Method for adjusting titanium content in molten iron

By controlling the titanium content in the furnace and adjusting the operating parameters, the problem of difficult control of the content of titanium element entering the molten iron in the blast furnace is solved, and the titanium content in the molten iron is significantly reduced and stable, meeting the requirements of the subsequent process.

CN118996027APending Publication Date: 2024-11-22BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129490.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the blast furnace operation, the content of titanium element entering molten iron is difficult to effectively control, resulting in excessive titanium element content in some steel grades, affecting the requirements of the subsequent process.

Method used

By controlling the titanium content in the furnace and adjusting the operating parameters, determine the distribution ratio of titanium elements between the slag and molten iron, calculate the upper limit of the titanium content allowed to enter the blast furnace, select the appropriate raw material supplier, and adjust the entry time of low titanium iron materials and smelting parameters to inhibit the reduction of titanium into the iron.

Benefits of technology

There is no need to add new equipment or investment to reduce the titanium content in molten iron, meet the requirements for the titanium content of molten iron during the subsequent process, and achieve a significant reduction and stability of the titanium content of molten iron.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996027A_ABST
    Figure CN118996027A_ABST
Patent Text Reader

Abstract

The invention discloses a method for adjusting the titanium content in molten iron, which comprises the following steps: performing correlation analysis on production parameters and the titanium content in the molten iron to obtain operation parameters with higher correlation with the titanium content in the molten iron, determining the distribution relation of titanium in slag and the molten iron under normal operation parameters, and adjusting the titanium content in the molten iron by determining the distribution relation. Calculating the upper limit value of the titanium content brought in by the furnace charge, determining the upper limit of the titanium content of the iron material needing to be adjusted according to the adjustment timeliness and the difficulty degree, and determining the upper limit of the titanium content of the iron ore concentrate for manufacturing the iron-containing material according to the upper limit value of the titanium content of the iron-containing material; and controlling the low-titanium iron ore concentrate to enter a production process by utilizing punctual pulling according to a smelting time sequence, and smelting the low-titanium molten iron by adopting a mode of controlling the si content of the molten iron in cooperation with a blast furnace. The method has the advantages that extra equipment does not need to be added for out-of-furnace titanium removal, the Ti content of the molten iron is reduced only by means of selection of low-titanium resources and a punctualized pulling mode, and the equipment investment can be greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to a method for adjusting the titanium content in molten iron. Background Art

[0002] During the operation of the blast furnace, most of the titanium brought into the smelting raw materials enters the slag, and a small part is reduced into the molten iron. The refining of some steel grades is more sensitive to the titanium content in the molten iron, and requires molten iron with a much lower titanium content than normal. The distribution of titanium into the slag and molten iron is significantly affected by the total amount of titanium brought into the blast furnace (titanium load) and the molten iron SI. How to control the titanium entering the blast furnace and take measures to inhibit the reduction of titanium into the molten iron so that the titanium content entering the molten iron is greatly reduced, thereby meeting the requirements of the subsequent process for the titanium content of the molten iron is the main problem to be solved by this method. Summary of the invention

[0003] The object of the present invention is to provide a method for effectively reducing the titanium content of molten iron by controlling the titanium content entering the furnace and adjusting operating parameters during the operation of the blast furnace.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention provides a method for adjusting the titanium content in molten iron, comprising the following steps:

[0006] 1) Determine the relationship between the Ti content in molten iron and the total amount of titanium entering the blast furnace;

[0007] 2) Determine the distribution ratio of titanium in slag and molten iron under daily operating parameters;

[0008] 3) calculating the upper limit of the titanium content allowed to be brought into the iron material entering the blast furnace by using the upper limit of the titanium content in the molten iron and the distribution coefficient of the titanium element between the slag and the molten iron determined in the previous step;

[0009] 4) Determine the iron material that needs to reduce titanium content based on the difficulty and timeliness of iron material adjustment;

[0010] 5) calculating the upper limit of the titanium content of the iron material that needs to adjust the titanium content according to the upper limit of the titanium content entering the blast furnace;

[0011] 6) Determine the upper limit of the Ti content of the raw material with large Ti fluctuations through the upper limit of the titanium content of the finished iron material, and select a suitable raw material supplier; use the iron concentrate with titanium content that meets the requirements supplied by the raw material supplier to produce iron materials with titanium content that meets the requirements;

[0012] 7) Determine the time when the low-titanium iron material enters the blast furnace tank according to the time of receiving the low-titanium iron water and the blast furnace smelting cycle combined with the blast furnace iron material tank storage;

[0013] 8) After the low-titanium ferromaterial enters the blast furnace, the smelting parameters are adjusted to inhibit the reduction of titanium into the molten iron, thereby significantly reducing the titanium content of the molten iron.

