Regenerated rubber and preparation method thereof

Through the physical and mechanical methods of using epoxidized soybean oil, rosin and other additives in rubber regeneration technology, the problems of low efficiency and complex equipment of traditional desulfurization methods are solved, low energy consumption and efficient rubber regeneration are achieved, and the products produced are in line with national standards and reduce production costs.

CN118978755APending Publication Date: 2024-11-19BEIJING PINGHE LIHUA TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411254095.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Among the existing rubber regeneration technology, traditional desulfurization methods have problems such as low production efficiency, large energy consumption, serious pollution and complex equipment, and cannot achieve industrial production, and there are too many additives added and the process equipment is complicated.

Method used

By using physical and mechanical methods, after mixing vulcanized rubber powder with epoxidized soybean oil, rosin, pine tar, anti-aging agent and accelerator, shearing and stirring in a shear mixer, and then insulate it in the insulation and return to the original machine. Finally, Refining is carried out in a cooler and a high shear refiner to achieve the return and regeneration of vulcanized rubber.

Benefits of technology

The rubber regeneration is achieved at a lower temperature, reducing energy consumption, reducing exhaust gas, waste water and waste slag emissions. The recycled rubber products produced comply with national standards, and the materials and equipment used are simple and easy to maintain, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978755A_ABST
    Figure CN118978755A_ABST
Patent Text Reader

Abstract

The invention discloses regenerated rubber and a preparation method thereof, and belongs to the technical field of rubber regeneration. The regenerated rubber is prepared from vulcanized rubber powder, vegetable oil, pine tar, rosin and auxiliaries. Preferably, the raw materials for preparing the vulcanized rubber powder are waste tires or other rubber products; preferably, the vegetable oil is epoxidized soybean oil. According to the preparation method, the adopted materials are sheared in a shearing stirrer which is low in temperature and high in shearing force, heat preservation and reversion are carried out under nitrogen protection, and cooling is carried out under nitrogen protection; and no waste gas, waste water or waste residue is discharged. And the obtained product completely meets the technical indexes of national regenerated rubber products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber regeneration, and relates to a regenerated rubber and a preparation method thereof, and in particular to a process and a formula composition for regenerating waste rubber by a physical and mechanical method. Background Art

[0002] Rubber is a system with a stable three-dimensional network structure after vulcanization. One of the main means of regeneration is desulfurization. For many years, the traditional desulfurization methods used to produce reclaimed rubber include oil method, water-oil method, high temperature and high pressure dynamic desulfurization method, but these methods have disadvantages such as low production efficiency, high energy consumption, and serious secondary pollution. In new desulfurization and regeneration methods such as electron beam radiation desulfurization method, microwave regeneration, and ultrasonic regeneration, there are shortcomings such as complex process equipment and unsatisfactory regeneration effect, which cannot be carried out in industrial production.

[0003] Chinese patent application CN200910306213.6 relates to a method for environmentally friendly white fine recycled rubber, which includes taking white vulcanized rubber for footwear as raw material, and obtaining environmentally friendly white fine recycled rubber through the processes of selection and impurity removal, crushing, desulfurization, kneading, filtering, refining, and forming. The method improves the previous desulfurization formula and desulfurization process conditions, and also improves the operating conditions of the crushing, kneading, filtering, and refining processes. The environmentally friendly white fine recycled rubber particles obtained are fine and odorless, and the chemical composition is simple. The method also has the problem of adding too many additives and complicated process equipment.

[0004] Chinese patent application CN200910172564.2 relates to a method for regenerating rubber, comprising the following steps: first, various waste steel wire tires are classified and processed, and crushed by crusher, medium crushed and fine crushed, and the fine rubber powder is loaded into the desulfurization tank; then, rubber activator and rubber softener auxiliary materials are added to the desulfurization tank, and the feed port is closed; the temperature of the raw materials in the desulfurization tank is heated to 220℃-230℃ and the pressure reaches 2.0-2.7MPa by heat source, and maintained for 2 hours, and after desulfurization and plasticization, the pressure relief valve is opened to discharge the gas in the desulfurization tank; after the desulfurized regenerated rubber powder is discharged from the tank, it is finally pressed into sheets by the refiner and open mill in the rubber pressing equipment to make recycled rubber products. In this method, many types of additives are added, the process equipment is complicated, and especially high temperature and high pressure conditions are required.

[0005] In order to better recycle waste tire rubber, there is always hope for a better method, such as a more environmentally friendly method.

