP can be maintained using 5 kg / ton of extruded starch in a low-cost furnish composition using 10% BCTMP.
[0171] Paper sample 4
[0172] In another example, standard waxy corn starch (Interstarch) was modified and extruded to have a nitrogen content of 0.35% by weight, a molecular weight of 4 x 10^6 daltons and an RSS value of 92%. The cationic extruded starch was added to a machine that produces tissue paper from a 100% deinked pulp (DIP) slurry. Deinked pulp is made from fibers collected from various sources after their primary use has expired. The fibers typically contain varying levels of inorganic mineral pigments, commonly referred to as fillers. The amount of pigment carried over the deinking process can be controlled to a certain extent. Keeping fillers in the DIP typically results in lower achievable strength properties because the fillers do not contribute to the strength of the paper sheet. On the other hand, removing fillers reduces the total waste paper production in the deinking process.
[0173] The machine produces 15.6g / m at a speed of 1400m / min 2 This tissue machine is called a gap former. In this system, the headbox feeds the pulp between two moving wires (a top wire and a bottom wire), which "drain" or "dewater" the pulp while carrying it along. After the forming section, the formed mat is transferred to a press station for further mechanical dewatering.
[0174] In this example, no chemical was used as a retention system to enhance retention.
[0175] In this example, the ash content was 2.5% and the basis weight was 15.6 g / m3 over a 3 month period prior to the addition of the extruded starch. 2 Ash is carried over from the deinked pulp. Extruded starch is added to the system at the exit of the mixing tank. The amount of extruded starch is adjusted to 2.7 kg per ton of finished tissue paper. The extruded starch is added over a 32-hour period.
[0176] The addition of extruded starch resulted in an increase in the ash content retention of the tissue paper from 2.5% to 3.3%. This represents an increase in production. In addition, the basis weight of the tissue paper produced during the addition of extruded starch was 15.3 g / m 2 Those skilled in the art of papermaking would expect that an increase in ash content would result in a loss of tensile strength in the tissue paper. Similarly, the basis weight increased from 15.6 g / m 2 Reduced to 15.3g / m 2 This is expected to result in lower tensile strength.
[0177] The solids content measured immediately after the press section was 45% to 47%. This press solids exceeds the minimum press solids in the papermaking process described in this disclosure. Minimum press solids D = 46 + (3.3 - 10) * 0.3 = 43.4%.
[0178] The tensile strength of the tissue paper was measured over a 3 month period prior to and during the addition of the extruded starch. The tensile strength of the tissue paper was measured in the machine direction (direction of web movement) and the cross-machine direction (perpendicular to the web direction). The tensile strength measurements were averaged over the 3 month period prior to and during the addition of the extruded starch.
[0179] The average tensile strength of the tissue paper without extruded starch, measured in the machine direction, was 178 N / m (Newtons per meter).
[0180] The average tensile strength of the tissue without extruded starch measured in the cross-machine direction was 89 N / m.
[0181] The average tensile strength of tissue made from extruded starch, measured in the machine direction, was 189 N / m (Newtons per meter).
[0182] The average tensile strength of tissue made from extruded starch was 83 N / m measured in the cross-machine direction.
[0183] Surprisingly, the increase in ash content and decrease in basis weight during the 2.7 kg / ton addition of extruded starch did not result in a loss in overall tensile strength of the tissue.
[0184] Furthermore, the softness of the tissue paper improved during the addition of 2.7 kg / ton of extruded starch. The softness during the addition of extruded starch was 55.6%, while the three-month average softness of the grade before the addition of extruded starch was 51.4%.
[0185] Paper sample 5
[0186] In another example, linerboard is produced using a base layer made from 100% recycled OCC (old corrugated container) furnish and a white top layer made from 100% virgin hardwood pulp with added precipitated calcium carbonate (PCC) filler. This linerboard is used to make corrugated boxes.
[0187] The paper machine produces linerboard grades with a total board basis weight of 175 g / m 2 The machine uses 10kg / ton of cationic starch in the top layer. Both the base and top layers use cationic polyacrylamide polymer and bentonite mineral as the retention system.
