Heterophase polypropylene cable insulating material and preparation method thereof

By adding main and auxiliary antioxidants and nucleating agents to the polypropylene cable insulation material and extrusion processing with multi-component polypropylene cable material, the problem of breakdown of polypropylene insulation material at high temperature is solved and the cable is improved The insulation breakdown strength and reliability achieve a comprehensive assessment of cable reliability.

CN118978767APending Publication Date: 2024-11-19CHINA ELECTRIC POWER RESEARCH INSTITUTE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411032536.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19

Smart Images

  • Figure CN118978767A_ABST
    Figure CN118978767A_ABST
Patent Text Reader

Abstract

The invention discloses a heterogeneous polypropylene cable insulating material and a preparation method thereof, and belongs to the technical field of electrical equipment. The heterogeneous polypropylene cable insulating material is prepared from the following raw materials in parts by weight: 0.1 to 0.5 part of a main antioxidant, 0 to 0.2 part of an auxiliary antioxidant, 0.1 to 0.3 part of a nucleating agent and 99.0 to 99.8 parts of a polypropylene base material, the total weight parts of the raw materials of the heterophase polypropylene cable insulating material are 100. The insulation breakdown strength of the material is higher in the application process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrical equipment, and more specifically, to a multiphase polypropylene cable insulation material and a preparation method thereof. Background Art

[0002] Polypropylene insulation is currently the widely recognized development direction in the power cable industry. However, due to its poor toughness, it is difficult to bend after being used in power cables, and is prone to breakdown problems under AC voltage. In particular, the breakdown caused by structural deformation under high temperature is more critical, so the reliability of existing solutions is poor.

[0003] In order to improve the reliability of polypropylene insulation, the material system needs to be optimized. In addition, effective methods need to be used for testing. The existing material compression specimens are not sufficient to evaluate the insulation reliability of power cables. There are large differences in the electrical resistance of the samples and the cables. Summary of the invention

[0004] In view of the above problems, the present invention proposes a multiphase polypropylene cable insulation material, wherein the multiphase polypropylene cable insulation material comprises the following raw materials: 0.1-0.5 parts by weight of a primary antioxidant, 0-0.2 parts by weight of an auxiliary antioxidant, 0.1-0.3 parts by weight of a nucleating agent and 99.0-99.8 parts by weight of a polypropylene base material;

[0005] The total weight of the raw materials of the multiphase polypropylene cable insulation material is 100 parts by weight.

[0006] Optionally, the polypropylene base material is a multi-component polypropylene cable material.

[0007] Optionally, the multi-component polypropylene cable material includes: a polypropylene cable material with an elastomer content greater than 20% and a polypropylene cable material with a melting temperature greater than 150°C.

[0008] Optionally, the selection principles for polypropylene cable materials with an elastomer content greater than 20% and a melting temperature greater than 150°C include:

[0009] The melt flow rates of polypropylene cable materials with an elastomer content greater than 20% and a melting temperature greater than 150°C are similar.

[0010] Optionally, the proportion of each component of the multi-component polypropylene cable material is 10%-50%.

[0011] Optionally, the nucleating agent is a β-crystalline nucleating agent.

[0012] Optionally, the β-crystal nucleating agent includes at least one of the following: a condensed ring compound with a quasi-planar structure, an aliphatic dicarboxylate nucleating agent, a rare earth nucleating agent, an aromatic amine nucleating agent and a polymer nucleating agent.

[0013] On the other hand, the invention also proposes a method for preparing a multiphase polypropylene cable insulation material, comprising:

[0014] Introducing 0.1-0.5 parts by weight of a primary antioxidant, 0-0.2 parts by weight of an auxiliary antioxidant and 0.1-0.3 parts by weight of a nucleating agent into 99.0-99.8 parts by weight of a polypropylene base material to form a uniformly dispersed cable material;

[0015] The cable material is subjected to extrusion processing to obtain a multiphase polypropylene cable insulation material.