[0006] The devulcanization process of recycled rubber is to restore the vulcanized rubber to an unvulcanized state. This process involves physical, chemical or other methods. The main purpose is to break the sulfur bonds (SS) and sulfur-carbon bonds (SC) in the three-dimensional network structure of the rubber without destroying the carbon-carbon bonds (CC). The devulcanization process has specific requirements for temperature, and different devulcanization technologies have different temperature controls.

[0007] In the traditional dynamic desulfurization tank process, waste tires and rubber products are crushed into rubber powder and placed in the desulfurization tank together with the regeneration agent. Desulfurization treatment is carried out under the conditions of pressurization, heating and water addition. The desulfurization tank needs to use a Class II pressure vessel, and the pressure during desulfurization is 2.2-4.0MPa. In order to prevent the rubber powder from being carbonized due to uneven heating at high temperatures, a certain amount of water is added during desulfurization to form steam or directly introduce water vapor as a heat transfer medium. The regenerated rubber desulfurization tank is a key equipment used in the rubber regeneration process. It restores the plasticity of vulcanized rubber through different desulfurization methods. Summary of the invention

[0008] The present invention overcomes the disadvantages of the above-mentioned technology and provides a method for regenerating waste rubber, including the following process and composition of waste tire rubber powder with a fineness of not more than 20 meshes. The first item is batching, in which various materials, vulcanized rubber powder, epoxidized oxidized soybean oil, rosin, pine tar ring, antioxidant, and accelerator are mixed; after being uniformly mixed, they are input into a shearing mixer through a conveyor. The shearing mixer is 100L and the speed is 1500 to 3000 rpm for stirring. After stirring, it is further returned to the original state so that the vulcanized rubber molecules can be changed. The purpose of the shearing mixer is to terminate the double radical combination of free radicals between molecules. After another 1.5-3 hours in the heat preservation and return machine, nitrogen is introduced to allow the vulcanized rubber polymer to be heat-insulated and returned to the original state. Then, the material is discharged when it is cooled to 60±3°C in the cooler, and nitrogen is also introduced into the cooler for nitrogen protection to prevent oxidation. Then it is transported to a high shear refining machine with a front and rear roller speed ratio of 1; 1.45-2.0 for refining. The roller temperature does not exceed 80±3℃. After refining for 4-6 times, the sheets are produced as finished products and then packaged.

[0009] Epoxidized soybean oil can increase the crosslinking density and mechanical properties of natural rubber. Epoxidized soybean oil is a soybean oil derivative treated by epoxidation reaction. Its main functions in reclaimed rubber include: 1. Plasticizer: Epoxidized soybean oil can be used as a plasticizer to increase the plasticity and flexibility of reclaimed rubber and improve its processing performance. The epoxy groups in the epoxidized soybean oil molecules can react with rubber molecules to improve compatibility. 2. Improve vulcanization performance: Epoxidized soybean oil may affect the vulcanization process of reclaimed rubber. It can be used as an active agent in the vulcanization process to promote the vulcanization reaction. 3. Improve the stability of the rubber compound: Epoxidized soybean oil can improve the thermal stability and antioxidant properties of reclaimed rubber and reduce thermal degradation during processing. 4. Enhance the adhesion of the rubber compound: Epoxidized soybean oil can enhance the adhesion between reclaimed rubber and fillers and reinforcing materials, thereby improving the mechanical properties of the final product. 5. Environmentally friendly: an additive of renewable resources. 6. Reduce costs: Epoxidized soybean oil can be used as a low-cost plasticizer to replace some traditional petroleum-based plasticizers, which helps to reduce the production cost of reclaimed rubber. 7. Improve the processing properties of rubber: Epoxidized soybean oil can reduce the viscosity of recycled rubber and improve its fluidity.

[0010] The functions of pine tar include: 1. Improving the adhesion of rubber. 2. Promoting the uniform dispersion of compounding agents. 3. Delaying vulcanization to prevent scorching. 4. Increasing the viscosity and plasticity of rubber to improve processing performance. 5. Activation: Pine tar can activate thiazole accelerators and increase the effects of various compounding agents.

[0011] Rosin mainly plays the following roles: 1. Softener: Rosin can be used as a softener to facilitate processing and kneading. It is beneficial to improve the elasticity and adhesion of the rubber, promote the dispersion of the compounding agent, and thus improve the processing performance of the reclaimed rubber. 2. Promote dispersion: Rosin helps the uniform dispersion of the accelerator and the compounding agent in the rubber. Rosin plays an important role in the processing of reclaimed rubber. Through reasonable use, it can significantly improve the performance and processing technology of the reclaimed rubber.