[0014] Furthermore, the step 1) specifically includes:

[0015] Statistics are taken on the titanium load entering the blast furnace and the average titanium content of molten iron in the blast furnace operation data. Statistics are taken from the lowest to the highest value of the titanium load with a step size of 1. All molten iron components within the corresponding interval with the titanium load are averaged and placed in the "average value item: molten iron Ti". The titanium content in molten iron is affected by the titanium load. The higher the titanium load, the higher the titanium content in molten iron. Therefore, to control the Ti content in molten iron, it is necessary to first control the total amount of Ti elements entering the blast furnace.

[0016] Furthermore, the step 2) specifically includes: defining the same batch output: Ti content in slag / Ti content in molten iron = titanium distribution coefficient, and statistically analyzing the titanium distribution coefficient under normal production conditions. The first quartile of the titanium distribution coefficient is 16.03, and the third quartile is 21.736, indicating that in the middle 50% of the cases least affected by abnormal conditions, the titanium distribution coefficient is between 16 and 22; in order to increase the success factor, the requirements for titanium content entering the furnace are tightened, and the distribution coefficient of 16 is taken for calculation, indicating that the Ti content in the slag is 16 times that in the molten iron.

[0017] Furthermore, in the step 4), the iron-containing raw materials used in the blast furnace are sintered and pelletized. Since the sintered ore has the problem of mixed ore pile and long material change time, the titanium content of the pellets is adjusted.

[0018] Furthermore, in the step 5), the upper limit of titanium content of a single batch of iron material entering the blast furnace minus the titanium content of a single batch of sintered ore = the upper limit of titanium content allowed to be brought into the pellets.

[0019] Furthermore, in step 7), since the time for sintering and converting the pellets into molten iron in the blast furnace is 6 hours and the blast furnace tank storage needs to consume 7 hours, it is required to manufacture the low-Ti pellets at least 13 hours in advance and transport them to the blast furnace raw material tank for loading.

[0020] Furthermore, in the step 8), a correlation analysis is performed on the components of Si and Ti in the molten iron, and it is found that the correlation coefficient between Si and Ti in the molten iron is relatively high and positively correlated. Therefore, after the low-titanium pellets enter the blast furnace, the blast furnace further refines the operating range to a lower operating range of 0.3-0.45 under the operating range of Si0.3-0.6, thereby further inhibiting Ti from being reduced and entering the molten iron.

[0021] Compared with the prior art, the beneficial technical effects of the present invention are:

[0022] The present invention provides a method for reducing the titanium content in molten iron by adjusting the titanium content of the iron material entering the furnace and the operating parameters during the normal operation of the blast furnace. The method does not require the addition of titanium removal equipment outside the furnace, does not require additional investment, and does not have the disadvantage that titanium removal outside the furnace will reduce the physical heat of molten iron. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The present invention will be further described below in conjunction with the accompanying drawings.

[0024] Figure 1 is the relationship between the Ti content in molten iron and the total Ti content entering the blast furnace, where the titanium load is the Ti content in the iron material required to smelt one ton of molten iron, kg / t;

[0025] Figure 2 Assign statistical results to Titanium;

[0026] Figure 3 It is a schematic diagram of the positive correlation between molten iron Si and molten iron Ti;

[0027] Figure 4 This is a diagram showing the effect of the control measures taken during the steelmaking process to produce silicon steel. DETAILED DESCRIPTION

[0028] In order to make the technical problems solved by the present invention, the technical solutions adopted and the technical effects achieved more clearly, the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0029] A method for adjusting the titanium content in molten iron, comprising:

[0030] Actual production situation: The titanium content of molten iron is required to be less than 0.100%. Each batch of ore contains 87010kg of sintered ore and 37290kg of pelletized ore; the Ti content of sintered ore is 0.16%; each batch of ore produces 69200kg of molten iron and 24289kg of slag. Pelletized ore ingredients: Ore type 1, proportion 46%, Ti content 0.16%; Ore type 2 proportion 1%, Ti content 0.18%; Ore type 3 proportion 53%;

[0031] 1) Determine the relationship between the Ti content in molten iron and the total Ti content entering the blast furnace.

[0032] Statistics are collected on the titanium load entering the blast furnace and the average titanium situation of molten iron in the blast furnace operation data (statistics are collected from the lowest value to the highest value of the titanium load with a step size of 1, and all molten iron components with titanium load falling within the corresponding interval are averaged and placed in the "average value item: molten iron Ti"), such as Figure 1 As shown, it can be seen that the titanium content in molten iron is affected by the titanium load. The higher the titanium load, the higher the titanium content in molten iron. Therefore, to control the Ti content in molten iron, it is necessary to first control the total amount of Ti elements entering the blast furnace.