[0016] Optionally, a screw with a mixing structure is used to extrude the cable material. The screw with a mixing structure includes: Insulation extruder;

[0017] Said The temperature of the insulation extruder in sections 5 to 6 is 160 to 205°C, the extrusion speed is 3m / min to 11m / min, and the screw speed is 6rpm to 21rpm;

[0018] The increment of extrusion speed is: 0.5~2m / min.

[0019] Optionally, the cable material is subjected to extrusion processing, including: extruding the cable material onto a copper wire with a diameter of 5 to 10 mm.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The invention provides a multiphase polypropylene cable insulation material, which comprises the following raw materials: 0.1-0.5 parts by weight of a primary antioxidant, 0-0.2 parts by weight of an auxiliary antioxidant, 0.1-0.3 parts by weight of a nucleating agent and 99.0-99.8 parts by weight of a polypropylene base material; the total amount of the raw materials of the multiphase polypropylene cable insulation material is 100 parts by weight. The material of the invention has higher insulation breakdown strength during application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a connection circuit diagram of the cable breakdown test of the present invention;

[0023] Figure 2 The present invention is a flow chart of the preparation method. DETAILED DESCRIPTION

[0024] Now, exemplary embodiments of the present invention are described with reference to the accompanying drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. These embodiments are provided to disclose the present invention in detail and completely and to fully convey the scope of the present invention to those skilled in the art. The terms used in the exemplary embodiments shown in the accompanying drawings are not intended to limit the present invention. In the accompanying drawings, the same units / elements are marked with the same reference numerals.

[0025] Unless otherwise specified, the terms (including technical terms) used herein have the commonly understood meanings to those skilled in the art. In addition, it is understood that the terms defined in commonly used dictionaries should be understood to have the same meanings as those in the context of the relevant fields, and should not be understood as idealized or overly formal meanings.

[0026] Embodiment 1:

[0027] The present invention provides a multiphase polypropylene cable insulation material, which comprises the following raw materials: 0.1-0.5 parts by weight of a primary antioxidant, 0-0.2 parts by weight of an auxiliary antioxidant, 0.1-0.3 parts by weight of a nucleating agent and 99.0-99.8 parts by weight of a polypropylene base material;

[0028] The total weight of the raw materials of the multiphase polypropylene cable insulation material is 100 parts by weight.

[0029] Wherein, the polypropylene base material is a multi-component polypropylene cable material.

[0030] The multi-component polypropylene cable material includes: a polypropylene cable material with an elastomer content greater than 20% and a polypropylene cable material with a melting temperature greater than 150°C.

[0031] Among them, the selection principles for polypropylene cable materials with elastomer content greater than 20% and melting temperature greater than 150°C include:

[0032] The melt flow rates of polypropylene cable materials with an elastomer content greater than 20% and a melting temperature greater than 150°C are similar.

[0033] The proportion of each component of the multi-component polypropylene cable material is 10%-50%.

[0034] Wherein, the nucleating agent is a β-crystal nucleating agent.

[0035] The β-crystal nucleating agent includes at least one of the following: a condensed ring compound with a quasi-planar structure, a fatty dicarboxylate nucleating agent, a rare earth nucleating agent, an aromatic amine nucleating agent and a polymer nucleating agent.

[0036] The present invention is further described below in combination with specific implementation cases, preparation methods and verification processes:

[0037] The preparation process is as follows:

[0038] Step 1 is mixing: using multi-component polypropylene cable material, introducing antioxidants and nucleating agents, etc., to form a uniformly dispersed cable material;

[0039] Step 2 is the preparation of the model cable sample: a screw with a mixing structure is used for extrusion processing to form cable samples and sample cables. Step 3 is the electrical performance test: the sample cable is connected to a voltage generator and the voltage is gradually increased until a breakdown occurs. After testing multiple cables, data analysis is performed.

[0040] Preferably, mixing can be carried out during the extrusion process in step 2 to reduce the first step of mixing and sampling, but the material mixing system needs to be sufficiently uniform.

[0041] First, base material selection and compounding: Insulation materials are prepared using common polypropylene from different sources and processing aids.