[0012] Antioxidant 4020 is a p-phenylenediamine rubber antioxidant. In reclaimed rubber, the role of antioxidant 4020 is mainly reflected in the following aspects: 1. Antioxidant performance: Antioxidant 4020 has good antioxidant performance and can effectively delay the oxidation aging process of reclaimed rubber. 2. Anti-ozone protection: It also has an anti-ozone effect, which can protect reclaimed rubber from ozone erosion and extend the service life of rubber products. 3. Anti-flex cracking: Antioxidant 4020 can reduce the cracking of reclaimed rubber when it is repeatedly deformed or stressed, and improve its fatigue resistance. 4. Inhibition of harmful metals: It can also inhibit the catalytic oxidation of harmful metals such as copper and manganese on rubber, thereby protecting rubber products. The main role of antioxidant 4020 in reclaimed rubber is to provide comprehensive aging protection and improve its performance stability.

[0013] Accelerator M is a vulcanization accelerator widely used in the rubber industry. In recycled rubber, the functions of accelerator M include: 1. Accelerate vulcanization reversion: Accelerator M can significantly accelerate the speed of the vulcanization reaction, making the vulcanization reversion process of recycled rubber faster and more efficient. 2. Reduce the tendency to scorch: Accelerator M helps to reduce the tendency of rubber to scorch during processing and improve processing safety. 3. Improve thermal stability: It can improve the thermal stability of vulcanized rubber and reduce performance loss at high temperatures. 4. Good compatibility: Accelerator M is compatible with a variety of rubbers and vulcanization systems and is suitable for a variety of rubber formulations.

[0014] The first aspect of the present invention is to disclose a regenerated rubber, the raw materials for preparing the regenerated rubber include vulcanized rubber powder, vegetable oil, pine tar, rosin and additives;

[0015] Preferably, the raw material for preparing the vulcanized rubber powder is waste tires or other rubber products;

[0016] Preferably, the vegetable oil is at least one of soybean oil, palm oil, rapeseed oil, sunflower oil, coconut oil, olive oil, linseed oil, castor oil, cottonseed oil, rice bran oil, peanut oil and sesame oil and epoxidation products thereof; more preferably epoxidized soybean oil.

[0017] In some embodiments of the present invention, the auxiliary agent includes an antioxidant and an accelerator;

[0018] Preferably, the antioxidant is at least one of antioxidant 4020, antioxidant 4010, antioxidant 4010NA, antioxidant 4030 and antioxidant RD;

[0019] Preferably, the accelerator is at least one of accelerator M, accelerator DM and accelerator TMTD.

[0020] In some embodiments of the present invention, the prepared raw materials include:

[0021] 100 parts by weight of vulcanized rubber powder;

[0022] 1-18 parts by weight of vegetable oil;

[0023] Rosin 1-6 parts by weight;

[0024] 3-18 parts by weight of pine tar;

[0025] 1-4 parts by weight of antioxidant;

[0026] 1-4 parts by weight of accelerator;

[0027] Preferably, the mesh number of the vulcanized rubber powder is not less than 20.

[0028] The second aspect of the present invention is to disclose a method for preparing regenerated rubber, comprising the following steps:

[0029] S01, raw material mixing;

[0030] S02, shear stirring;

[0031] S03, return to the original state under inert gas insulation;

[0032] S04, cooling under inert gas;

[0033] S06, refining until the viscosity is acceptable, and then cutting into slices;

[0034] and optional, S07, package.

[0035] In some embodiments of the present invention, the qualified viscosity means the qualified Mooney degree.

[0036] In some embodiments of the present invention, in S02, the temperature of the shear stirring is lower than 180°C, preferably lower than 173°C.

[0037] In some embodiments of the present invention, in S03, the temperature of the heat preservation and returning to the original state is lower than 180°C, preferably lower than 173°C.

[0038] In some embodiments of the present invention, in S04, cooling to 55-65°C is performed.

[0039] In some embodiments of the present invention, in S05, during the refining, the speed ratio of the front and rear rollers is 1; 1.45-2.0.

[0040] In some embodiments of the present invention, in S05, during the refining, the roller temperature does not exceed 80±3°C.

[0041] In some embodiments of the present invention, in S05, refining is performed 4-6 times.

