Design method for double-arc hole pattern of hot-rolled round rod
Through the double arc hole design method, the problem of insufficient control of the width direction of the material type in traditional design is solved, the stability of the finished product size and high pass rate are achieved, and the incidence of unqualified products is reduced.
Patent Information
- Application Number
- CN202410976276.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-20
- Publication Date
- 2024-11-19
AI Technical Summary
The traditional large sidewall arc hole design has the width direction control of the material type and the insufficient wrapping of the finished product size in the production of rolled steel rods, resulting in the occurrence of unqualified products, especially the non-roundness exceeding the standard, the diameter exceeding the standard and the ear problems. .
The double arc hole type design method is adopted, and the calculation formula of setting the hole type height and width is combined with the hole type expansion angle and notch design to form a double arc hole type to ensure the dimensional stability of the finished product width direction and pass through the bottom of the groove The coordination between the base circle and the hole expansion angle is designed to tangent the arc to improve the accuracy of the hole design.
It effectively reduces the incidence of unqualified products such as non-roundness exceeding the standard, diameter exceeding the standard and ears, and the rolling pass rate reaches more than 99.99%, meeting the production and manufacturing needs.
Smart Images

Figure CN118981843A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel rolling technology, in particular to a double arc hole design method for hot-rolled round bars. Background Art
[0002] In the production of rolled steel bars, round steel is one of the main products. The main defects of round steel include excessive diameter, ears and out-of-roundness. The hot-rolled round bar series hole design has long adopted the traditional large sidewall arc hole design method. This method has certain limitations on the width direction control of the material and the finished product size wrapping. The material is prone to overfilling during the production process, which leads to defective products. In order to better control the material shape and improve the wrapping of the hole shape on the finished product size, it is urgently needed to provide a hot-rolled round bar double arc hole design method to better solve the hole design problem for round bars. Summary of the invention
[0003] In order to solve the above problems, the present invention provides a double arc hole design method, which adopts the width direction dimension of the finished product to be stably controlled, and the defective products such as excessive out-of-roundness, excessive diameter and ears are greatly reduced, and the rolling qualification rate reaches more than 99.99%, which can better meet the production and manufacturing needs.
[0004] The technical solution adopted by the present invention is:
[0005] A method for designing a double arc pass profile for hot-rolled round bars comprises the following steps:
[0006] S1. Set basic parameters;
[0007] S2. The calculation formula for the design hole height h is: h = thermal expansion coefficient × (nominal size of round steel - 0.9 × minimum negative deviation allowed by national standards);
[0008] S3. The calculation formula for the design hole width w is: w = thermal expansion coefficient × (nominal size of round steel + 0.7 × maximum positive deviation allowed by national standards);
[0009] S4, set the hole profile roll gap s = 2mm, the hole profile expansion angle θ = 30°;
[0010] S5, the radius is represented by R1, in the two-dimensional coordinate system, make a hole base circle C1 with h=2R, make a hole expansion angle θ along the center of the circle and draw a line l1, the intersection of l1 and the hole base circle C1 is point P, continue to operate on the base circle, make a straight line l2 with a value of 1 / 2 times s parallel to the x-axis, make a straight line l3 with a value of 1 / 2 times w parallel to the y-axis, at this time l2 and l3 intersect at point Q, connect PQ to generate a line segment, set the midpoint of PQ as point G, and make a perpendicular line l4 to the line segment PQ along point G, at this time l4 and l1 intersect at point H, take point H as the center of the circle, HP (or HQ) as the radius to draw a circle C2, the radius of C2 is R2, leave the arc corresponding to the chord PQ segment, delete the rest of the arcs, set the notch fillet to r=1~1.5mm (designed to be 1mm, it can be enlarged to 1.5mm according to the production of the finished product), and complete the other parts of the hole;
[0011] S6. After the design of different round bar specifications is completed, the production will process and assemble the rollers according to the hole pattern drawings, and then put them on the rolling line to produce round bars.
[0012] Furthermore, in step S1, the basic parameters include the nominal size of the round steel. Specifically, the size (1) is implemented according to the third group of standards in "Table 1 Allowable deviations of the dimensions of hot-rolled round steel and square steel" in accordance with the national standard "GB / T702-2017 Hot-rolled steel bar dimensions, shape, weight and allowable deviations".
[0013] Furthermore, in step S2, the thermal expansion coefficient is a practical experience value, and a value in the range of 1.007 to 1.03 is selected when designing the pass according to the rolling process, rolling specifications and supply requirements.
[0014] Furthermore, in step S2, the designed hole height is also the diameter of the hole base circle.
[0015] Furthermore, in step S3, the thermal expansion coefficient is a practical experience value, and a value in the range of 1.007 to 1.03 is selected during the hole design according to the rolling process, rolling specifications and supply requirements.
