High-flux-density iron-cobalt-based nanocrystalline soft magnetic alloy with low coercive force and high magnetic conductivity and preparation method of high-flux-density iron-cobalt-based nanocrystalline soft magnetic alloy
Through alloy composition optimization and longitudinal magnetic field heat treatment, the problem of low saturation flux density of iron-based nanocrystalline alloys in high power density scenarios is solved, and iron-cobalt-based nanometers with high saturation flux density, low coercivity and low loss are achieved. Crystal soft magnetic alloys significantly improve the amorphous formation ability and soft magnetic properties of nanocrystals.
Patent Information
- Application Number
- CN202411283297.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-22
AI Technical Summary
Existing iron-based nanocrystalline alloys have low saturation flux density in high power density scenarios. The reduction of non-ferromagnetic elements leads to grains that are prone to abnormal growth, and the nanocrystallation process is difficult to control, and the excessive iron content leads to non-alloy system. The crystal formation ability is limited, making it difficult to have high saturation flux density, low loss and excellent processability.
Through the optimization of alloy composition design and combined with longitudinal magnetic field heat treatment methods, the content and proportion of elements such as Cu, P, Co, Fe are controlled to form a uniform fine nanocrystal structure, broaden the crystallization temperature range, and promote heteronucleation of α-Fe nanocrystals. , and the nucleation-growth process of nanocrystals is affected by magnetic fields, inhibiting rapid growth and diffusion of grains, and improving amorphous formation ability and soft magnetic properties.
Immuno-cobalt-based nanocrystalline soft magnetic alloy with high saturation flux density, low coercivity and low loss has been achieved. The effective magnetic permeability is significantly improved, the coercivity is reduced, the grain number density and uniformity are improved, and the magnetic domain structure rules are regular. The magnetization mechanism transforms into a uniform domain wall displacement dominant, significantly improving soft magnetic properties.
Smart Images

Figure CN119008162A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal materials, and relates to a nanocrystalline soft magnetic alloy and a preparation method thereof, and in particular to a high magnetic density iron-cobalt-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and a preparation method thereof. Background Art
[0002] Magnetic materials are widely used in power transmission and electromagnetic conversion systems, among which iron-based nanocrystalline soft magnetic alloys have attracted widespread attention due to their low loss and high energy conversion efficiency. Compared with silicon steel, the significantly reduced effective magnetocrystalline anisotropy of iron-based nanocrystalline alloys makes them have smaller intrinsic hysteresis losses, and the thickness is reduced by one order of magnitude, and the resistivity is increased by about two times, which further reduces the eddy current loss of the alloy. However, the relatively low saturation flux density of iron-based nanocrystalline alloys has become the main factor limiting their application in high power density scenarios. To increase the saturation flux density of nanocrystalline alloys, it is necessary to minimize the content of non-ferromagnetic elements, especially Nb, Mo, W, Ta, Zr, Hf and other elements with large atomic radius that promote the formation of amorphous and nanocrystals. Based on the composition design idea of increasing the content of ferromagnetic elements, a series of FeSi(B,P,C)Cu nanocrystalline soft magnetic alloy systems with high saturation flux density have been developed one after another.
[0003] Patent CN111910054B discloses a heat treatment method for a high-performance iron-based amorphous nanocrystalline strip. The chemical composition of the nanocrystalline alloy is: Fe 83 4B 10 P2Cu1, coercivity is 5.8-8.1A / m, saturation magnetic flux density is 1.80-1.82 T. The heat treatment method disclosed in the patent is high temperature short time heat treatment, heating rate is 150-200℃ / s, heat treatment time is 30-60s.
[0004] Patent CN106834930B discloses an iron-based nanocrystalline alloy with high magnetic induction intensity and high impurity compatibility and a method for preparing the alloy using industrial raw materials. The series of FeBSiPCCu and FeBSiPCu nanocrystalline alloys are prepared by conventional heat treatment methods, with a coercive force of 4.7-6.7A / m, an effective magnetic permeability (1kHz) of 16000-23000, and a saturation magnetic induction intensity of 1.78-1.83T.
[0005] These alloys have obvious shortcomings in the actual production process. The reduction in the content of non-ferromagnetic elements makes it easy for the grains to grow abnormally, which makes the nanocrystallization process difficult to control and the overall soft magnetic properties deteriorate. In addition, the excessively high iron content leads to limited amorphous formation ability of the alloy system, which is prone to surface crystallization during rapid quenching. With the rapid development of strategic emerging industries such as 5G / 6G communications, new energy vehicles, smart grids, and wireless charging, the research and development of nanocrystalline soft magnetic alloys with high saturation flux density, high magnetic permeability, low loss and excellent processability has become an urgent need in my country's power electronics field.
[0006] Many studies have shown that adding a high content of P element to Fe-based nanocrystalline alloys can effectively reduce the grain size. P element and Cu element have negative mixing enthalpy (-9kJ / mol), which easily forms P-Cu clusters, which act as nucleation particles to promote the rapid nucleation of α-Fe grains (IEEE Transactions on Magnetics 2014, 50: 2003304; Journal of Magnetism and Magnetic Materials 2016, 401: 1123-1129). However, according to relevant literature reports, in FeSiBPCu and FeBPCu nanocrystalline alloy systems, when the addition of P element exceeds 6at.%, not only the improvement of coercivity and permeability is limited, but also the saturation flux density of the nanocrystalline alloy is significantly reduced (Thin Solid Films 2011, 519: 8283-8286; Journal of Alloys and Compounds 2011, 509: S431-S433).