[0042] In some embodiments of the present invention, the shear stirring of S02 uses a shear mixer.

[0043] In some embodiments of the present invention, the heat preservation and restoration in S03 uses a heat preservation and restoration machine.

[0044] In some embodiments of the present invention, S04 is cooled using a cooling machine.

[0045] In some embodiments of the present invention, the refining of S05 adopts a high shear refiner with front and rear rollers.

[0046] Beneficial effects:

[0047] First, the temperature used in the present invention is lower than that in the above inventions and documents and the actual industrial production temperature at present, and the production is carried out below 160°C. The principle of the present invention to achieve rubber regeneration at a lower temperature is that there are three indispensable conditions in the rubber vulcanization process: one is temperature, the second is pressure, and the third is time. The accelerator promotes the vulcanization of rubber. At the same time, if the rubber is to be restored to its original state, it is also due to the effects of these three elements. The return of the vulcanized rubber to its original state also requires these three conditions. The first is that the temperature is slightly higher than the vulcanization temperature, and the second is that the pressure is greater than the vulcanization pressure. The present invention uses shear force, and excessive shear force will cause the rubber to return to its original state after vulcanization: the third is time. At a certain time, the accelerator will have a certain effect on the cross-linked network structure, thereby causing the rubber to return to its original state.

[0048] Second, the material is sheared in a high shear mixer.

[0049] Third, there is no emission of waste gas, waste water or waste residue.

[0050] Fourth, the obtained product fully complies with the national technical indicators for recycled rubber products. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 The present invention provides a process for preparing recycled rubber according to one embodiment of the present invention. DETAILED DESCRIPTION

[0052] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0053] Unless otherwise specified, the examples and comparative examples are parallel tests with the same components, component contents, preparation steps, preparation parameters, dimensions, etc. The national standard for "recycled rubber" refers to "GB / T 13460-2016 General Specification for Recycled Rubber".

[0054] In the following examples and comparative examples, the shear mixer is model YXKY-JQ200 manufactured by Beijing Yixiang Keyu Technology Development Co., Ltd., the heat preservation regeneration machine is model PHLH-10 manufactured by Beijing Yixiang Keyu Technology Development Co., Ltd., the ventilation water jacket cooler is model LTJ-TP1T manufactured by Beijing Pinghe Lihua Technology Co., Ltd., and the front and rear roller speed ratios of the high shear force refiner are 1:1.20 respectively. The roller temperature is 80±3°C.

[0055] Example 1

[0056] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of whole tire rubber powder R-TW (20 mesh), 4kg of epoxidized soybean oil, 2kg of rosin, 20kg of pine tar, 1kg of antioxidant 4020, and 1kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The shear mixer rotates at a speed of 1500 rpm to return the vulcanized rubber to its original state; the shear stirring temperature is 158±3℃; and the time is 20 minutes. Then, convey the material to the heat preservation and return machine. The temperature inside the heat preservation and return machine is 158±3℃, and nitrogen is introduced at the same time with a nitrogen flow rate of 8m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 3 hours. After 3 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 14m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then sent to the next refiner. After entering the refiner for 5 times in total, the required product can be obtained, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0057] Example 2

[0058] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of whole tire rubber powder R-TW (20 mesh), 18kg of epoxidized soybean oil, 5kg of rosin, 2kg of pine tar, 40202kg of antioxidant, and 4kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 2000 rpm, and the shear stirring temperature is 158±3℃; the time is 20 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature inside the heat preservation return machine is 160±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 16m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 2.5 hours; after 2.5 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 16m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining twice, and then to the next refining. A total of 5 times of refining can be entered into the refiner to obtain the required product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0059] Example 3

[0060] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of whole tire rubber powder R-TW (20 mesh), 6kg of epoxidized soybean oil, 3kg of rosin, 18kg of pine tar, 1kg of antioxidant 4020, and 2kg of accelerator M. Mixing temperature, room temperature; mixing time 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 3000 rpm, and the shear stirring temperature is 158±3℃; the time is 20 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature of the heat preservation return machine is 170±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 18m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 1.5 hours; after 1.5 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 25m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then to the next refining. A total of 5 times of refining can achieve the desired product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0061] Example 4

[0062] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; wherein, 100kg of whole tire rubber powder R-TW (40 mesh), 10kg of epoxidized soybean oil, 2kg of rosin, 10kg of pine tar, 40202kg of antioxidant, and 3kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 1500 rpm, and the shear stirring temperature is 158±3℃; the time is 20 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature of the heat preservation return machine is 158±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 14m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 3 hours; after 3 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 14m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then to the next refining. A total of 5 times of refining can achieve the desired product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0063] Example 5