[0016] The beneficial effects of the present invention are as follows:
[0017] The double arc hole design method for hot-rolled round bars provided by the present invention comprises the following steps: S1, setting basic parameters; S2, designing a calculation formula for hole height h, where h=thermal expansion coefficient×(nominal size of round steel-0.9×minimum negative deviation allowed by national standard); S3, designing a calculation formula for hole width w, where w=thermal expansion coefficient×(nominal size of round steel+0.7×maximum positive deviation allowed by national standard); S4, setting hole roll gap s=2mm, hole expansion angle θ=30°; S5, the radius is represented by R1, a hole base circle C1 with h=2R is made in a two-dimensional coordinate system, a line l1 is made along the center of the circle with the hole expansion angle θ, the intersection of l1 and hole base circle C1 is point P, and the operation is continued on the base circle, and a 1 / 2 times s value is made parallel to x The straight line l2 of the axis is made into a straight line l3 with a value of 1 / 2 times w and parallel to the y-axis. At this time, l2 and l3 intersect at point Q. Connect PQ to generate a line segment. Let the midpoint of PQ be point G. Draw a perpendicular line l4 to the line segment PQ along point G. At this time, l4 and l1 intersect at point H. Take point H as the center and HP (or HQ) as the radius to draw a circle C2. The radius of C2 is R2. Leave the arc corresponding to the chord PQ segment, delete the rest of the arcs, set the notch radius to r = 1 ~ 1.5mm (designed to be 1mm, which can be enlarged to 1.5mm according to the production of finished products), and complete the other parts of the hole type; S6, after the design is completed according to different round bar specifications, the production will process and assemble the rollers according to the hole type drawings, and then put them on the rolling line for round bar production. Compared with the traditional large sidewall arc hole type, the present application utilizes the groove bottom base circle and the hole expansion angle, and designs another arc through the expansion angle and the groove width, and the arcs at both ends are tangent to form a double arc hole design method. This hole type has been applied in the production practice of hot-rolled round bar series products. The width direction size of the finished product is stably controlled, and the defective products such as excessive out-of-roundness, excessive diameter and ears are greatly reduced. The rolling qualification rate reaches more than 99.99%, which can better meet the production and manufacturing needs. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a design drawing of a double arc hole for hot-rolled round bars of the present invention. DETAILED DESCRIPTION
[0019] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively by way of examples, and preferred embodiments of the present invention are given below. However, the present invention can be implemented in a variety of different forms and is not limited to the embodiments described herein. Any other implementation schemes obtained by modifying or equivalently replacing the technical scheme of the present invention without creative results are within the protection scope of the present invention.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for describing specific embodiments and are not intended to limit the present invention.
[0021] The numerical values disclosed in the embodiments of the present invention are approximate values, not definite values. When the error or experimental conditions permit, all values within the error range may be included without being limited to the specific numerical values disclosed in the embodiments of the present invention.
[0022] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0023] Example 1
[0024] This embodiment takes the finished pass of a φ20mm hot-rolled round bar as an example to design a double arc pass. The specific steps are as follows:
[0025] S1. Set basic parameters, including the nominal size of round steel, and implement the third group standard of "Table 1 Allowable deviation of hot-rolled round steel and square steel size" as ±0.4mm according to the national standard "GB / T702-2017 Hot-rolled steel bar size, shape, weight and allowable deviation";
[0026] S2. The calculation formula for the design hole height h is based on production experience and data research: h = thermal expansion coefficient × (nominal size of round steel - 0.9 × minimum negative deviation allowed by national standard), where the thermal expansion coefficient is a practical experience value. A value in the range of 1.007 to 1.03 is selected for hole design. Since hot-rolled round bars are delivered by actual weight, the general size control is positive deviation. The thermal expansion coefficient uses the maximum value of 1.03 this time, that is, h = 1.03 × (20-0.9 × 0.4) = 20.23 mm (also the diameter of C1 is 20.23 mm);
[0027] S3. The calculation formula for the design hole width w is based on production experience and data research: w = thermal expansion coefficient × (nominal size of round steel + 0.7 × maximum positive deviation allowed by national standards), where the thermal expansion coefficient is a practical experience value. A value in the range of 1.007 to 1.03 is selected for hole design. Since hot-rolled round bars are delivered by actual weight, the general size control is positive deviation. Combined with the aspect ratio size control and hole design principles, the thermal expansion coefficient is selected as 1.025 this time, that is, w = 1.025 × (20 + 0.7 × 0.4) = 20.78 mm;
[0028] S4, set the hole profile roll gap s = 2mm, the hole profile expansion angle θ = 30°;
[0029] S5, the radius is represented by R1, draw the double hole type, the specific steps are as follows:
[0030] 1) Make a hole base circle C1 with a length of h=2R in a two-dimensional coordinate system, make a hole expansion angle θ along the center of the circle and draw a line l1. The intersection of l1 and the hole base circle C1 is point P;
[0031] 2) Continue to operate on the base circle, make a straight line l2 with a value of 1 / 2 times s parallel to the x-axis, and make a straight line l3 with a value of 1 / 2 times w parallel to the y-axis. At this time, l2 and l3 intersect at point Q;
[0032] 3) Connect PQ to generate line segments;
[0033] 4) Let the midpoint of PQ be point G, and draw a perpendicular line l4 to the line segment PQ along point G. At this time, l4 intersects l1 at point H;
[0034] 5) Draw a circle C2 with point H as the center and HP (or HQ) as the radius, then the radius of C2 is R2 = 24.11 mm;
[0035] 6) Keep the arc corresponding to the chord PQ segment and delete the rest of the arcs;
[0036] 7) Set the notch radius to r = 1.5 mm (designed to be 1.5 mm to avoid ears on small sizes).
