Preparation method of sun-proof nano titanium white color paste
By using a combination of chitosan modifier and nanosilicon dioxide regulator in nanotitanium white slurry, the problem of poor sun protection performance in the prior art is solved, the coordinated improvement of sun protection and hydrophobic properties is achieved, and the product is improved Overall performance.
Patent Information
- Application Number
- CN202410978366.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-19
AI Technical Summary
The existing nanotitanium white slurry has poor sun protection performance and is difficult to coordinate sun protection and hydrophobic properties, which limits the efficiency of the product.
Using a combination of nanotitanium dioxide pigment, chitosan modifier and nanosilica regulator, the sunscreen nanotitanium white slurry is prepared through stirring and ball milling, and the chitosan modifier and nanosilica regulator are coordinated. Effective, enhance sun protection and hydrophobic properties.
It significantly improves the sun protection and hydrophobic properties of the product, coordinates and improves the performance between the two, and improves the stability and interface activity of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium white slurry, and in particular to a method for preparing sunscreen nano titanium white slurry. Background Art
[0002] Color paste is a semi-finished product made of pigment or pigment and filler dispersed in paint. The one with pure oil as binder is called oily color paste. The one with resin paint as binder is called resin color paste. The color paste with water as medium and surfactant added to disperse the color filler is called water-based color paste.
[0003] The existing nano titanium white paste has poor sun protection performance. In order to improve the sun protection performance of the product, it is easy to cause the hydrophobicity of the product to deteriorate. It is difficult to achieve coordinated improvement of the sun protection and hydrophobicity of the product, which limits the use efficiency of the product. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a method for preparing a sunscreen nano titanium white slurry to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution: The present invention provides a method for preparing a sunscreen nano titanium white slurry, comprising the following steps: Weighing of raw materials: 35-45 parts of nano titanium dioxide pigment, 4-8 parts of chitosan modifier, 3-5 parts of nano silicon dioxide regulator; The raw materials are added into a mixer in sequence, blended thoroughly, and then ball-milled thoroughly. The ball-milling speed is 300 r / min and the ball-milling is performed for 2 hours to obtain a nano titanium white slurry for sunscreen.
[0006] Preferably, the preparation method of the chitosan modifier is: S01: adding a sodium silicate solution accounting for 10-15% of the total amount of the chitosan solution to a chitosan solution having a mass fraction of 5%, stirring and mixing, and then adding an yttrium nitrate solution accounting for 2-5% of the total amount of the chitosan solution, stirring and mixing to obtain a chitosan solution; S02: Immerse the glass fiber in a sufficient amount of 2% by mass hydrochloric acid solution and mix it thoroughly, then wash it with water and dry it. Stir the dried glass fiber and chitosan solution in a weight ratio of 2:5 to obtain a chitosan modifier.
[0007] Preferably, the mass fraction of the sodium silicate solution is 10-15%; the mass fraction of the yttrium nitrate solution is 2-4%.
[0008] Preferably, the preparation method of the nano silicon dioxide regulator is: S101: The bentonite is first heat treated at a temperature of 210-230°C for 10-15 minutes, then cooled to 55-60°C at a rate of 2-4°C / min, and heat-insulated; S102: adding 3-5 parts of nano-silicon dioxide, 2-4 parts of isopropyl triisostearoyl titanate, and 1-3 parts of hexadecyltrimethylammonium bromide to 6-10 parts of sodium citrate solution and stirring to obtain nano-silicon dioxide liquid; S103: subjecting the heat-insulated bentonite and nano-silicon dioxide liquid to ultrasonic modification treatment at a weight ratio of 2:5, and after the ultrasonic modification is completed, washing with water and drying to obtain a nano-silicon dioxide regulator.
[0009] Preferably, the mass fraction of the sodium citrate solution is 10-15%.
[0010] Preferably, the ultrasonic power of the ultrasonic modification treatment is 350-400W, and the ultrasonic time is 20-30min.
[0011] Preferably, the blending is fully stirred at a speed of 1350-1450 r / min for 65-75 min.