[0007] Adding Co element to Fe-based nanocrystalline alloys can often effectively improve the saturation magnetic flux density of the alloy. On the one hand, the d orbital hybridization effect between Fe atoms and the nearest neighbor Co atoms causes electron redistribution, the local electronic state density of Fe and Co changes, and the average magnetic moment of the alloy, especially the local magnetic moment of Fe atoms, increases with the increase of Co content (Physical Review B 2011, 83: 054202). On the other hand, an α-FeCo grain phase with a saturation magnetic flux density of about 2.45T can be formed, which is significantly higher than the 2.18T of the α-Fe grain phase (Journal of Magnetism and Magnetic Materials 2017, 441: 174-179).
[0008] Patent CN116864253B discloses a nanocrystalline soft magnetic material and its preparation method. The molecular formula of the nanocrystalline material is: Fe a Co b Si cB d X e , X includes Nb and Cu. 0.76 Si 0.13 B 0.08 Nb 0.03 Nanocrystalline alloy, Fe 0.72 Co 0.04 Si 0.13 B 0.08 Nb 0.03 The saturation magnetic flux density of the nanocrystalline alloy is significantly improved from 1.37 T to 1.52 T, but at the same time, the coercivity is significantly increased. This is due to the large magnetocrystalline anisotropy constant of the Co element and the local induced anisotropy from the orderly arrangement of Co atoms in the nanocrystalline phase [Scripta Materialia 2012, 67: 548-553]. Ordinary heat treatment often leads to the deterioration of the soft magnetic properties of Fe-Co-based nanocrystalline alloys.
[0009] The study found that longitudinal magnetic field heat treatment, by applying an external longitudinal magnetic field, causes some atoms inside the alloy to rearrange during the diffusion process, introducing long-range uniaxial anisotropy. Compared with methods such as tensile stress heat treatment and transverse magnetic field heat treatment, it can significantly improve the soft magnetic properties such as coercivity and effective permeability of a series of classic nanocrystalline alloy systems such as Finemet, Nanoperm and Hitperm [Journal of Magnetism and Magnetic Materials 2003, 254-255: 477-479; Physica Status Solidi B 2011, 248: 2382-2388; IEEE Transactions on Magnetics 2015, 51: 2004704].
[0010] Patent CN109722517B provides a high-performance iron-based amorphous nanocrystalline alloy heat treatment method, the heat treatment method is to combine compressive stress on Fe at 673-713K 85.7 Si 0.5 B 9.3 Cu 0.7 P 3.5 C 0.3 The alloy strips were subjected to nanocrystallization heat treatment, and then the nanocrystalline alloy strips were subjected to magnetic field heat treatment at 573-633 K to further optimize the soft magnetic properties, and the coercivity was reduced to 5.6-6.5 A / m.
[0011] Patent CN111057970B provides a method for preparing amorphous nanocrystalline alloys with high magnetic permeability. Fe-Co-Si-B-Cu-(V, Ta, Nb)-(Ti, Zr, Hf, Ni, Ge, Cr, Mn, W, Zn, Sn, Sb, Mo, Y, Al) series nanocrystalline alloys are obtained by transverse magnetic field heat treatment. The magnetic permeability reaches more than 35,000 at a frequency of 100 kHz, and the saturation magnetic flux density is 1.42-1.56 T.
[0012] None of the above patent documents involve the use of longitudinal magnetic field crystallization heat treatment method to optimize the soft magnetic properties of high saturation magnetic flux density nanocrystalline alloys, and there is a lack of research on the influence of magnetic field on the nanocrystallization process and nanocrystalline microstructure. Therefore, it is necessary to combine composition design with longitudinal magnetic field heat treatment process to prepare iron-based nanocrystalline soft magnetic alloys with high saturation magnetic flux density, low loss, high magnetic permeability and low coercivity, and explore the influence of longitudinal magnetic field heat treatment on the microstructure, crystallization behavior, magnetization process and magnetic anisotropy of nanocrystalline alloys. Summary of the invention
[0013] Purpose of the invention: The technical problem to be solved by the present invention is to provide a high magnetic density iron-cobalt based nanocrystalline soft magnetic alloy with low coercivity and high magnetic permeability.
[0014] The technical problem that the present invention also solves is to provide a method for preparing a high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity and high magnetic permeability.
[0015] Technical solution: In order to solve the above technical problems, the present invention provides a high magnetic density iron-cobalt-based nanocrystalline soft magnetic alloy with low coercivity and high magnetic permeability. The molecular formula of the iron-cobalt-based nanocrystalline soft magnetic alloy is: Fe a Co b B c Si d C e P f Cu g , where a, b, c, d, e, f, and g represent the atomic percentages of the corresponding alloying elements and satisfy the following conditions: 74 <a≤75,7<b≤8,7<c<10,2<d<3,2<e<3,0<f<5,0<g≤1,a+b+g=84,c:d:e=10:3:3,a+b+c+d+e+f+g=100。
[0016] The present invention optimizes alloy properties by alloy composition design, specifically considering the following aspects:
[0017] 1. Construct uniform and dense nanocrystalline structure
[0018] (1) Cu is a key element in inducing the precipitation of uniform and fine nanocrystals from the amorphous matrix in the alloy of the present invention. There is a positive mixing enthalpy between Cu and Fe (+13 J mol -1 ) and immiscible, during the heat treatment process, the Cu element segregates to form Cu-rich clusters with a near-fcc structure, promoting the heterogeneous nucleation of α-Fe nanocrystals. The present invention regulates the Cu element content so that the amorphous forming ability of the alloy is not significantly reduced to prepare a completely amorphous quenched strip, while widening the crystallization temperature range and promoting the formation of high-density nucleation points during the heat treatment process.