[0037] 8) Complete the other parts of the hole pattern and the hole pattern design is completed. The design process is as follows: Figure 1 :
[0038] S6. After the design of different round bar specifications is completed, the production will process and assemble the rollers according to the hole pattern drawings, and then put them on the rolling line to produce round bars. Specifically, after the hole pattern design is completed, it is necessary to roll on the line to verify the effect of the hole pattern:
[0039] 1) Hole processing and machine preparation
[0040] The production planning department sends the designed φ20mm double arc finished pass to the production preparation area. The machining team in the production preparation area designs the CNC machining program and processes a set of rolls with this pass. After the machining is completed, it is handed over to the rolling mill assembly team for roll assembly. After the assembly is completed, it is handed over to the rolling line, where the rolling mill workers adjust the rolling mill and the rolling line is put into trial rolling after the adjustment.
[0041] 2) Φ20mm round bar rolling
[0042] ① Select 165mm*165mm*12000mm continuous casting billet and heat it to 1140℃ to 1160℃ in a heating furnace.
[0043] ② After heating is completed, the steel is taken out of the furnace and rolled. During the rolling process, the rolling workers use calipers and wooden samples to control the process.
[0044] ③ After 16 rolling passes, the sampler takes samples on the cooling bed to observe the surface condition of the finished product.
[0045] The size and appearance of the Φ20mm finished product are summarized in Table 1:
[0046] Table 1 φ20mm finished product dimensions and appearance
[0047]
[0048]
[0049] Implementation Case 2
[0050] This embodiment takes the φ38mm hot-rolled round bar finished product pass profile as an example to design a double arc pass profile, and the steps are as follows:
[0051] S1. Set basic parameters, including the nominal size of round steel, and implement the third group standard of "Table 1 Allowable deviation of hot-rolled round steel and square steel size" as ±0.6mm according to the national standard "GB / T702-2017 Hot-rolled steel bar size, shape, weight and allowable deviation";
[0052] S2. The calculation formula for the design hole height h is based on production experience and data research: h = thermal expansion coefficient × (nominal size of round steel - 0.9 × minimum negative deviation allowed by national standard), where the thermal expansion coefficient is a practical experience value. A value in the range of 1.007 to 1.03 is selected for hole design. Since hot-rolled round bars are delivered in actual weight, the general size control is positive deviation. The thermal expansion coefficient uses the maximum value of 1.03 this time, that is, h = 1.03 × (38-0.9 × 0.6) = 38.58 mm (also the diameter of C1 is 38.58 mm);
[0053] S3. The calculation formula for the design hole width w is based on production experience and data research: w = thermal expansion coefficient × (nominal size of round steel + 0.7 × maximum positive deviation allowed by national standards), where the thermal expansion coefficient is a practical experience value. Since the hot-rolled round bars are delivered by actual weight, the general size control is positive deviation. Combined with the aspect ratio size control and hole design principles, the thermal expansion coefficient uses the maximum value of 1.016, that is, w = 1.016 × (38 + 0.7 × 0.6) = 39.03mm;
[0054] S4, set the hole profile roll gap s = 2mm, the hole profile expansion angle θ = 30°;
[0055] S5, the radius is represented by R1, draw the double hole type, the specific steps are as follows:
[0056] 1) Make a hole base circle C1 with a length of h=2R in a two-dimensional coordinate system, make a hole expansion angle θ along the center of the circle and draw a line l1. The intersection of l1 and the hole base circle C1 is point P;
[0057] 2) Continue to operate on the base circle, make a straight line l2 with a value of 1 / 2 times s parallel to the x-axis, and make a straight line l3 with a value of 1 / 2 times w parallel to the y-axis. At this time, l2 and l3 intersect at point Q;
[0058] 3) Connect PQ to generate line segments;
[0059] 4) Let the midpoint of PQ be point G, and draw a perpendicular line l4 to the line segment PQ along point G. At this time, l4 intersects l1 at point H;
[0060] 5) Draw a circle C2 with point H as the center and HP (or HQ) as the radius, then the radius of C2 is R2 = 24.11 mm;
[0061] 6) Keep the arc corresponding to the chord PQ segment and delete the rest of the arcs;
[0062] 7) Set the notch radius to r = 1 mm (designed to 1 mm, which can be enlarged to 1.5 mm depending on the finished product).