[0012] Compared with the prior art, the present invention has the following beneficial effects: The nano titanium white slurry of the present invention uses nano titanium white pigment as a matrix, and a chitosan modifier is coordinated with a nano silicon dioxide regulator. The two coordinate and work synergistically to enhance the sunscreen and hydrophobic properties of the product, and coordinate and improve the performance effects of the two. DETAILED DESCRIPTION
[0013] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0014] Example 1. A method for preparing a sunscreen nano titanium white slurry in this embodiment comprises the following steps: Weighing of raw materials: 35 parts of nano titanium dioxide pigment, 4 parts of chitosan modifier, 3 parts of nano silicon dioxide regulator; The raw materials are added into a mixer in sequence, blended thoroughly, and then ball-milled thoroughly. The ball-milling speed is 300 r / min and the ball-milling is performed for 2 hours to obtain a nano titanium white slurry for sunscreen.
[0015] The preparation method of the chitosan modifier of this embodiment is: S01: adding a sodium silicate solution accounting for 10% of the total amount of the chitosan solution to a chitosan solution having a mass fraction of 5%, stirring and mixing, and then adding an yttrium nitrate solution accounting for 2-5% of the total amount of the chitosan solution, stirring and mixing to obtain a chitosan solution; S02: Immerse the glass fiber in a sufficient amount of 2% by mass hydrochloric acid solution and mix it thoroughly, then wash it with water and dry it. Stir the dried glass fiber and chitosan solution in a weight ratio of 2:5 to obtain a chitosan modifier.
[0016] The mass fraction of the sodium silicate solution in this embodiment is 10%; the mass fraction of the yttrium nitrate solution is 2%.
[0017] The preparation method of the nano silicon dioxide regulator of this embodiment is: S101: The bentonite is first heat treated at 210°C for 10 min, then cooled to 55°C at a rate of 2°C / min, and heat-insulated; S102: adding 3 parts of nano-silicon dioxide, 2 parts of isopropyl triisostearoyl titanate, and 1 part of hexadecyltrimethylammonium bromide to 6 parts of sodium citrate solution and stirring to obtain nano-silicon dioxide liquid; S103: subjecting the heat-insulated bentonite and nano-silicon dioxide liquid to ultrasonic modification treatment at a weight ratio of 2:5, and after the ultrasonic modification is completed, washing with water and drying to obtain a nano-silicon dioxide regulator.
[0018] The mass fraction of the sodium citrate solution in this embodiment is 10%.
[0019] The ultrasonic power of the ultrasonic modification treatment in this embodiment is 350W, and the ultrasonic time is 20min.
[0020] The blending in this embodiment is fully stirred at a speed of 1350 r / min for 65 min.
[0021] Example 2. A method for preparing a sunscreen nano titanium white slurry in this embodiment comprises the following steps: Weighing of raw materials: 45 parts of nano titanium dioxide pigment, 8 parts of chitosan modifier, 5 parts of nano silicon dioxide regulator; The raw materials are added into a mixer in sequence, blended thoroughly, and then ball-milled thoroughly. The ball-milling speed is 300 r / min and the ball-milling is performed for 2 hours to obtain a nano titanium white slurry for sunscreen.
[0022] The preparation method of the chitosan modifier of this embodiment is: S01: adding a sodium silicate solution accounting for 15% of the total amount of the chitosan solution to a chitosan solution having a mass fraction of 5%, stirring and mixing, and then adding an yttrium nitrate solution accounting for 5% of the total amount of the chitosan solution, stirring and mixing to obtain a chitosan solution; S02: Immerse the glass fiber in a sufficient amount of 2% by mass hydrochloric acid solution and mix it thoroughly, then wash it with water and dry it. Stir the dried glass fiber and chitosan solution in a weight ratio of 2:5 to obtain a chitosan modifier.
[0023] The mass fraction of the sodium silicate solution in this embodiment is 15%; the mass fraction of the yttrium nitrate solution is 4%.
[0024] The preparation method of the nano silicon dioxide regulator of this embodiment is: S101: The bentonite is first heat treated at 230°C for 15 min, then cooled to 60°C at a rate of 4°C / min, and heat-treated; S102: adding 3 parts of nano-silicon dioxide, 2 parts of isopropyl triisostearoyl titanate, and 1 part of hexadecyltrimethylammonium bromide to 6 parts of sodium citrate solution and stirring to obtain nano-silicon dioxide liquid; S103: subjecting the heat-insulated bentonite and nano-silicon dioxide liquid to ultrasonic modification treatment at a weight ratio of 2:5, and after the ultrasonic modification is completed, washing with water and drying to obtain a nano-silicon dioxide regulator.
[0025] The mass fraction of the sodium citrate solution in this embodiment is 10%.
[0026] The ultrasonic power of the ultrasonic modification treatment in this embodiment is 350W, and the ultrasonic time is 20min.