[0188] The extruded cationic waxy corn starch (nitrogen content 0.35 wt %, molecular weight 4×10 6 Daltons, with an RSS value of 92%) was added to the base layer only at the inlet of the blend chest at a rate of 4 kg / ton of finished linerboard for a period of time (referred to as a trial). No adjustments were made to the weight ratios of the top (printing) or bottom layers. The addition of extruded starch resulted in a reduction in the required amount of retention aid.
[0189] The ash content measured during the addition of the extruded starch was 15.5%. The solids content measured immediately after the press section was 48% to 49%. This press solids exceeds the minimum press solids in the papermaking process described in this disclosure. Minimum press solids D = 46 + (15.5 - 10) * 0.3 = 47.7%.
[0190] The key tests for evaluating linerboard strength are the short span compression test (SCT), the burst test, and the Scott bond test.
[0191] SCT is performed by cutting a 15 mm wide strip of manufactured linerboard and clamping the sample between two clamps (typically 0.7 mm apart). A compressive force is applied to the sample. The maximum compressive strength is reported in kilonewtons per meter. The basis weight is then subtracted to obtain units of Newton meters per gram (Nm / g).
[0192] Burst pressure is another indicator used to determine the strength of linerboard and the resulting corrugated board. It is used to indicate the performance of packaging containers in withstanding stress during transportation. It is defined as the maximum pressure that the linerboard surface can withstand in the vertical direction before it breaks. Burst strength is expressed in kilopascals square meters per gram (kPa m2 / g). 2 / g) indicates.
[0193] The Scott Bond Test is a measurement of the energy required to rapidly peel a linerboard specimen. The force is applied using a pendulum of known mass and speed. The pendulum assembly provides a rotational tensile stress that produces a minimum shear stress, causing rupture in the z-direction. When the specimen ruptures in the z-direction, the energy absorbed due to the elongation and stretching of the fiber matrix is recorded. The stronger the fiber web, the greater the energy absorbed when the specimen ruptures. The Scott Bond is measured in Joules per square meter (J / m 2 ). The result is as follows:
[0194]
[0195] This shows that, despite a 15.6% increase in ash content during the trial, which was detrimental to linerboard strength, extruded cationic starch resulted in increases in measured strength SCT (3.4% increase), burst (8.9% increase), and Scott bond (21.8% increase).
[0196] Previous attempts to increase strength on this machine were made by adding 3 kg / ton of cationic jet cooked starch to the base layer, with no effect on strength as measured by SCT, burst and Scott bond.
[0197] Paper sample 6
[0198] In another example, standard waxy corn starch (Interstarch) was modified and extruded to a nitrogen content of 0.35% by weight, a molecular weight of 4X10^6 Daltons and an RSS value of 92%. The cationic extruded starch was added to a machine that produces paper for graphic printing. The slurry consisted of 75% short fibers, 23% long fibers and 2% BCTMP pulp. In addition, ground calcium carbonate (GCC) "filler" was added to the pulp to give an ash content of 31% for the final paper. In addition, an anionic polyacrylamide emulsion was added as a retention system. In addition, 8 kg / ton of the above-mentioned cationic starch was added. The ingredients were added to the fourdrinier wire from the headbox. The total basis weight of the finished paper was 120 g / m 2 The paper production speed is 680 m / min.
[0199] In this example, 4.3 kg of extruded starch was added per ton of finished paper. Extruded starch was added at the outlet of the short fiber slurry pool. Paper strength was tested before, during, and after the addition of extruded starch. Strength tests showed that the Scott bond strength of paper produced during the period of adding 4.3 kg / ton of extruded starch was 35% higher than that of paper produced before and after the addition of extruded starch. Furthermore, the tensile strength of paper produced during the period of adding extruded starch was 15% higher than that of paper produced without the addition of extruded starch.
[0200] Previous attempts to improve paper strength by adding traditional cooked starches did not result in additional strength.
