Photonic crystal laser based on quasi-two-dimensional perovskite and preparation method thereof
By using a quasi-two-dimensional perovskite film and array arrangement of dielectric pores or dielectric column structure in photonic crystal lasers, the problem of high precision and loss of photonic crystal laser manufacturing process in the prior art is solved, and efficient and stable green is achieved Single mode laser exit and optical characteristic regulation in optical band.
Patent Information
- Application Number
- CN202411126985.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art has achieved efficient and stable visible-light band photonic crystal lasers, especially short-wavelength regions, and faces the problems of high manufacturing process accuracy requirements, high cost, low yield, and large scattering and absorption losses of light in the medium.
Using a photonic crystal laser based on quasi-two-dimensional perovskite, the photonic crystal layer and quasi-two-dimensional perovskite film are designed using optical simulation software to design the photonic crystal structure, combined with spin coating Method and annealing treatment, high-precision photonic crystal laser was prepared to realize laser emission in a single mode of green light band.
The construction of a high-precision photonic crystal laser is realized, which effectively reduces optical loss, improves laser efficiency, realizes a single-mode laser emission to the green light band, and can adjust the photon energy band structure to control the wavelength, polarization and exit direction of the laser .
Smart Images

Figure CN119009669A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of micro-nano laser technology, and more specifically, to a quasi-two-dimensional perovskite-based photonic crystal laser and a preparation method thereof. Background Art
[0002] With the rapid development of nanotechnology and materials science, perovskite materials have become a hot topic of research due to their unique optoelectronic properties, especially in the field of optoelectronic devices, where they have great application potential. Among them, quasi-two-dimensional (2D) perovskites, due to the introduction of organic spacer layers in their layered structures, not only effectively suppress the common ion migration problems in three-dimensional (3D) perovskites, and improve the environmental stability and photostability of the materials, but also significantly enhance the fluorescence quantum yield and reduce non-radiative recombination through quantum confinement effects, thereby showing excellent optical properties.
[0003] Traditional laser designs usually rely on complex optical resonant cavity structures, while photonic crystal lasers represent a novel design approach. The core of this laser is the photonic crystal structure, which can form a photonic bandgap through artificially designed periodic micro-nanostructures, similar to the electronic energy band in semiconductor materials. Within the bandgap, light of a specific wavelength is prohibited from propagating, while at the edge of the bandgap or at defect states, an optical mode can be formed to achieve light amplification and feedback, thereby stimulating laser light. This mechanism allows for more flexible control of laser emission characteristics, such as wavelength and directionality, opening up new avenues for realizing miniaturized, integrated, and multifunctional photonic devices.
[0004] However, there are still many challenges to achieve efficient and stable photonic crystal lasers in the visible light band, especially in the short-wavelength region. First, the wavelength of short-wavelength light is shorter, requiring the structure of the photonic crystal to have higher precision and smaller feature size, which undoubtedly places extremely high demands on the manufacturing process. Traditional lithography or self-assembly technology is often accompanied by high costs and low yields when achieving such high precision. Secondly, the scattering and absorption losses of short-wavelength light in the medium are large, which poses a serious restriction on the performance of photonic crystal lasers. Summary of the invention
[0005] In view of this, the present disclosure provides a quasi-two-dimensional perovskite-based photonic crystal laser and a method for preparing the same.
[0006] One aspect of the present disclosure provides a quasi-two-dimensional perovskite-based photonic crystal laser, comprising: a photonic crystal layer, comprising a dielectric film, the dielectric film having an array of dielectric holes or dielectric columns; a gain medium layer, located on the photonic crystal layer, the gain medium layer being a quasi-two-dimensional perovskite film; the quasi-two-dimensional perovskite film has a luminescence spectrum covering a range of 510nm-560nm.
[0007] According to the embodiments of the present disclosure, the thickness of the dielectric film is 10nm-200nm, the periods of the dielectric holes and dielectric columns are 100nm-800nm, the diameters of the dielectric holes and dielectric columns are 50nm-300nm; the thickness of the gain dielectric layer is 50nm-200nm.
[0008] According to an embodiment of the present disclosure, the array arrangement includes a triangular lattice, a tetragonal lattice or a composite lattice.
[0009] According to an embodiment of the present disclosure, the overall size of the arrayed dielectric holes or dielectric columns is greater than 5 μm×5 μm.
[0010] According to an embodiment of the present disclosure, it is characterized in that the material of the dielectric film includes silicon oxide or magnesium fluoride.