[0019] (2) P and Cu have a strong affinity and are easy to form Cu3P clusters, which are similar to Cu clusters and can reduce the nucleation activation energy to promote the precipitation of α-Fe nanocrystals and inhibit the growth of nanocrystals. In addition, during the crystallization of α-Fe, P is insoluble in the grains. It slowly diffuses into the remaining amorphous matrix and forms an enriched layer, which effectively limits the rapid diffusion of Fe and improves the thermal stability of the amorphous matrix, thereby hindering the rapid growth of grains. The present invention controls the content of P to below 6 at.%, ensuring the grain refinement effect without significantly reducing the saturation flux density and amorphous forming ability, and avoiding the precipitation of primary crystal phase in the quenched strips.
[0020] 2. Ensure high saturation flux density
[0021] (1) In order to obtain a high saturation magnetic flux density, the alloy must have a high content of ferromagnetic elements. However, too high a content of ferromagnetic elements will significantly reduce the amorphous forming ability. In the present invention, the atomic percentage of ferromagnetic elements must meet the requirements of both high saturation magnetic flux density and large amorphous forming ability. The atomic percentage of ferromagnetic elements is controlled at 83 at.%, so that the alloy composition is close to the eutectic point.
[0022] (2) The increase in the mass percentage of non-magnetic elements such as Cu and P that promote the formation of nanocrystals causes the saturation flux density to decrease. Therefore, the Co element is used to partially replace the Fe element, and the strong exchange coupling between Fe and Co is introduced to improve the saturation flux density without deteriorating the amorphous forming ability and process performance. However, excessive addition of Co elements will reduce the saturation flux density and increase the cost of raw materials. Considering the soft magnetic properties and raw material costs, the Co element content is optimized.
[0023] 3. Ensure the alloy's amorphous forming ability
[0024] In the present invention, when the Fe and Co contents are maintained at 83 at.%, from the perspective of thermodynamics and topology, the contents of B, Si, C, and P elements need to be in a specific ratio to obtain good amorphous forming ability. Therefore, when adjusting the P element content to refine the nano-grains, the atomic percentage ratio B:Si:C=10:3:3 is maintained.
[0025] Based on the above considerations, the Cu content in the designed alloy is ~1at.%, the P content is 1-5at.%, the Co content is ~8at.%, the total content of Fe and Co elements is ~83at.%, the atomic percentage ratio of B, Si and C elements is 10:3:3, and the obtained iron-cobalt based nanocrystalline alloy has high saturation magnetic flux density, good amorphous forming ability and uniform and fine nanocrystalline structure.
[0026] The iron-cobalt-based nanocrystalline soft magnetic alloy has an amorphous-nanocrystalline dual-phase structure, a crystallization volume fraction of 53-62%, an average grain size of 11-13 nm, and a grain number density of (5.5-7.7)×10 23 m -3 .
[0027] The iron-cobalt-based nanocrystalline soft magnetic alloy has a coercive force of 1.1-4.0 A / m, an effective magnetic permeability of 22900-31300, a loss of 0.05-0.09 W / kg, and a saturation magnetic flux density of 1.77-1.83 T.
[0028] The iron-cobalt-based nanocrystalline soft magnetic alloy has a wide crystallization temperature range of 145-152K.
[0029] Although the above-mentioned inventive alloy composition can ensure high saturation magnetic flux density and control the nanocrystalline structure, the nanocrystalline alloy obtained by the ordinary crystallization heat treatment method has uneven induced anisotropy distribution, and the soft magnetic properties still have a lot of room for improvement.
[0030] To address this problem, the present invention also includes a method for preparing the high magnetic density iron-cobalt-based nanocrystalline soft magnetic alloy with low coercivity and high magnetic permeability, comprising the following steps:
[0031] (1) 15 g of a mixed raw material consisting of single elements Fe, Co, B, Si, Cu and Fe-C (5 wt.% C) and Fe-P (26.4 wt.% P) master alloys were weighed according to atomic percentage, and the prepared raw materials were induction melted under a protective atmosphere to obtain a master alloy ingot with uniform composition, and the master alloy ingot was prepared into an alloy strip by a single-roll quenching method under a protective atmosphere, and the strip width and thickness were 0.8-1.2 mm and 16-24 μm, respectively;
[0032] (2) subjecting the alloy strip obtained in step (1) to longitudinal magnetic field heat treatment under vacuum conditions, and cooling the strip by water cooling to obtain the iron-cobalt-based nanocrystalline soft magnetic alloy.
[0033] Wherein, in step (1), the process parameters of the single-roller rapid cooling method are: the copper roller surface linear speed is 40-50m / s, the spraying temperature is 1320-1420K, and the spraying pressure is 0.015-0.030MPa, so as to obtain an alloy strip with high surface quality and uniform thickness.
[0034] Wherein, in step (2), the longitudinal magnetic field heat treatment applies a longitudinal magnetic field during the heating and insulation stages of the alloy strip to affect the nucleation-growth process of the nanocrystals.
[0035] Wherein, in step (2), the longitudinal magnetic field heat treatment generates a magnetic anisotropy energy of 550-670 J / m in the Fe-Co-based nanocrystalline alloy. 3 .
[0036] Wherein, in step (2), the process parameters of the longitudinal magnetic field heat treatment are: heat treatment temperature is 663-763K, heat treatment time is 3-5min, vacuum degree is (2-8)×10 -2 Pa, the magnetic field strength is 0.05-0.10T, and the water cooling time is 1-2min to fully eliminate the residual internal stress and avoid the formation of coarse grain structure or surface oxidation to deteriorate the soft magnetic properties.