[0201] Paper sample 7
[0202] Made with 100% DIP compound and weighing 16.8g / m 2 The target strength is 130-172N / m in the machine direction (MD) and 65-68N / m in the cross direction (CD). After adding 2kg / T of extruded cationic waxy corn starch, the MD tensile strength is 158N / m and the CD tensile strength is 80N / m. TM After PC 50 potato starch, MD tensile strength is 154N / m, DC tensile strength is 75N / m. Add 2.4kg / T extruded cationic Raisamyl TM After adding 80051 wheat starch, the MD tensile strength was 153 N / m and the CD tensile strength was 77 N / m. Corn, potato, and wheat starches all achieved or exceeded the target strength at acceptable addition levels.
[0203] The embodiments described herein are intended to be exemplary only. Those skilled in the art may alter, modify, and / or vary the specific embodiments. The scope of the claims should not be limited by the specific embodiments described herein, but should be interpreted in a manner consistent with the specification as a whole.
[0204] While various aspects, embodiments and / or examples of the present disclosure have been thus described, it will be recognized that variations may be made therein without departing from the spirit and scope of the disclosure, and that such variations are intended to be included within the scope of the appended claims.
[0205] All publications, patents, and patent applications mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent, or patent application was specifically and individually indicated to be incorporated by reference.
Claims
1. A method for making paper, The following steps are involved: providing a slurry comprising a fibrous material, an extruded starch, water, and optionally one or more inorganic fillers; forming a paper web from the pulp; Pressing paper web; as well as Drying the paper web, Therein, the solids content of the pressed paper web in % by weight is at least as great as the minimum solids content D(x) defined by formula (I): D(x)=46+(x-10)*0.3(I) where x is the ash content of the dry paper.
2. The method according to claim 1, in, The ash content is determined according to ISO 1762:2019.
3. The method according to claim 1 or 2, in, The weight of the paper is 12-240 g / m 2 .
4. A method as claimed in any one of claims 1 to 3 comprising adding the extruded starch to an aqueous suspension of fibrous material.
5. The method according to any one of claims 1 to 4, in, Before the slurry is drained, the slurry has a fiber material concentration of 0.5 g / L to 15 g / L.
6. The method of claim 5, comprising providing the thick stock at an initial concentration of the fiber material of 0.5 g / L to 40 g / L, 10-40 g / L or 20-40 g / L, and diluting the thick stock to a concentration of 0.5 g / L to 15 g / L.
7. The method according to claim 6, in, The inorganic filler concentration of the thick slurry is 0 to 20 g / L.
8. The method according to any one of claims 1 to 7, in, The extruded starch in the slurry is 0.05 to 5 wt%, or 0.06 to 2 wt%, relative to the weight of the dry fiber material.
9. The method according to any one of claims 1 to 8, in, The extruded starch is not cross-linked.
10. The method according to any one of claims 1 to 8, in, The extruded starch is cross-linked.
11. The method according to any one of claims 1 to 10, in, The extruded starch is cationic.
12. The method according to any one of claims 1 to 11, in, The fiber material includes softwood fibers, hardwood fibers, non-wood fibers, or a combination thereof.
13. The method according to any one of claims 1 to 12, in, The fiber material includes waste paper, commercial pulp, paper machine broke, recycled fiber or a combination thereof.
14. The method according to any one of claims 1 to 13, in, The inorganic filler comprises one or more pigments selected from the group consisting of metal oxides, silicates, carbonates, calcium carbonate, ground lime, chalk, marble (GCC), precipitated calcium carbonate (PCC), talc, kaolin, bentonite, satin white, calcium sulfate, barium sulfate and titanium dioxide.
15. A method as claimed in any one of the preceding claims, in, At least a portion of the inorganic filler is provided as part of the recycled fiber material.
16. A method as claimed in any one of the preceding claims, in, The slurry comprises one or more paper aids, optionally selected from the group consisting of sizing agents, wet strength agents, retention aids, drainage aids, dry strength enhancers, optical brighteners, defoamers, biocides, paper dyes, or combinations thereof.
17. A method as claimed in any one of the preceding claims, in, The paper has an ash content of about 0 wt % to about 40 wt %.