[0027] The blending of this embodiment is fully stirred at a speed of 1450 r / min for 75 minutes.
[0028] Example 3. A method for preparing a sunscreen nano titanium white slurry in this embodiment comprises the following steps: Weighing of raw materials: 40 parts of nano titanium dioxide pigment, 6 parts of chitosan modifier, 4 parts of nano silicon dioxide regulator; The raw materials are added into a mixer in sequence, blended thoroughly, and then ball-milled thoroughly. The ball-milling speed is 300 r / min and the ball-milling is performed for 2 hours to obtain a nano titanium white slurry for sunscreen.
[0029] The preparation method of the chitosan modifier of this embodiment is: S01: adding a sodium silicate solution accounting for 12.5% of the total amount of the chitosan solution to a chitosan solution having a mass fraction of 5%, stirring and mixing, and then adding an yttrium nitrate solution accounting for 3.5% of the total amount of the chitosan solution, stirring and mixing to obtain a chitosan solution; S02: Immerse the glass fiber in a sufficient amount of 2% by mass hydrochloric acid solution and mix it thoroughly, then wash it with water and dry it. Stir the dried glass fiber and chitosan solution in a weight ratio of 2:5 to obtain a chitosan modifier.
[0030] The mass fraction of the sodium silicate solution in this embodiment is 12.5%; the mass fraction of the yttrium nitrate solution is 3%.
[0031] The preparation method of the nano silicon dioxide regulator of this embodiment is: S101: The bentonite is first heat treated at 220°C for 12 min, then cooled to 58°C at a rate of 3°C / min, and heat-insulated; S102: adding 4 parts of nano-silicon dioxide, 3 parts of isopropyl triisostearoyl titanate, and 2 parts of hexadecyltrimethylammonium bromide to 8 parts of sodium citrate solution and stirring to obtain nano-silicon dioxide liquid; S103: subjecting the heat-insulated bentonite and nano-silicon dioxide liquid to ultrasonic modification treatment at a weight ratio of 2:5, and after the ultrasonic modification is completed, washing with water and drying to obtain a nano-silicon dioxide regulator.
[0032] The mass fraction of the sodium citrate solution in this embodiment is 12.5%.
[0033] The ultrasonic power of the ultrasonic modification treatment in this embodiment is 370W, and the ultrasonic time is 25min.
[0034] A method for preparing a sunscreen nano titanium white slurry in this embodiment comprises the following steps: Chitosan modifier, silane coupling agent KH560, and nano-silica regulator raw materials are added to the mixer in sequence, and then nano-titanium dioxide pigment, acrylic resin, polyester resin, acetone solvent, phosphate buffer solution, and sodium metaphosphate are added and blended to obtain nano-titanium dioxide slurry for sunscreen.
[0035] The blending of this embodiment is fully stirred at a speed of 1400 r / min for 70 min.
[0036] Comparative Example 1. The difference from Example 3 is that no chitosan modifier is added.
[0037] Comparative Example 2. The difference from Example 3 is that no dry glass fiber is added in the preparation of the chitosan modifier.
[0038] Comparative Example 3. The difference from Example 3 is that no yttrium nitrate solution is added in the preparation of the chitosan modifier.
[0039] Comparative Example 4. The difference from Example 3 is that no nano silicon dioxide regulator is added.
[0040] Comparative Example 5. The difference from Example 3 is that no thermally-insulated bentonite is added in the preparation of the nano-silicon dioxide regulator.
[0041] Comparative Example 6. The difference from Example 3 is that no isopropyl triisostearyl titanate and cetyl trimethyl ammonium bromide are added to the nano-silicon dioxide liquid.
[0042] The nano titanium white slurry adopts nano titanium white pigment as a matrix, adds acrylic resin, polyester resin and acetone solvent, silane coupling agent KH560, phosphate buffer solution and sodium metaphosphate as raw material additives, and coordinates with a chitosan modifier to prepare a nano silicon dioxide regulator. The two coordinate and synergize to enhance the sunscreen and hydrophobic properties of the product, and coordinate and improve the performance effects of the two. The nano silicon dioxide regulator adopts bentonite that is heat-treated at a temperature of 210-230°C for 10-15min, and then cooled to 55-60°C at a rate of 2-4°C / min to optimize the bentonite flake layer The spacing is improved, the interface effect of the system raw materials and the interlaced system structure are improved, and the stability of the system is enhanced. Nano silica, isopropyl triisostearoyl titanate, hexadecyltrimethylammonium bromide and sodium citrate solution are coordinated and matched, so that the synergistic effect of the obtained nano silica liquid and bentonite is further enhanced. The distribution system is further combined with a chitosan modifier, and the chitosan solution, sodium silicate solution and yttrium nitrate in the chitosan modifier are combined to enhance the interfacial activity of the system. At the same time, the glass fiber is further reinforced to strengthen the system structure, so that the sun protection and hydrophobic properties of the product are further coordinated and improved.