[0042] The polypropylene base material is a two-component material, one of which has a higher elastomer content but a lower melting temperature, and the other is a homopolymer polypropylene with a lower elastomer content and a higher melting temperature. The selection principle requires that the melt flow rates of the two materials are close to ensure that the matrix after blending can be effectively compatible.

[0043] Preferably, the polypropylene with high elastomer content can be selected from brands K8303, T8002, SP179, EPC31, 1343. The polypropylene with high melting temperature can be selected from brands K1003, K1008, C1008, J700, J701, 4553, etc., but not limited to these brands. The two brands of cable materials are added in a ratio of 10% to 50%.

[0044] For example, 1343 and 4553 grades of polypropylene are both low melt index cable materials, with melt flow rates (MFR) of 9g / 10min and 7.2g / 10min respectively, which are suitable for use in power cable insulation compounds without compatibility issues. Two materials produced by Yanshan Petrochemical Company were selected and blended 50 / 50.

[0045] In order to prevent oxidative degradation of polypropylene materials during processing, antioxidants need to be introduced. The main brands of primary antioxidants are 330, 1010, 1076, 412S, and the main brands of secondary antioxidants are B215, BHT, and 225.

[0046] Preferably, Irganox 1010 and Chimasorb 944 are two antioxidant additives, which are added in a mass ratio of 0.2% and 0.1% respectively, wherein the former is used as a primary antioxidant and the latter is used as an auxiliary antioxidant.

[0047] β-crystal nucleating agents mainly include the following categories: condensed ring compounds with quasi-planar structures; fatty dicarboxylate nucleating agents; rare earth nucleating agents; aromatic amine nucleating agents. Polymer nucleating agents, etc. In order to ensure compatibility, this scheme selects a polymer-type commercially available β-nucleating agent, Dongguan Xinhua Plastic Raw Materials Co., Ltd., and adds 0.1-0.3% according to the proportion. Put it into the mixer and mix it evenly. The mixer is selected from Zhejiang Ruicheng Rubber and Plastic Machinery's ST-10L.

[0048] After mixing the above components, add them into the internal mixer (CF-2L): Dongguan Changfeng Rubber & Plastic Machinery Technology Co., Ltd. After extrusion, form a strip sample, and use a pelletizer to cut into pellets. The pelletizer is CT-5kg from Zhejiang Ruicheng Rubber & Plastic Machinery. If the mixer is uniform enough, the internal mixer and granulation step can be omitted and extrusion can be carried out directly on the extruder with a mixing device.

[0049] Secondly, polypropylene insulated cable samples were made by extruding the mixed materials onto copper wires with a diameter of 5 to 10 mm. The insulation extruder uses the SAT150 device with mixing produced by Jiangsu Yuesheng Technology Co., Ltd. The temperature of the 5th to 6th stage is 160-205℃. With the increase of the extrusion speed (from 3m / min to 11m / min in increments of 1m / min), the extruder current gradually increases steadily, and the screw speed gradually increases from 6rpm to 21rpm. The extrusion speed, extruder current and screw speed increase evenly, showing a trend of gradual increase. It is required that at different extrusion line speeds, the extruder current fluctuation is maintained within the range of ±2A, the extruder current is stable, and the outer diameter of the wire core fluctuates slightly. The conductor specifications of the polypropylene insulated cable produced by the above method range from 20mm2 to 75mm2, and the insulation thickness ranges from 1.2mm to 4.5mm. After gradually increasing the production speed to 4m / min, the screw speed basically guarantees a linear and stable increase, the outer diameter of the wire core fluctuates within 1mm, and the extruder current changes no more than 5A. For the selected wire sample, a semi-conductive polymer mesh can also be extruded on the top of the insulation layer as an electrode. A twin-screw extruder (SHJ-20) was used: Nanjing Jieente Electromechanical Co., Ltd.; an extrusion device with a mixing device.