[0011] According to an embodiment of the present disclosure, the photonic crystal layer further includes a substrate, and the dielectric film is disposed on the substrate.
[0012] Another aspect of the present disclosure provides a method for preparing a photonic crystal laser based on a quasi-two-dimensional perovskite, comprising: using optical simulation software to simulate a photonic crystal structure, designing a photonic crystal structure, and calculating a photonic band gap; based on the simulation result, generating a dielectric film having arrayed dielectric holes or dielectric columns on a substrate to obtain a photonic crystal layer; using a spin coating method to first drop a precursor solution on the photonic crystal layer, then drop chlorobenzene, and perform annealing treatment to prepare a quasi-two-dimensional perovskite film to obtain a photonic crystal laser based on a quasi-two-dimensional perovskite; wherein the precursor solution is obtained by dissolving phenethylammonium bromide, methylammonium bromide, and lead bromide in an N,N-dimethylformamide solution.
[0013] According to an embodiment of the present disclosure, a method for preparing array-arranged dielectric holes includes: firstly coating a dielectric film on a substrate, and then performing photolithography, etching and cleaning on the dielectric film to obtain array-arranged dielectric holes.
[0014] According to an embodiment of the present disclosure, a method for preparing array-arranged dielectric columns includes: first performing photolithography on a substrate, then coating a dielectric film on the photolithographic substrate, and then cleaning and peeling off to obtain array-arranged dielectric columns.
[0015] According to an embodiment of the present disclosure, when the material of the dielectric film is silicon oxide, the method further includes subjecting the photonic crystal layer to ultraviolet ozone treatment before preparing the quasi-two-dimensional perovskite film.
[0016] According to the embodiments of the present disclosure, the wavelength of the green light band is adjusted and single-mode laser emission is achieved by using the array-arranged dielectric holes or dielectric pillars of the photonic crystal layer.
[0017] According to the embodiments of the present disclosure, the use of a quasi-two-dimensional perovskite film having excellent optical gain performance effectively compensates for the loss caused by the processing of the photonic crystal laser, thereby achieving the construction of a high-precision photonic crystal laser. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:
[0019] Figure 1 A schematic side view of a quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is shown;
[0020] Figure 2 A schematic diagram of a top view of a quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is shown;
[0021] Figure 3a The photon band structure of a quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is schematically shown;
[0022] Figure 3b The photonic band structure of a quasi-two-dimensional perovskite-based photonic crystal laser with a duty cycle of 0.6 according to an embodiment of the present disclosure is schematically shown;
[0023] Figure 3c The photonic band structure of a quasi-two-dimensional perovskite-based photonic crystal laser with a duty cycle of 0.9 according to an embodiment of the present disclosure is schematically shown;
[0024] Figure 4 A scanning electron microscope image schematically shows a dielectric column photonic crystal structure of a tetragonal lattice according to an embodiment of the present disclosure;
[0025] Figure 5 A scanning electron microscope image schematically shows a dielectric hole photonic crystal structure of a tetragonal lattice according to an embodiment of the present disclosure;
[0026] Figure 6 A scanning electron microscope image schematically shows a dielectric hole photonic crystal structure of a triangular lattice according to an embodiment of the present disclosure;
[0027] Figure 7 Schematically shows an optical photograph of the entire photonic crystal structure according to an embodiment of the present disclosure;
[0028] Figure 8 The preparation process of the quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is schematically shown;
[0029] Fig. 9Schematically shows the photoluminescence spectrum of the quasi-two-dimensional perovskite film according to an embodiment of the present disclosure;
[0030] Fig.10 The photoluminescence spectrum of a quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is schematically shown;
[0031] Fig.11 The light emission spectrum of a quasi-two-dimensional perovskite-based photonic crystal laser at different pump powers according to an embodiment of the present disclosure is schematically shown;
[0032] Fig.12 The photoluminescence spectrum of a quasi-two-dimensional perovskite-based photonic crystal laser based on another photonic crystal structure according to an embodiment of the present disclosure is schematically shown. DETAILED DESCRIPTION
[0033] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of the embodiments of the present disclosure. However, it is apparent that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.
[0034] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.
[0035] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification and should not be interpreted in an idealized or overly rigid manner.
[0036] When using expressions such as "at least one of A, B, and C, etc.", they should generally be interpreted according to the meaning of the expression commonly understood by those skilled in the art (for example, "a system having at least one of A, B, and C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.).