[0043] The products of Examples 1-3 and Comparative Examples 1-6 were subjected to performance tests; The products of Examples 1-3 and Comparative Examples 1-6 were placed under sunlight for 10 days and immersed in water for 48 hours. At the same time, 27 parts of acrylic resin, 12 parts of polyester resin, 28 parts of acetone solvent, 6 parts of chitosan modifier, and 4 parts of silane coupling agent KH560 were blended to form a test product. The performance test of color difference under sunlight and immersion conditions was as follows:
[0044] It can be seen from Comparative Examples 1-6 and Examples 1-3 that; The product of Example 3 still has stable color difference performance under sunlight and water immersion conditions. At the same time, no chitosan modifier and no nano-silicon dioxide regulator are added, and the performance of the product shows a significant trend of deterioration. The two are used in combination and synergistically, and the performance effect of the product is the most significant; When no dry glass fiber is added in the preparation of the chitosan modifier, no yttrium nitrate solution is added in the preparation of the chitosan modifier, no thermal insulation treated bentonite is added in the preparation of the nano-silica regulator, and no isopropyl triisostearyl titanate and hexadecyltrimethylammonium bromide are added to the nano-silica liquid, the performance of the products tends to deteriorate. The chitosan modifier and nano-silica regulator prepared by the method of the present invention have the most significant performance effect.
[0045] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0046] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a sunscreen nano titanium white slurry, characterized in that: The following steps are involved: Weighing of raw materials: 35-45 parts of nano titanium dioxide pigment, 4-8 parts of chitosan modifier, 3-5 parts of nano silicon dioxide regulator; The raw materials are added into a mixer in sequence, blended sufficiently, and then ball-milled sufficiently to obtain a nano titanium white slurry for sun protection.
2. The method for preparing a sunscreen nano titanium white slurry according to claim 1, characterized in that: The preparation method of the chitosan modifier is: S01: adding a sodium silicate solution accounting for 10-15% of the total amount of the chitosan solution to a chitosan solution having a mass fraction of 5%, stirring and mixing, and then adding an yttrium nitrate solution accounting for 2-5% of the total amount of the chitosan solution, stirring and mixing to obtain a chitosan solution; S02: Immerse the glass fiber in a sufficient amount of 2% by mass hydrochloric acid solution and mix it thoroughly, then wash it with water and dry it. Stir the dried glass fiber and chitosan solution in a weight ratio of 2:5 to obtain a chitosan modifier.
3. The method for preparing a sunscreen nano titanium white slurry according to claim 1, characterized in that: The mass fraction of the sodium silicate solution is 10-15%; the mass fraction of the yttrium nitrate solution is 2-4%.
4. The method for preparing a sunscreen nano titanium white slurry according to claim 1, characterized in that: The preparation method of the nano silicon dioxide regulator is: S101: The bentonite is first heat treated at a temperature of 210-230°C for 10-15 minutes, then cooled to 55-60°C at a rate of 2-4°C / min, and heat-insulated; S102: adding 3-5 parts of nano-silicon dioxide, 2-4 parts of isopropyl triisostearoyl titanate, and 1-3 parts of hexadecyltrimethylammonium bromide to 6-10 parts of sodium citrate solution and stirring to obtain nano-silicon dioxide liquid; S103: subjecting the heat-insulated bentonite and nano-silicon dioxide liquid to ultrasonic modification treatment at a weight ratio of 2:5, and after the ultrasonic modification is completed, washing with water and drying to obtain a nano-silicon dioxide regulator.
5. The method for preparing a sunscreen nano titanium white slurry according to claim 4, characterized in that: The mass fraction of the sodium citrate solution is 10-15%.
6. The method for preparing a sunscreen nano titanium white slurry according to claim 4, characterized in that: The ultrasonic power of the ultrasonic modification treatment is 350-400W, and the ultrasonic time is 20-30min.