18. A method as claimed in any one of the preceding claims, in, The extruded starch has one or more of the following attributes: the extruded starch is cationic; the extruded starch is not cross-linked; the solubility of the extruded starch is 40-99% or 40-93%; the molecular weight of the extruded starch is greater than 300,000 Da or greater than 500,000 Da or greater than 2,000,000 Da, or is 4,000,000 Da or greater; the molecular weight of the extruded starch is 12,000,000 Da or less, or 10,000,000 Da or less, or 8,000,000 Da or less; the weight fraction (WF / dLog M) of the extruded starch at 30,000,000 Da is 0.05 or less; the cumulative weight fraction of the extruded starch at a molecular weight of 1,000,000 Da or less or 100,000 Da or less is 0-8% or 0-1%; the RVA viscosity of the extruded starch is 15,000 cP or less or 5,000 cP or less; and the extruded starch is chemically or enzymatically modified during the extrusion process.
19. A method for preparing a starch-containing product, The following steps are involved: The starch-containing material is processed in an extruder or in other high shear and / or high specific mechanical energy environment, preferably using a twin screw extruder, optionally with one or more mixing and / or high shear sections, substantially without the use of a crosslinking agent.
20. The method of claim 19, in, The starch-containing material is chemically or enzymatically modified in an extruder or other high shear environment, for example the starch is acid-hydrolyzed and / or made cationic.
21. The method according to claim 19 or 20, in, The molecular weight (Mw) of the resulting product is 300,000 Da or more, or 500,000 Da or more, or 2,000,000 Da or more, or 4,000,000 Da or more, or 5,000,000 Da or more, optionally up to 12,000,000 Da.
22. The method according to any one of claims 19 to 21, in, The obtained products have basically no molecular weight greater than 3*10 7 Big part.
23. The method according to any one of claims 19 to 22, in, The starch-containing material includes natural starch or flour.
24. The method according to any one of claims 19 to 23, in, The starch-containing material includes corn starch, such as waxy corn starch.
25. The method according to any one of claims 19 to 24, in, The starch-containing material includes cereal starch (such as corn, wheat or barley starch), root or tuber starch (such as potato or tapioca starch), legume starch (such as pea or lentil starch), or combinations thereof.
26. The method according to any one of claims 19 to 25, in, The resulting product has an RVA viscosity of 15,000 cP or less or 5,000 cP or less at 20% solids.
27. The method according to any one of claims 19 to 26, in, The extrusion or other treatment is carried out on a starch-containing material having a SME of 100 Wh / kg or more, or on a starch-containing material having a SME of 150 Wh / kg or more.
28. The method according to any one of claims 19 to 27, in, The extrusion or other processing is carried out at a maximum barrel temperature of 180°C or less, or 160°C or less.
29. The method according to any one of claims 19 to 28, in, Humectants, plasticizers or polyols are added to the extruder.
30. A starch-containing product having a molecular weight (Mw) of more than 300,000 Da and having one or more of the following characteristics: a) an RVA viscosity of 15,000 cP or less at 20% solids, b) substantially no weight fraction exceeding 30,000,000 Da (i.e., within 3*10 7 Da WF / dLogMW is 0.05 or less), c) solubility is 40-99%, d) molecular weight is 1000000Da or less or the cumulative weight fraction of 100000Da or less is 0-8% or 0-1%, e) Mw is 12000000Da or less.
31. The product of claim 30, having a molecular weight (Mw) of 4,000,000 Da or more.
32. The product of claim 30 or 31 having an RVA viscosity at 20% solids of 15,000 cP or less or 10,000 cP or less.
33. A product as claimed in any one of claims 30 to 32, further comprising one or more of the following: a humectant, a plasticiser, and a polyol, such as glycerol.
34. A product as claimed in any one of claims 30 to 33, consisting predominantly, i.e. 80% or more by dry weight, of one or more of starch, protein or other material found in native starch or flour, or a derivative thereof, optionally waxy maize starch.
35. The product of any one of claims 30 to 34 having a solubility (RSS) of 40-93% or 40-92%.
36. A product as claimed in any one of claims 30 to 35 which is cationic, for example having a bound nitrogen content excluding protein nitrogen of about 0.1-1.6% or 0.1-0.8%.