[0064] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of whole tire rubber powder R-TW (40 mesh), 15kg of epoxidized soybean oil, 1kg of rosin, 5kg of pine tar, 40204kg of antioxidant, and 2kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 1500 rpm, and the shear stirring temperature is 158±3℃; the time is 20 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature of the heat preservation return machine is 158±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 12m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 3 hours; after 3 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 14m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then to the next refining. A total of 5 times of refining can achieve the desired product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0065] Example 6

[0066] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of whole tire rubber powder R-TW (60 mesh), 10kg of epoxidized soybean oil, 6kg of rosin, 10kg of pine tar, 40203kg of antioxidant, and 1kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 1500 rpm, and the shear stirring temperature is 158±3℃; the time is 15 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature of the heat preservation return machine is 158±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 12m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 3 hours; after 3 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 24m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then to the next refining. A total of 5 times of refining can achieve the desired product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0067] Example 7

[0068] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of tread rubber powder R-TT (20 mesh), 4kg of epoxidized soybean oil, 2kg of rosin, 20kg of pine tar, 1kg of antioxidant 4020, and 1kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The shear mixer rotates at a speed of 1500 rpm to return the vulcanized rubber to its original state; the shear stirring temperature is 158±3℃; the time is 20 minutes. Then, convey the material to the heat preservation and return machine, the temperature inside the heat preservation and return machine is 158±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 8m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 3 hours. After 3 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 14m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then sent to the next refiner. After entering the refiner for 5 times in total, the required product can be obtained, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0069] Example 8

[0070] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of tread rubber powder R-TT (20 mesh), 18kg of epoxidized soybean oil, 5kg of rosin, 2kg of pine tar, 40202kg of antioxidant, and 4kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 2000 rpm, and the shear stirring temperature is 158±3℃; the time is 20 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature inside the heat preservation return machine is 160±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 16m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 2.5 hours; after 2.5 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 16m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining twice, and then to the next refining. A total of 5 times of refining can be entered into the refiner to obtain the required product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0071] Example 9

[0072] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of tread rubber powder R-TT (20 mesh), 6kg of epoxidized soybean oil, 3kg of rosin, 18kg of pine tar, 1kg of antioxidant 4020, and 2kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 3000 rpm, and the shear stirring temperature is 158±3℃; the time is 20 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature of the heat preservation return machine is 170±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 18m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 1.5 hours; after 1.5 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 25m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then to the next refining. A total of 5 times of refining can achieve the desired product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0073] Example 10

[0074] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; wherein, 100kg of tread rubber powder R-TT (40 mesh), 10kg of epoxidized soybean oil, 2kg of rosin, and 10kg of pine tar. Antiaging agent 4020, 2kg, accelerator M3kg. Mixing temperature, room temperature; mixing time 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 1500 rpm, and the shear stirring temperature is 158±3℃; the time is 20 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature of the heat preservation return machine is 158±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 14m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 3 hours; after 3 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 14m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then to the next refining. A total of 5 times of refining can achieve the desired product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0075] Embodiment 11

[0076] like Figure 1 As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of tread rubber powder R-TT (40 mesh), 15kg of epoxidized soybean oil, 1kg of rosin, 5kg of pine tar, 40204kg of antioxidant, and 2kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 1500 rpm, and the shear stirring temperature is 158±3℃; the time is 20 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature of the heat preservation return machine is 158±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 12m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 3 hours; after 3 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 14m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then to the next refining. A total of 5 times of refining can achieve the desired product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0077] Example 12

[0078] like Figure 1As shown, weigh the following raw materials in sequence and add them into a 200L mixing tank for mixing; among them, 100kg of tread rubber powder R-TT (60 mesh), 10kg of epoxidized soybean oil, 6kg of rosin, 10kg of pine tar, 40203kg of antioxidant, and 1kg of accelerator M. Mixing temperature: room temperature; mixing time: 15 minutes. After mixing, convey the above mixture to a 100L shear mixer. The speed of the shear mixer is 1500 rpm, and the shear stirring temperature is 158±3℃; the time is 15 minutes to return the vulcanized rubber to its original state. Then, convey the material to the heat preservation return machine, the temperature of the heat preservation return machine is 158±3℃, and nitrogen is introduced at the same time, with a nitrogen flow rate of 12m 3 / h for heat preservation and return to the original state; there is stirring in the heat preservation and return to the original state machine, stirring at 15 revolutions / h. The whole time is 3 hours; after 3 hours, the material is transported to the ventilation water jacket cooler, and nitrogen is introduced into the cooler at a nitrogen flow rate of 24m 3 / h. When the material in the cooler reaches 60℃, the material is discharged and sent to the high shear force refiner for refining once, and then to the next refining. A total of 5 times of refining can achieve the desired product, and then the product is packaged and weighed as the finished product. The finished product is inspected according to the national standard of "Recycled Rubber", see the table below.