[0050] Then, the extruded wire and cable samples were tested to simulate the field distribution in the real cable insulation and eliminate the need for the guard ring. The test mainly analyzed the breakdown performance. Using the modified HIGH VOLTAGE dielectric strength test device (cable breakdown test connection loop) Figure 1 As shown, an AC breakdown test was performed. A wire sample, typically 1 meter long, was immersed in a glass water bath. The conductor of the wire acted as one electrode and the water as the other. The system is capable of providing up to 75 kV AC voltage and 4 mA trigger-off AC current. In order to track any possible electrical aging effects, the test was repeated at three ramp rates: 0.5 kV / s, 2 kV / s and 5 kV / s. When recording the breakdown voltage, care was taken to distinguish between true dielectric breakdown and so-called arc crossing in the surrounding air and disconnection triggered by excessive AC current. Although the test configuration can be adjusted to avoid low-voltage arc crossings, the sample length must be reduced to limit the AC current to below the trigger-off current. In both cases, the apparent voltage is recorded as a "pause" in the Weibull analysis.

[0051] Finally, the data results are processed: the breakdown of polymer insulation materials is random, and the data is usually best analyzed within the framework of the Weibull distribution. If an apparently identical polymer insulation system is exposed to the same test in which the voltage increases linearly with time, a different breakdown voltage is usually observed for each insulation sample. The breakdown voltage obtained in this way can be characterized by a statistical distribution that describes the probability of breakdown as a function of voltage. According to the Weibull method, during a progressive stress test with a ramp rate of V·=dV / dt (rate of voltage increase), the failure probability PF(V) at a voltage V is given by the following formula:

[0052]

[0053] Where V C is the breakdown voltage at 63% probability (scale), and β is the trapezoidal shape parameter of the Weibull fit. The shape parameter and the characteristic breakdown voltage can be obtained by plotting the test results on Weibull probability paper.

[0054] The present invention blends two different grades of polypropylene resins, one of which has a high rubber phase content and a low modulus, and the other has a high melting point and a low rubber phase. When the two materials have similar flow melt indexes, they can be effectively compatible, thereby achieving system optimization, which can provide the high temperature requirements required by the power cable and meet the bending toughness requirements of the cable installation and laying;

[0055] The present invention can improve the resin system without adding the mixing and granulation process. After the material is mixed by a stirrer, a mixer is used to mix and extrude the material in the cabling process. This has great advantages in optimizing the process of cabling and can meet the development of power cables with different insulation performance requirements.

[0056] The present invention can avoid the limitations of traditional pressed sample testing and more comprehensively consider the process performance of cabling processing such as polypropylene insulation, including performing step-by-step voltage boosting breakdown on multiple cables and using Weibull distribution to process the results, so that the distribution of data and cabling reliability can be more effectively evaluated.

[0057] Polypropylene samples of different components were tested, and the prepared samples are shown in Table 1 below:

[0058] Table 1

[0059] Sample No. Homopolymer Copolymerization Primary Antioxidant Secondary antioxidant Insulation thickness Semiconducting S01 10 90 0.2 0.2 0.4 have S02 15 85 0.2 0.2 0.4 have S03 20 80 0.2 0.2 0.4 have S04 25 75 0.2 0.2 0.4 have S05 30 70 0.2 0.2 0.7 have S06 35 65 0.2 0.2 0.7 have S07 40 60 0.2 0.2 0.7 have S08 45 55 0.2 0.2 0.7 have S09 50 50 0.2 0.2 0.4 none S10 55 45 0.2 0.2 0.4 none S11 60 40 0.2 0.2 0.4 none S12 65 35 0.2 0.4 0.4 none S13 70 30 0.2 0.2 0.7 none S14 75 25 0.2 0.2 0.7 none S15 80 20 0.2 0.2 0.7 none S16 85 15 0.2 0.2 0.7 none

[0060] Through the breakdown test, the breakdown test was performed at a speed of 0.5kV / s and 2kV / s respectively. The test results are shown in Table 2 below:

[0061] Table 2

[0062]

[0063]

[0064] It can be seen from the test results that the breakdown voltage of S04 and S08 components is higher, which can meet the needs of power cable development and can be further screened and analyzed.