[0037] Preferably, in step (2), the longitudinal magnetic field crystallization heat treatment temperature is 703-763K, which is always lower than the Curie temperature of the alloy crystallization phase, so that the atomic diffusion and arrangement inside the alloy are affected by the longitudinal magnetic field, generating longitudinal easy-axis magnetic anisotropy.
[0038] The specific steps of step (2) are as follows: cutting a number of alloy strips with a length of 6-8 cm and placing them into a quartz tube, sealing the quartz tube and evacuating the tube to a vacuum of (2-8)×10 -2 Pa; then, the quartz tube is placed in a heat treatment furnace with a temperature reaching a preset value of 663-763K for isothermal crystallization heat treatment, and at the same time, the magnetic field generating device is turned on to apply a magnetic field with an intensity of 0.05-0.10T along the length direction of the strip to the strip; finally, after reaching the preset insulation time of 3-5min, the quartz tube is quickly taken out and placed in 293K water for quenching and cooling for 1-2min.
[0039] The present invention also includes using an X-ray diffractometer (XRD) to test the alloy strip structure obtained in step (1) to evaluate the amorphous forming ability of the alloy. The crystallization behavior of the alloy strip obtained in step (1) is analyzed by a differential scanning calorimeter (DSC), and the heating rate is 40K / min to determine the first crystallization temperature (T x1 ) and the second crystallization temperature (T x2 ).
[0040] The present invention also includes measuring the soft magnetic properties of the nanocrystalline alloy after the treatment in step (2) by means of magnetic testing equipment, including measuring the loss and coercive force by means of an AC / DC BH loop tester, measuring the effective magnetic permeability by means of an impedance analyzer, and measuring the saturation magnetic flux density by means of a vibrating sample magnetometer (VSM) and calculating the induced anisotropy energy.
[0041] The present invention also includes using XRD and transmission electron microscopy (TEM) to characterize the microstructure of the nanocrystalline alloy after the treatment in step (2), and statistically analyzing the grain size distribution, crystallization volume fraction and grain number density. A magneto-optical Kerr microscope is used to observe the magnetic domain structure and magnetization process of the nanocrystalline alloy after the treatment in step (2).
[0042] Beneficial effects: Compared with the prior art, the advantages of the present invention include:
[0043] (1) The alloy composition designed in the present invention meets the requirements of the amorphous forming ability of the strip, so that the alloy quenched strip does not precipitate the primary crystal phase. During the crystallization heat treatment process, the nucleation and growth process of the amorphous matrix is synchronized, and the competition between the grains hinders the rapid growth of the grains.
[0044] (2) The iron-cobalt-based nanocrystalline soft magnetic alloy of the present invention has a wide crystallization temperature range, and the distance between the first crystallization peak and the second crystallization peak is as wide as 145-152K, which broadens the nanocrystallization heat treatment temperature window.
[0045] (3) The iron-cobalt-based nanocrystalline soft magnetic alloy of the present invention has a uniform and fine nanocrystalline structure, a crystallization volume fraction of 51-57%, an average grain size of 11-17 nm, and a grain number density of (2.2-7.6)×10 23 m -3 .
[0046] (4) The iron-cobalt-based nanocrystalline soft magnetic alloy of the present invention has a high saturation magnetic flux density, which is ≥1.77 T, or even ≥1.83 T. The coercive force is 4.8-6.7 A / m, the effective magnetic permeability (1 A / m, 1 kHz) is 8000-15100, and the loss (1.0 T, 50 Hz) is 0.11-0.16 W / kg.
[0047] (5) The longitudinal magnetic field crystallization heat treatment method of the present invention has the effect of greatly improving the effective magnetic permeability, reducing the coercive force and loss of the alloy of the present invention, so that the effective magnetic permeability (1A / m, 1kHz) is increased from 8000-15100 to 31300, the coercive force is reduced from 4.8-6.7A / m to 1.1-4.0A / m, and the loss (1.0T, 50Hz) is reduced from 0.11-0.16W / kg to 0.05-0.09W / kg.
[0048] (6) The longitudinal magnetic field crystallization heat treatment method of the present invention has the effect of further refining the nanocrystalline structure of the alloy of the present invention. On the one hand, the magnetic field promotes the rapid precipitation of α-(Fe, Co) nuclei with Cu clusters as heterogeneous nucleation points, increases the nucleation rate of α-(Fe, Co) grains, and refines the grains through the growth process driven by high-density grain competition. On the other hand, the magnetic field reduces the grain growth rate by inhibiting element diffusion. The grain number density is reduced from (2.2-7.6)×10 23 m -3 Increased to (5.5-7.7)×10 23 m -3 , the crystallization volume fraction increased from 51-57% to 53-62%, and the average grain size decreased from 11-17nm to 11-13nm.
[0049] (7) The longitudinal magnetic field crystallization heat treatment method of the present invention produces a longitudinal easy axis magnetic anisotropy of 550-670 J / m 3 , suppressing the local magnetic anisotropy fluctuations.
[0050] (8) The longitudinal magnetic field crystallization heat treatment method of the present invention enables the alloy of the present invention to form regular magnetic domains and arrange them longitudinally along the strips. There is no local magnetization fluctuation inside the magnetic domains, and the magnetization mechanism is transformed into being dominated by uniform domain wall displacement. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 is the DSC curve of the quenched alloy strip prepared in Example 1-5;
[0052] Figure 2 is the XRD pattern of Example 1-5;
[0053] Figure 3 is the effective magnetic permeability of Examples 1-5 and Comparative Examples 1-5;
[0054] Figure 4 is the coercive force of Examples 1-5 and Comparative Examples 1-5;
[0055] Figure 5 The power frequency loss and working magnetic induction change curves of Examples 1-5 and Comparative Examples 1-5;
[0056] Figure 6 TEM bright field images of Example 1 and Comparative Example 1;
[0057] Figure 7 This is the magnetic domain evolution image of the magnetization process of Example 3;
[0058] Figure 8 This is the magnetic domain evolution image of the magnetization process of comparative example 3. DETAILED DESCRIPTION
[0059] The present invention is described in further detail below.