[0079] Table 1 Example product performance

[0080]

[0081]

[0082] The results show that the products of the embodiments all meet the national standards.

[0083] The raw materials used in the present invention are all environmentally friendly materials.

[0084] The process used in the present invention is slightly higher than the rubber vulcanization temperature, produces less cracking reaction, and is beneficial to environmental protection.

[0085] The recycled rubber production equipment used in the present invention, such as a shearing mixer, a heat preservation reduction machine with nitrogen, a cooling machine with nitrogen, and a high shear force refining machine. All of them are easy to process equipment; the equipment has a simple structure, is easy to maintain, and the overall production line price is low. Compared with the existing technology for producing recycled rubber equipment; such as multi-stage screw extruder equipment for producing recycled rubber, twin-screw extruder equipment for producing recycled rubber, single-screw extruder equipment for producing recycled rubber, conical screw extruder equipment for producing recycled rubber, mechanical chemical activation machine equipment for producing recycled rubber, grinding machine equipment for producing recycled rubber, etc., the physical and mechanical properties of the processed and manufactured recycled rubber products are equivalent to those of the equipment, and all meet the national technical indicators and quality standards for recycled rubber.

[0086] The preferred specific implementation modes and embodiments of the present invention are described in detail above, but the present invention is not limited to the above implementation modes and embodiments, and various changes can be made within the knowledge scope of those skilled in the art without departing from the concept of the present invention.

Claims

1. A reclaimed rubber, characterized in that: The raw materials for the preparation include vulcanized rubber powder, vegetable oil, pine tar, rosin and additives; Preferably, the raw material for preparing the vulcanized rubber powder is waste tires or other rubber products; Preferably, the vegetable oil is at least one of soybean oil, palm oil, rapeseed oil, sunflower oil, coconut oil, olive oil, linseed oil, castor oil, cottonseed oil, rice bran oil, peanut oil and sesame oil and epoxidation products thereof; more preferably epoxidized soybean oil.

2. The reclaimed rubber according to claim 1, characterized in that: The auxiliary agents include antioxidants and accelerators; Preferably, the antioxidant is at least one of antioxidant 4020, antioxidant 4010, antioxidant 4010NA, antioxidant 4030 and antioxidant RD; Preferably, the accelerator is at least one of accelerator M, accelerator DM and accelerator TMTD.

3. The reclaimed rubber according to claim 1 or 2, characterized in that: The raw materials for preparation include: 100 parts by weight of vulcanized rubber powder; 1-18 parts by weight of vegetable oil; 1-6 parts by weight of rosin; 3-18 parts by weight of pine tar; 1-4 parts by weight of antioxidant; 1-4 parts by weight of accelerator; Preferably, the mesh number of the vulcanized rubber powder is not less than 20.

4. A method for preparing recycled rubber, characterized in that: The following steps are involved: S01, raw material mixing; S02, shear stirring; S03, return to the original state under inert gas insulation; S04, cooling under inert gas; S06, refining until the viscosity is acceptable, and then cutting into slices; and optional, S07, package.

5. The preparation method according to claim 4, characterized in that: In S02, the shear stirring temperature is lower than 180°C, preferably lower than 173°C.

6. The preparation method according to claim 4 or 5, characterized in that: In S03, the temperature of the heat preservation and returning to the original state is lower than 180°C, preferably lower than 173°C.

7. The preparation method according to any one of claims 4 to 6, characterized in that: In S04, cool to 55-65°C.

8. The preparation method according to any one of claims 4 to 7, characterized in that: In S05, during the refining, the speed ratio of the front and rear rollers is 1; 1.45-2.

0.

9. The preparation method according to any one of claims 4 to 8, characterized in that: In S05, during the refining, the roller temperature does not exceed 80±3°C.

10. The preparation method according to any one of claims 4 to 9, characterized in that: In S05, refine 4-6 times.