[0033] 2) Determine the distribution ratio of titanium element in slag and molten iron.

[0034] Define the same batch output: Ti content in slag / Ti content in molten iron = titanium distribution coefficient. Statistical analysis of the titanium distribution coefficient under normal production conditions shows the following results: Figure 2 As shown, it can be seen that the first quartile of the titanium distribution coefficient is 16.03 and the third quartile is 21.736, indicating that the titanium distribution coefficient is between 16 and 22 in the middle 50% of the cases that are least affected by abnormal conditions. In order to increase the success factor, the requirements for titanium content entering the furnace are tightened, and the distribution coefficient is taken as 16 for calculation (indicating that the Ti content in the slag is 16 times that in the molten iron).

[0035] 3) The upper limit of the titanium content brought into each batch of sintered ore plus pellets is calculated by the upper limit of the required value of the titanium content in the molten iron and the distribution coefficient of titanium between slag and molten iron determined in the previous step.

[0036] When smelting special steel, the upper limit of titanium content in molten iron is 0.100%. According to the distribution coefficient determined in the above step, the titanium content in slag is 0.100% x 16 = 1.600%. Using the weight of batch iron x titanium content in molten iron + weight of batch slag x titanium content in slag = titanium content brought into batch material, the upper limit of the total titanium content in the batch iron material is 69200 x 0.100% + 24289 x 1.600% = 457.824 kg.

[0037] 4) Determine the iron material that needs to have its titanium content reduced based on the difficulty and timeliness of adjusting the iron material.

[0038] The iron-containing raw materials used in blast furnaces are sintering and pelletizing. Since sintering ore has problems with mixed ore pile and long material change time, the titanium content of the pellets is adjusted.

[0039] 5) The upper limit of the titanium content of the pellets that needs to be adjusted is calculated based on the upper limit of the titanium content entering the blast furnace.

[0040] The upper limit of titanium content in a single batch of iron material entering the blast furnace - the titanium content in a single batch of sintered ore = the upper limit of titanium content allowed to be brought into the pellets.

[0041] 457.824-0.16%╳87010=318.608kg (the upper limit of titanium allowed to be brought into a single batch of pellets);

[0042] The upper limit of titanium allowed to be brought into a single batch of pellets / the weight of a single batch of pellets = the upper limit of Ti content in the pellets (318.608 / 37290=0.854%).

[0043] 6) Determine the upper limit of Ti content in the pellets for the ore species with room for adjustment.

[0044] Ti content of pellets = Ti content of ore type 1 + Ti content of ore type 2 + Ti content of ore type 3

[0045] Then: The upper limit of Ti content in ore type 3 = the upper limit of Ti content in pelletized ore - the Ti content in ore type 1 - the Ti content in ore type 2

[0046] Mineral 3, Ti content upper limit = 1.5%

[0047] The raw material supplier is selected according to the upper limit of Ti content of 1.5%. All iron ore concentrates supplied by suppliers with Ti content meeting the requirements are used for ore type 3.

[0048] 7) Determine the time when the low titanium pellets enter the blast furnace tank.

[0049] Since it takes 6 hours for sintered and pelletized ore to be converted into molten iron in the blast furnace and the blast furnace tank storage needs to be consumed for 7 hours, it is required to manufacture the low-Ti pelletized ore at least 13 hours in advance and transport it to the blast furnace raw material tank for loading.

[0050] 8) After the low-titanium ferromaterial enters the blast furnace, the low-Si smelting parameters are adjusted to inhibit titanium reduction from entering the molten iron to produce low-titanium molten iron.

[0051] The correlation analysis of Si and Ti components in molten iron is carried out. Figure 3 As shown, it can be seen that the correlation coefficient between molten iron Si and molten iron Ti is high and positively correlated. Therefore, after the low-titanium pellets enter the blast furnace, the blast furnace further refines the operating range under the operating range of Si0.3-0.6 to a lower operating range of 0.3-0.45 to further inhibit Ti reduction from entering the molten iron.

[0052] Effect verification:

[0053] In daily blast furnace production, the total amount of Ti element entering the blast furnace fluctuates between 320kg and 686kg per batch of ore, and the Ti content of the output pig iron fluctuates between 0.075% and 2.050%, with an average value of Figure 4 ( Figure 4 The figure on the left shows that without special control, the silicon steel cannot meet the requirements of Ti content in molten iron (significantly higher than the upper limit) and stability (needs to be continuously lower than the upper limit of Ti requirement to enable continuous production of steelmaking). Through the calculation of the balance and flow of Ti elements in the pre-iron production line, after the low Ti resource is pulled, from the line chart ( Figure 4 As can be seen from the figure on the right, after the control measures taken by this method during the period of silicon steel refining in the steelmaking process, the total amount of Ti element entering the blast furnace is controlled below 458kg, and the Si content of molten iron is controlled at around 0.40. The Ti content of molten iron drops from 0.1476% to 0.0734%, meeting the requirement of Ti<0.100%. The Ti content of molten iron drops significantly and can remain stable for a long time within the range that meets the requirements, laying the foundation for the subsequent refining of silicon steel.