[0060] Example 1
[0061] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 16 P1] 16 / 17 The method for preparing an iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0062] (1) The single elements Fe, Co, B, Si, Cu and the master alloys of Fe-C (5 wt.% C) and Fe-P (26.4 wt.% P) were mixed according to the atomic percentage of Fe:Co:B:Si:Cu:C:P=75:8:9.4118:2.8235:1:2.8235:0.9412 to obtain 15 g of a mixed material;
[0063] (2) using an induction melting furnace to melt the prepared mixed material under argon protection at a melting temperature of 1450K to obtain a master alloy ingot with uniform composition;
[0064] (3) crushing the master alloy ingot and placing it in a quartz tube with a nozzle at the bottom, fixing the quartz tube in an induction coil, and rapidly melting the small alloy ingot at 1650K by induction heating under the protection of high-purity argon gas, then turning off the heating power supply, and waiting for the alloy melt to cool to 1320K, using a single-roller rapid cooling strip spinning technology at a copper roller surface linear speed of 40m / s and a spray pressure of 0.015MPa to prepare a 1mm wide and 20μm thick alloy strip with a smooth surface and uniform thickness;
[0065] (4) Cut several alloy strips with a length of 6-8 cm and place them in a quartz tube. Seal the quartz tube and evacuate it to 8×10 -2 Pa; then, the quartz tube is placed in a heat treatment furnace with a temperature reaching a preset value of 743K for isothermal crystallization heat treatment, and at the same time, the magnetic field generating device is turned on to apply a magnetic field with an intensity of 0.1T along the length direction of the strip to the strip; finally, after reaching the preset insulation time of 5 minutes, the quartz tube is quickly taken out and placed in 293K water for quenching and cooling for 2 minutes to obtain a nanocrystalline alloy sample with a grain size of 13nm.
[0066] Example 2
[0067] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 15 P2] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0068] (1) The single elements Fe, Co, B, Si, Cu and the master alloys of Fe-C (5 wt.% C) and Fe-P (26.4 wt.% P) were mixed according to the atomic percentage of Fe:Co:B:Si:Cu:C:P=75:8:8.8235:2.6471:1:2.6471:1.8824 to obtain 15 g of a mixed material;
[0069] (2) using an induction melting furnace to melt the prepared mixed material under argon protection at a melting temperature of 1450K to obtain a master alloy ingot with uniform composition;
[0070] (3) crushing the master alloy ingot and placing it in a quartz tube with a nozzle at the bottom, fixing the quartz tube in an induction coil, and rapidly melting the small alloy ingot at 1650K by induction heating under the protection of high-purity argon gas, then turning off the heating power supply, and waiting for the alloy melt to cool to 1320K, using a single-roller rapid cooling strip spinning technology at a copper roller surface linear speed of 40m / s and a spray pressure of 0.015MPa to prepare a 1mm wide and 20μm thick alloy strip with a smooth surface and uniform thickness;
[0071] (4) Cut several alloy strips with a length of 6-8 cm and place them in a quartz tube. Seal the quartz tube and evacuate it to 8×10 -2 Pa; then, the quartz tube is placed in a heat treatment furnace with a temperature reaching a preset value of 743K for isothermal crystallization heat treatment, and at the same time, the magnetic field generating device is turned on to apply a magnetic field with an intensity of 0.1T along the length direction of the strip to the strip; finally, after reaching the preset insulation time of 5 minutes, the quartz tube is quickly taken out and placed in 293K water for quenching and cooling for 2 minutes to obtain a nanocrystalline alloy sample with a grain size of 11nm.
[0072] Example 3
[0073] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 14 P3] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0074] (1) The single elements Fe, Co, B, Si, Cu and the master alloys of Fe-C (5 wt.% C) and Fe-P (26.4 wt.% P) were mixed according to the atomic percentage of Fe:Co:B:Si:Cu:C:P=75:8:8.2353:2.4706:1:2.4706:2.8235 to obtain 15 g of a mixed material;
[0075] (2) using an induction melting furnace to melt the prepared mixed material under argon protection at a melting temperature of 1500K to obtain a master alloy ingot with uniform composition;
[0076] (3) crushing the master alloy ingot and placing it in a quartz tube with a nozzle at the bottom, fixing the quartz tube in an induction coil, and rapidly melting the small alloy ingot at 1700K by induction heating under the protection of high-purity argon gas, then turning off the heating power supply, and waiting for the alloy melt to cool to 1420K, using a single-roller rapid cooling strip spinning technology with a copper roller surface linear speed of 40m / s and a spray pressure of 0.030MPa to prepare a 0.8mm wide and 24μm thick alloy strip with a smooth surface and uniform thickness;
[0077] (4) Cut several alloy strips with a length of 6-8 cm and place them in a quartz tube. Seal the quartz tube and evacuate it to 2×10 -2 Pa; then, the quartz tube is placed in a heat treatment furnace with a temperature reaching a preset value of 763K for isothermal crystallization heat treatment, and at the same time, the magnetic field generating device is turned on to apply a magnetic field with a strength of 0.05T along the length direction of the strip to the strip; finally, after reaching the preset insulation time of 3 minutes, the quartz tube is quickly taken out and placed in 293K water for quenching and cooling for 1 minute to obtain a nanocrystalline alloy sample with a grain size of 11nm.