[0063] 8) Complete the other parts of the hole pattern and the hole pattern design is completed. The design process is as follows: Figure 1 :
[0064] S6. After the design of different round bar specifications is completed, the production will process and assemble the rollers according to the hole pattern drawings, and then put them on the rolling line to produce round bars. Specifically, after the hole pattern design is completed, it is necessary to roll on the line to verify the effect of the hole pattern:
[0065] 1) Hole processing and machine preparation
[0066] The production planning department sends the designed φ38mm double arc finished pass to the production preparation area. The machining team in the production preparation area designs the CNC machining program and then processes a set of rolls with this pass. After the machining is completed, it is handed over to the rolling mill assembly team for roll assembly. After the assembly is completed, it is handed over to the rolling line, where the rolling mill workers adjust the rolling mill and the rolling mill is put on line for trial rolling after the adjustment.
[0067] 2)φ38mm round bar rolling
[0068] ①Select 165mm*165mm*12000mm continuous casting billet and heat it to 1140℃ to 1160℃ in a heating furnace;
[0069] ② After heating, the steel is taken out of the furnace for rolling. During the rolling process, the rolling workers use calipers and wooden samples to control the process;
[0070] ③ After 12 rolling passes, the sampler takes samples on the cooling bed to observe the surface condition of the finished product.
[0071] The size and appearance of the Φ38mm finished product are summarized in Table 2:
[0072] Table 2 φ38mm finished product dimensions and appearance
[0073]
[0074]
[0075] In summary, referring to the finished size and appearance of the φ20mm and φ38mm round bars in the above embodiments 1-2, it can be seen that the present application utilizes the groove bottom base circle and the hole expansion angle, and designs a circular arc with the expansion angle and the groove width, and the arcs at both ends are tangent to form a double arc hole design method. The hole has been applied in the production practice of a series of hot-rolled round bars. The width direction size of the finished product is stably controlled, and the number of defective products such as excessive out-of-roundness, excessive diameter and ears is greatly reduced, and the rolling qualification rate reaches more than 99.99%.
[0076] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for designing a double arc pass for hot rolled round bars, characterized in that: The steps include: S1. Set basic parameters; S2. The calculation formula for the design hole height h is: h = thermal expansion coefficient × (nominal size of round steel - 0.9 × minimum negative deviation allowed by national standards); S3. The calculation formula for the design hole width w is: w = thermal expansion coefficient × (nominal size of round steel + 0.7 × maximum positive deviation allowed by national standards); S4, set the hole profile roll gap s = 2mm, the hole profile expansion angle θ = 30°; S5, the radius is represented by R1, in the two-dimensional coordinate system, make a hole base circle C1 with h=2R, make a hole expansion angle θ along the center of the circle and draw a line l1, the intersection of l1 and the hole base circle C1 is point P, continue to operate on the base circle, make a straight line l2 with a value of 1 / 2 times s parallel to the x-axis, make a straight line l3 with a value of 1 / 2 times w parallel to the y-axis, at this time l2 and l3 intersect at point Q, connect PQ to generate a line segment, set the midpoint of PQ as point G, and make a perpendicular line l4 to the line segment PQ along point G, at this time l4 and l1 intersect at point H, take point H as the center of the circle, and draw a circle C2 with HP (or HQ) as the radius, the radius of C2 is R2, keep the arc corresponding to the chord PQ segment, delete the rest of the arcs, set the notch fillet to r=1~1.5mm, and complete the other parts of the hole; S6. After the design of different round bar specifications is completed, the production will process and assemble the rollers according to the hole pattern drawings, and then put them on the rolling line to produce round bars.
2. The method for designing a double arc pass for hot rolled round bars according to claim 1, characterized in that: In step S1, the basic parameters include the nominal size of the round steel.
3. The method for designing a double arc pass for hot rolled round bars according to claim 1, characterized in that: In step S2, the thermal expansion coefficient is a practical experience value, and a value in the range of 1.007 to 1.03 is selected when designing the pass according to the rolling process, rolling specifications and supply requirements.
4. The method for designing a double arc pass for hot rolled round bars according to claim 1, characterized in that: In step S2, the designed hole height is also the diameter of the hole base circle.
5. The method for designing double arc pass of hot rolled round bar according to claim 1, characterized in that: In step S3, the thermal expansion coefficient is a practical experience value, and a value in the range of 1.007 to 1.03 is selected during the hole design according to the rolling process, rolling specifications and supply requirements.