[0054] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for adjusting the titanium content in molten iron, characterized in that: The steps include: 1) Determine the relationship between the Ti content in molten iron and the total amount of titanium entering the blast furnace; 2) Determine the distribution ratio of titanium in slag and molten iron under daily operating parameters; 3) calculating the upper limit of the titanium content allowed to be brought into the iron material entering the blast furnace by using the upper limit of the titanium content in the molten iron and the distribution coefficient of the titanium element between the slag and the molten iron determined in the previous step; 4) Determine the iron material that needs to reduce titanium content based on the difficulty and timeliness of iron material adjustment; 5) calculating the upper limit of the titanium content of the iron material that needs to adjust the titanium content according to the upper limit of the titanium content entering the blast furnace; 6) Determine the upper limit of the Ti content of the raw material with large Ti fluctuations through the upper limit of the titanium content of the finished iron material, and select a suitable raw material supplier; use the iron concentrate with titanium content that meets the requirements supplied by the raw material supplier to produce iron materials with titanium content that meets the requirements; 7) Determine the time when the low-titanium iron material enters the blast furnace tank according to the time of receiving the low-titanium iron water and the blast furnace smelting cycle combined with the blast furnace iron material tank storage; 8) After the low-titanium ferromaterial enters the blast furnace, the smelting parameters are adjusted to inhibit the reduction of titanium into the molten iron, thereby significantly reducing the titanium content of the molten iron.

2. The method for adjusting the titanium content in molten iron according to claim 1, characterized in that: The step 1) specifically includes: Statistics are collected on the titanium load entering the blast furnace and the average titanium content of molten iron in the blast furnace operation data. The titanium load is counted from the lowest value to the highest value with a step size of 1. All molten iron components with titanium load falling within the corresponding interval are averaged and placed in the "Average Item: Molten Iron Ti". The titanium content in molten iron is affected by the titanium load. The higher the titanium load, the higher the titanium content in molten iron. Therefore, to control the Ti content in molten iron, it is necessary to first control the total amount of Ti entering the blast furnace.

3. The method for adjusting the titanium content in molten iron according to claim 1, characterized in that: The step 2) specifically includes: defining the same batch output: Ti content in slag / Ti content in molten iron = titanium distribution coefficient, and statistically analyzing the titanium distribution coefficient under normal production conditions. The first quartile of the titanium distribution coefficient is 16.03, and the third quartile is 21.736, indicating that the titanium distribution coefficient is between 16 and 22 in the middle 50% of the cases that are least affected by abnormal conditions; in order to increase the success rate, the requirements for titanium content entering the furnace are tightened, and a distribution coefficient of 16 is taken for calculation, indicating that the Ti content in the slag is 16 times that in the molten iron.

4. The method for adjusting the titanium content in molten iron according to claim 1, characterized in that: In the step 4), the iron-containing raw materials used in the blast furnace are sintered ore and pellets. Since the sintered ore has the problem of mixed ore pile and long material change time, the titanium content of the pellets is adjusted.

5. The method for adjusting the titanium content in molten iron according to claim 4, characterized in that: In the step 5), the upper limit of titanium content in a single batch of iron material entering the blast furnace minus the titanium content in a single batch of sintered ore = the upper limit of titanium content allowed to be brought into the pellets.

6. The method for adjusting the titanium content in molten iron according to claim 1, characterized in that: In the step 7), since the time for sintering and converting the pellets into molten iron in the blast furnace is 6 hours and the blast furnace tank storage needs to consume 7 hours, it is required to manufacture the low-Ti pellets at least 13 hours in advance and transport them to the blast furnace raw material tank for loading.

7. The method for adjusting the titanium content in molten iron according to claim 1, characterized in that: In the step 8), a correlation analysis is performed on the components of Si and Ti in the molten iron, and it is found that the correlation coefficient between Si and Ti in the molten iron is relatively high and positively correlated. Therefore, after the low-titanium pellets enter the blast furnace, the blast furnace further refines the operating range to a lower operating range of 0.3-0.45 under the operating range of Si0.3-0.6, thereby further inhibiting Ti from being reduced and entering the molten iron.