[0078] Example 4
[0079] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 13 P4] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0080] (1) The single elements Fe, Co, B, Si, Cu and the master alloys of Fe-C (5 wt.% C) and Fe-P (26.4 wt.% P) were mixed according to the atomic percentage of Fe:Co:B:Si:Cu:C:P=75:8:7.6471:2.2941:1:2.2941:3.7647 to obtain 15 g of a mixed material;
[0081] (2) using an induction melting furnace to melt the prepared mixed material under argon protection at a melting temperature of 1500K to obtain a master alloy ingot with uniform composition;
[0082] (3) crushing the master alloy ingot and placing it in a quartz tube with a nozzle at the bottom, fixing the quartz tube in an induction coil, and rapidly melting the small alloy ingot at 1650K by induction heating under the protection of high-purity argon gas, then turning off the heating power supply, and waiting for the alloy melt to cool to 1400K, using a single-roller rapid cooling strip spinning technology at a copper roller surface linear speed of 50m / s and a spray pressure of 0.020MPa to prepare a 1.2mm wide and 16μm thick alloy strip with a smooth surface and uniform thickness;
[0083] (4) Cut several alloy strips with a length of 6-8 cm and place them in a quartz tube. Seal the quartz tube and evacuate it to 8×10 -2 Pa; then, the quartz tube is placed in a heat treatment furnace with a temperature reaching a preset value of 723K for isothermal crystallization heat treatment, and at the same time, the magnetic field generating device is turned on to apply a magnetic field with an intensity of 0.1T along the length direction of the strip to the strip; finally, after reaching the preset insulation time of 5 minutes, the quartz tube is quickly taken out and placed in 293K water for quenching and cooling for 2 minutes to obtain a nanocrystalline alloy sample with a grain size of 12nm.
[0084] Example 5
[0085] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 12 P5] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0086] (1) The single elements Fe, Co, B, Si, Cu and the master alloys of Fe-C (5 wt.% C) and Fe-P (26.4 wt.% P) were mixed according to the atomic percentage of Fe:Co:B:Si:Cu:C:P=75:8:7.0588:2.1176:1:2.1176:4.7059 to obtain 15 g of a mixed material;
[0087] (2) using an induction melting furnace to melt the prepared mixed material under argon protection at a melting temperature of 1500K to obtain a master alloy ingot with uniform composition;
[0088] (3) crushing the master alloy ingot and placing it in a quartz tube with a nozzle at the bottom, fixing the quartz tube in an induction coil, and rapidly melting the small alloy ingot at 1650K by induction heating under the protection of high-purity argon gas, then turning off the heating power supply, and waiting for the alloy melt to cool to 1400K, using a single-roller rapid cooling strip spinning technology at a copper roller surface linear speed of 50 m / s and a spray pressure of 0.020 MPa to prepare a 1 mm wide, 20 μm thick alloy strip with a smooth surface and uniform thickness;
[0089] (4) Cut several alloy strips with a length of 6-8 cm and place them in a quartz tube. Seal the quartz tube and evacuate it to 8×10 -2 Pa; then, the quartz tube is placed in a heat treatment furnace with a temperature reaching a preset value of 723K for isothermal crystallization heat treatment, and at the same time, the magnetic field generating device is turned on to apply a magnetic field with an intensity of 0.1T along the length direction of the strip to the strip; finally, after reaching the preset insulation time of 5 minutes, the quartz tube is quickly taken out and placed in 293K water for quenching and cooling for 2 minutes to obtain a nanocrystalline alloy sample with a grain size of 20nm.
[0090] The thermal performance parameters of the quenched alloy strips obtained in step (3) of Examples 1-5 were measured by DSC. Figure 1 As shown, the T x1 They are 679, 679, 678, 676, 674K, T x2 They are 828, 831, 829, 823 and 819 K respectively, thus determining that the optimized heat treatment temperature range is 703-763 K.
[0091] The nanocrystalline alloy strip structure obtained in step (4) of Example 1-5 was tested by XRD, and the results were as follows: Figure 2 As shown in the figure, all the prepared nanocrystalline alloy samples have sharp crystallization diffraction peaks corresponding to the (110), (200) and (211) crystal plane indices of the α-Fe phase. For Examples 4 and 5, as the P content increases, the (200) diffraction peak intensity gradually increases and exceeds the (110) diffraction peak intensity, indicating that a coarse crystal texture appears on the surface of the strip. This shows that controlling the P content is an effective method to regulate the amorphous forming ability and nanocrystalline structure. There is an optimal range for the P element, which requires system optimization.
[0092] The following comparative examples 1-5 are set up. The difference from embodiments 1-5 is that step (4) only performs ordinary heat treatment, and analyzes and compares the effects of the longitudinal magnetic field heat treatment method and the ordinary heat treatment method on the soft magnetic properties, microstructure and magnetization process of the iron-cobalt based nanocrystalline alloy.
[0093] Comparative Example 1
[0094] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 16 P1] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0095] Steps (1) to (3) are the same as those in Example 1, except that step (4) is as follows:
[0096] Cut several alloy strips with a length of 6-8 cm and put them into a quartz tube. After sealing the quartz tube, evacuate it to 8×10 -2 Pa; then, the quartz tube was placed in a heat treatment furnace with a temperature reaching a preset value of 743K for isothermal crystallization heat treatment. After the preset holding time of 5 minutes, the quartz tube was quickly taken out and placed in 293K water for quenching and cooling for 2 minutes to obtain a nanocrystalline alloy sample with a grain size of 17nm.