[0065] Embodiment 2:

[0066] The present invention also provides a method for preparing a multiphase polypropylene cable insulation material, such as Figure 2 As shown, including:

[0067] Step 1, introducing 0.1-0.5 parts by weight of a primary antioxidant, 0-0.2 parts by weight of an auxiliary antioxidant and 0.1-0.3 parts by weight of a nucleating agent into 99.0-99.8 parts by weight of a polypropylene base material to form a uniformly dispersed cable material;

[0068] Step 2: Extruding the cable material to obtain a multiphase polypropylene cable insulation material.

[0069] Among them, a screw with a mixing structure is used to extrude the cable material, and the screw with a mixing structure includes: Insulation extruder;

[0070] Said The temperature of the insulation extruder in sections 5 to 6 is 160 to 205°C, the extrusion speed is 3m / min to 11m / min, and the screw speed is 6rpm to 21rpm;

[0071] The increment of extrusion speed is: 0.5~2m / min.

[0072] The extrusion process of the cable material comprises: extruding the cable material onto a copper wire with a diameter of 5 to 10 mm.

[0073] The power cable obtained by the invention has higher insulation breakdown strength in engineering applications, and has important engineering significance for improving the reliability of polypropylene insulated power cables.

[0074] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0075] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A multiphase polypropylene cable insulation material, characterized in that: The multiphase polypropylene cable insulation material comprises the following raw materials: 0.1-0.5 parts by weight of a primary antioxidant, 0-0.2 parts by weight of an auxiliary antioxidant, 0.1-0.3 parts by weight of a nucleating agent and 99.0-99.8 parts by weight of a polypropylene base material; The total weight of the raw materials of the multiphase polypropylene cable insulation material is 100 parts by weight.

2. The multiphase polypropylene cable insulation material according to claim 1, characterized in that: The polypropylene base material is a multi-component polypropylene cable material.

3. The multiphase polypropylene cable insulation material according to claim 2, characterized in that: The multi-component polypropylene cable material comprises: a polypropylene cable material with an elastomer content greater than 20% and a polypropylene cable material with a melting temperature greater than 150°C.

4. The multiphase polypropylene cable insulation material according to claim 3, characterized in that: The selection principles of the polypropylene cable material with an elastomer content greater than 20% and the polypropylene cable material with a melting temperature greater than 150° C. include: The melt flow rates of polypropylene cable materials with an elastomer content greater than 20% and a melting temperature greater than 150°C are similar.

5. The multiphase polypropylene cable insulation material according to claim 2, characterized in that: The proportion of each component of the multi-component polypropylene cable material is 10%-50%.

6. The multiphase polypropylene cable insulation material according to claim 1, characterized in that: The nucleating agent is a β-crystal nucleating agent.

7. The multiphase polypropylene cable insulation material according to claim 6, characterized in that: The β-crystal nucleating agent includes at least one of the following: a condensed ring compound with a quasi-planar structure, a fatty dicarboxylate nucleating agent, a rare earth nucleating agent, an aromatic amine nucleating agent and a polymer nucleating agent.

8. A method for preparing a multiphase polypropylene cable insulation material, characterized in that: include: Introducing 0.1-0.5 parts by weight of a primary antioxidant, 0-0.2 parts by weight of an auxiliary antioxidant and 0.1-0.3 parts by weight of a nucleating agent into 99.0-99.8 parts by weight of a polypropylene base material to form a uniformly dispersed cable material; The cable material is subjected to extrusion processing to obtain a multiphase polypropylene cable insulation material.

9. The preparation method according to claim 8, characterized in that: The cable material is extruded by using a screw with a mixing structure, wherein the screw with a mixing structure comprises: a φ150 insulating extruder; The temperature of the φ150 insulation extruder in sections 5 to 6 is 160 to 205°C, the extrusion speed is 3m / min to 11m / min, and the screw speed is 6rpm to 21rpm; The increment of extrusion speed is: 0.5~2m / min.

10. The preparation method according to claim 8, characterized in that: The extrusion processing of the cable material comprises: extruding the cable material onto a copper wire with a diameter of 5 to 10 mm.