37. A method for producing paper, card and paperboard, the method comprising draining a pulp comprising a mixture of paper fibers, an inorganic filler, water and at least one extruded starch, forming a paper sheet in a wire section, further removing water from the wet paper sheet by pressing the paper sheet in a press section, and finally removing water by heat treatment in a dryer section to form a product, in: The pulp has a fiber concentration of 0.5 g / L to 40 g / L and an inorganic filler concentration of 0 g / L to 20 g / L, and contains at least one starch dispersion obtained by extruding starch, wherein the pulp containing the starch dispersion is diluted to a fiber concentration of 0.5 g / L to 15 g / L before the papermaking process, such as the first dewatering step, and then the diluted pulp is drained to form a paper sheet, and the paper sheet is pressed in a press section to a solid content D(x) weight % or more, D(x) being calculated according to the following formula D(x)=46+(x-10)·0.3 wherein x is the numerical value of the inorganic filler content of the product (in wt %), D(x) is the minimum solids content (in wt %) to which the sheet is pressed, and wherein the extruded starch providing the starch dispersion is obtained by mixing the feed starch with an aqueous liquid and applying mechanical and thermal energy in an extruder by shearing and / or additional heating.
38. The method of claim 37, in, Extruded starch is added to the thick or thin stock in the wet end system of the paper machine.
39. The method of claim 37 or 38, in, The aqueous liquid is water or alcohol or a mixture of the two.
40. The method of any one of claims 37 to 39, in, The feed starch can be any kind of cationic starch, cross-linked cationic starch, anionic starch, cross-linked anionic starch, non-ionic starch, cross-linked non-ionic starch, amphoteric starch, cross-linked amphoteric starch, all of which may or may not be subjected to other chemical modifications, such as carboxylation, oxidation, hydrolysis, etherification, esterification, etc.
41. The method of any one of claims 37 to 40, in, In the step of mixing the feed starch and the aqueous liquid to obtain a mixture, an additional plasticizer is added in addition to water.
42. The method of any one of claims 37 to 41, in, During the extrusion process, reactants carrying cationic or anionic functional groups are added to the extruder to react with the starch.
43. The method of any one of claims 37 to 42, in, The cross-linking agent is added to the extruder and / or is added to the mixture of feed starch and aqueous liquid before the mixture is added to the extruder.
44. The method of any one of claims 37 to 43, in, One or more chemical agents are added to the extruder and / or one or more chemical agents are added to the mixture of feed starch and aqueous liquid before the mixture is added to the extruder.
45. The method of any one of claims 37 to 44, in, A hydroxyl liquid is injected at the last stage of the extruder and the mixture is dispersed in the extruder or outside the extruder or inside and outside the extruder to obtain a dispersion with a solid content of 20% to 50% by weight, wherein the hydroxyl liquid used in the extrusion process is water, a mixture of water and alcohol or an alcohol, wherein the obtained dispersion has a solid content of 20% to 50% by weight, optionally it can be added directly to the pulp or after pre-dilution with waste water.
46. The method of any one of claims 37 to 45, in, A highly viscous starch melt leaves the extruder at an outlet with a dry content of at least 65 wt. %, wherein the remaining water evaporates to less than 14 wt. % or less than 10 wt. %, wherein after cooling, the viscous material becomes a brittle solid which can be comminuted into small pieces in a hammer mill, cryogenic grinding or similar comminution step / device, wherein the resulting powder product is characterized by a completely amorphous state, has no signs of birefringence and provides a stable dispersion of starch particles with a particle size between 0.2 and 100 μm when mixed with cold water at a solids concentration of 1 wt. %, wherein the starch powder dispersed in water is added to the thick stock and / or thin stock of a paper machine, or is added earlier in the pulp preparation process, preferably wherein the starch powder is added directly to the pulp in thick stock and / or thin stock conditions to form a dispersion with the liquid components of the pulp.
47. The method of any one of claims 37 to 46, in, The solids content of starch in the final pulp composition is between 500 g dry starch per ton of dry paper fiber and 50 kg dry starch per ton of dry paper.
48. The method of any one of claims 37 to 47, in, The drying section of the papermaking process consists at least partly of a Yankee cylinder type arrangement.
49. The method of any one of claims 37 to 48, in, The extruded starch is characterized by a RSS of 92% or less.