[0097] Comparative Example 2
[0098] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 15 P2] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0099] Steps (1) to (3) are the same as those in Example 2, except that step (4) is as follows:
[0100] Cut several alloy strips with a length of 6-8 cm and put them into a quartz tube. After sealing the quartz tube, evacuate it to 8×10 -2 Pa; then, the quartz tube was placed in a heat treatment furnace with a temperature reaching a preset value of 743K for isothermal crystallization heat treatment. After the preset insulation time of 5 minutes, the quartz tube was quickly taken out and placed in 293K water for quenching and cooling for 2 minutes to obtain a nanocrystalline alloy sample with a grain size of 11nm.
[0101] Comparative Example 3
[0102] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 14 P3] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0103] Steps (1) to (3) are the same as those in Example 3, except that step (4) is as follows:
[0104] Cut several alloy strips with a length of 6-8 cm and put them into a quartz tube. Seal the quartz tube and evacuate it to 2×10 -2 Pa or less; then, the quartz tube is placed in a heat treatment furnace where the temperature reaches the preset value of 763K for isothermal crystallization heat treatment. After the preset insulation time of 3 minutes, the quartz tube is quickly taken out and placed in 293K water for quenching and cooling for 1 minute to obtain a nanocrystalline alloy sample with a grain size of 11nm.
[0105] Comparative Example 4
[0106] The molecular formula is Fe75 Co8Cu1[(B 10 Si3C3) 13 P4] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0107] Steps (1) to (3) are the same as those in Example 4, except that step (4) is as follows:
[0108] Cut several alloy strips with a length of 6-8 cm and put them into a quartz tube. After sealing the quartz tube, evacuate it to 8×10 -2 Pa; then, the quartz tube was placed in a heat treatment furnace with a temperature reaching a preset value of 723K for isothermal crystallization heat treatment. After the preset holding time of 5 minutes, the quartz tube was quickly taken out and placed in 293K water for quenching and cooling for 2 minutes to obtain a nanocrystalline alloy sample with a grain size of 14nm.
[0109] Comparative Example 5
[0110] The molecular formula is Fe 75 Co8Cu1[(B 10 Si3C3) 12 P5] 16 / 17 The preparation method of the iron-cobalt-based nanocrystalline soft magnetic alloy comprises the following steps:
[0111] Steps (1) to (3) are the same as those in Example 5, except that step (4) is as follows:
[0112] Cut several alloy strips with a length of 6-8 cm and put them into a quartz tube. After sealing the quartz tube, evacuate it to 8×10 -2 Pa; then, the quartz tube was placed in a heat treatment furnace with a temperature reaching a preset value of 723K for isothermal crystallization heat treatment. After the preset insulation time of 5 minutes, the quartz tube was quickly taken out and placed in 293K water for quenching and cooling for 2 minutes to obtain a nanocrystalline alloy sample with a grain size of 26nm.
[0113] Performance comparison of the nanocrystalline alloy samples prepared in Examples 1 to 5 and Comparative Examples 1 to 5:
[0114] The effective magnetic permeability and coercivity of the nanocrystalline alloy strips prepared in step (4) of Examples 1-5 and Comparative Examples 1-5 were measured at 1 kHz and 1 A / m by an impedance analyzer and a DC BH loop tester, respectively. Figure 3 , 4As shown in Table 1, with the increase of the P element content, the effective magnetic permeability of the embodiments and comparative examples both show a trend of first increasing and then decreasing, while the coercive force both show a trend of first decreasing and then increasing. Comparing the embodiments and comparative examples with the same composition, the longitudinal magnetic field heat treatment always shows the effect of significantly improving the effective magnetic permeability and reducing the coercive force, but for Example 5 and Comparative Example 5, the improvement of the effective magnetic permeability and coercive force by the magnetic field heat treatment is significantly reduced. The effective magnetic permeability of Examples 1-4 measured under the conditions of 1kHz and 1A / m is increased to 22900-31300, and the coercive force is reduced to 1.1-4.0A / m. The loss characteristics of Examples 1-5 and Comparative Examples 1-5 are analyzed using an AC BH loop tester. The test frequency is 50Hz. The results are as follows: Figure 5 As shown in Table 1, with the increase of P element content, the loss of the embodiment and the comparative example at the same working magnetic induction shows a trend of first decreasing and then increasing, and the embodiment with the same P content always shows lower loss than the comparative example. The loss measured in Examples 1-4 at 1.0T and 50Hz is reduced to 0.05-0.09W / kg. In addition, the saturation magnetic flux density of Examples 1-5 and Comparative Examples 1-5 is measured at a magnetic field of 800kA / m using a vibrating sample magnetometer. As shown in Table 1, with the increase of P content, the saturation magnetic flux density of the nanocrystalline alloy system decreases monotonically from 1.83T to 1.75T. Therefore, preferably adjusting the P element content to 2-3at.% and combining it with the longitudinal magnetic field heat treatment method can obtain excellent comprehensive soft magnetic properties.
[0115] Table 1: Effective magnetic permeability, coercivity, loss and saturation magnetic flux density of nanocrystalline alloy strips prepared in step (4) of Examples 1-5 and Comparative Examples 1-5. The symbols in Table 1 have the following meanings: μ e is the effective magnetic permeability, H c is the coercive force, P 10 / 50 is the loss under 1.0T and 50Hz conditions, B s is the saturation flux density.
[0116]
[0117] The nanocrystalline alloy strips obtained in step (4) of Example 1 and Comparative Example 1 were characterized by microstructure, and the obtained TEM bright field images are as follows: Figure 6 As shown in the figure, both have a typical amorphous-nanocrystalline dual-phase structure, with high-density and randomly oriented nanocrystalline grains distributed in the amorphous matrix. However, the grain distribution and average size of Example 1 and Comparative Example 1 show obvious differences. The grain size of Example 1 is significantly smaller than that of Comparative Example 1, and the grain size distribution range decreases from 7-31nm to 5-23nm, and the average grain size decreases from 17nm to 13nm. It can be further estimated that the number density of nanocrystalline grains in Example 1 and Comparative Example 1 is 5.8×1023 and 2.2×10 23 m -3 , and the corresponding crystallization volume fractions are 62% and 57%, respectively, indicating that longitudinal magnetic field heat treatment can greatly increase the grain number density and promote grain refinement and uniform distribution.
[0118] The magnetization process of the nanocrystalline alloy sample was observed using a magneto-optical Kerr microscope. The dynamic magnetic domain evolution of the nanocrystalline alloy strips obtained in step (4) of Example 3 and Comparative Example 3 were as follows: Figure 7 , 8 As shown, the magnetization processes of both are dominated by domain wall displacement. However, compared with Comparative Example 3, the effective magnetocrystalline anisotropy constant in Example 3 is reduced, and the magnetic field heat treatment induces longitudinal uniform anisotropy, thereby suppressing the local magnetic anisotropy fluctuation and forming regular plate-like wide domains. The domain wall moves smoothly in the direction perpendicular to the external magnetic field, which greatly improves the soft magnetic properties of the nanocrystalline alloy.
Claims
1. A high magnetic density iron-cobalt-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability, characterized in that: The molecular formula of the iron-cobalt-based nanocrystalline soft magnetic alloy is: Fe a Co b B c Si d C e P f Cu g , where a, b, c, d, e, f, and g represent the atomic percentages of the corresponding alloying elements and satisfy the following conditions: 74 <a≤75,7<b≤8,7<c<10,2<d<3,2<e<3,0<f<5,0<g≤1,a+b+g=84,c:d:e=10:3:3,a+b+c+d+e+f+g=100。 2. The high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to claim 1, characterized in that: The iron-cobalt-based nanocrystalline soft magnetic alloy has an amorphous-nanocrystalline dual-phase structure, a crystallization volume fraction of 53-62%, an average grain size of 11-13 nm, and a grain number density of (5.5-7.7)×10 23 m -3 .
3. The high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to claim 1, characterized in that: The iron-cobalt-based nanocrystalline soft magnetic alloy has a coercive force of 1.1-4.0 A / m, an effective magnetic permeability of 22900-31300, a loss of 0.05-0.09 W / kg, and a saturation magnetic flux density of 1.77-1.83 T.
4. The high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to claim 1, characterized in that: The iron-cobalt-based nanocrystalline soft magnetic alloy has a wide crystallization temperature range of 145-152K.
5. The method for preparing the high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) According to Fe a Co b B c Si d C e P f Cu g The raw materials are weighed and mixed with atomic percentages of single elements Fe, Co, B, Si, Cu, Fe-C and Fe-P, the prepared raw materials are induction-melted under a protective atmosphere to obtain a master alloy ingot with uniform composition, and the master alloy ingot is prepared into an alloy strip by a single-roller rapid cooling method under a protective atmosphere, and the strip width and thickness are 0.8-1.2 mm and 16-24 μm respectively; (2) subjecting the alloy strip obtained in step (1) to longitudinal magnetic field heat treatment under vacuum conditions, and cooling the strip by water cooling to obtain the iron-cobalt-based nanocrystalline soft magnetic alloy.
6. The method for preparing the high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to claim 5, characterized in that: In step (1), the process parameters of the single-roller rapid cooling method are: the copper roller surface linear velocity is 40-50 m / s, the spraying temperature is 1320-1420 K, and the spraying pressure is 0.015-0.030 MPa.
7. The method for preparing the high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to claim 5, characterized in that: In step (2), the longitudinal magnetic field heat treatment applies a longitudinal magnetic field during the heating and insulation stages of the alloy strip.
8. The method for preparing the high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to claim 5, characterized in that: In step (2), the longitudinal magnetic field heat treatment produces a magnetic anisotropy energy of 550-670 J / m in the Fe-Co-based nanocrystalline alloy. 3 .
9. The method for preparing the high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to claim 5, characterized in that: In step (2), the process parameters of the longitudinal magnetic field heat treatment are: heat treatment temperature is 663-763K, heat treatment time is 3-5min, vacuum degree is (2-8)×10 -2 Pa, magnetic field strength is 0.05-0.10T, and water cooling time is 1-2min.
10. The method for preparing the high magnetic density Fe-Co-based nanocrystalline soft magnetic alloy with low coercivity, high magnetic permeability and high magnetic density according to claim 5, characterized in that: Step (2) The specific steps are as follows: cut a number of alloy strips with a length of 6-8 cm and put them into a quartz tube, seal the quartz tube and evacuate to (2-8)×10 -2 Pa; then, the quartz tube is placed in a heat treatment furnace with a temperature reaching a preset value of 663-763K for isothermal crystallization heat treatment, and at the same time, the magnetic field generating device is turned on to apply a magnetic field with an intensity of 0.05-0.10T along the length direction of the strip to the strip; finally, after reaching the preset insulation time of 3-5min, the quartz tube is quickly taken out and placed in 293K water for quenching and cooling for 1-2min.
Citation Information
Cited By
Iron-based nanocrystalline soft magnetic alloy powder, soft magnetic composite material and preparation method of iron-based nanocrystalline soft magnetic alloy powder
CN120183837A
Preparation method of amorphous nanocrystalline alloy and application of amorphous nanocrystalline alloy in industrial robot
CN122406128A