[0037] Photonic crystal lasers diffract light fields through periodic changes in refractive index, thereby generating photon energy bands. The photon energy bands can be controlled by adjusting the period, units, and arrangement of the photonic crystal structure, giving the resonant cavity more optical characteristics.
[0038] At present, in the visible light band, especially in the preparation process of short-wavelength photonic crystal lasers, any slight processing error may lead to the destruction of the photonic bandgap structure, causing additional scattering and absorption losses. These losses will significantly affect the optical properties of photonic crystals and reduce the efficiency and threshold characteristics of lasers.
[0039] Therefore, the present invention adopts a photonic crystal layer with array-arranged dielectric holes or dielectric columns and a quasi-two-dimensional perovskite film with a luminescence spectrum covering a range of 510nm-560nm as a gain medium layer, which effectively realizes the single-mode laser emission in the green light band of the present application, and by adjusting the period, unit and arrangement of the photonic crystal structure, it is possible to achieve the regulation of optical characteristics such as different wavelengths, polarizations, emission directions or phases, and the construction of high-precision photonic crystal lasers.
[0040] Figure 3b The photonic band structure of a quasi-two-dimensional perovskite-based photonic crystal laser with a duty cycle of 0.6 according to an embodiment of the present disclosure is schematically shown;
[0041] Figure 3c The photonic band structure of a quasi-two-dimensional perovskite-based photonic crystal laser with a duty cycle of 0.9 according to an embodiment of the present disclosure is schematically shown;
[0042] like Figure 3b and Figure 3c As shown, it is the photon band diagram of the tetragonal lattice medium hole, where Figure 3b The duty cycle is 0.6, Figure 3c The duty cycle is 0.9, the ordinate is p / λ, p is the period of the circular hole, λ is the wavelength, and the abscissa is the wave vector.
[0043] The photonic crystal laser disclosed in the present invention utilizes the characteristic that the group velocity of the low-order mode at the high symmetry point (Γ) is 0 to achieve mode selection and amplification.
[0044] As in Figure 3b According to the ordinate, there are three modes (i.e., 3 lines) at a p / λ of about 0.57. If a specific wavelength needs to be amplified, the period can be determined according to the wavelength, i.e., p=0.57×λ. Therefore, the wavelength of the laser can be controlled by adjusting the period.
[0045] In addition, it can also be determined by adjusting the duty cycle, where the duty cycle is defined as d / p, where d is the diameter of the circular hole. It can be found that as the duty cycle changes, the ordinate of each mode changes. If the period remains unchanged, it means that the wavelength has changed, so the wavelength of the laser can also be adjusted by changing the duty cycle.
[0046] An embodiment of the present disclosure provides a quasi-two-dimensional perovskite-based photonic crystal laser, comprising: a photonic crystal layer, comprising a dielectric film, the dielectric film having an array of dielectric holes or dielectric columns; a gain medium layer, located on the photonic crystal layer, the gain medium layer being a quasi-two-dimensional perovskite film; the luminescence spectrum of the quasi-two-dimensional perovskite film covers a range of 510nm-560nm.
[0047] In the embodiments of the present disclosure, a photonic crystal layer is used as a resonant cavity, and the refractive index changes of a periodic medium and a quasi-two-dimensional perovskite on a two-dimensional plane are used to realize feedback mode selection of a light field; and a quasi-two-dimensional perovskite thin film layer is used as a gain medium to realize amplification of the light field, thereby generating laser light and realizing single-mode laser emission in the green light band.
[0048] According to the embodiments of the present disclosure, the thickness of the dielectric film is 10nm-200nm, the periods of the dielectric pores and dielectric columns are 100nm-800nm, and the diameters of the dielectric pores and dielectric columns are 50nm-300nm; the thickness of the gain medium layer is 50nm-200nm, and the thickness of the gain medium layer can be controlled by adjusting the concentration of the precursor.
[0049] According to an embodiment of the present disclosure, the array arrangement includes a triangular lattice, a tetragonal lattice or a composite lattice.
[0050] According to an embodiment of the present disclosure, the overall size of the arrayed dielectric holes or dielectric columns is greater than 5 μm×5 μm.
[0051] According to an embodiment of the present disclosure, the cross-sectional shape of the dielectric hole or dielectric column includes a circle, an ellipse, a square, a triangle or other polygons.
[0052] According to an embodiment of the present disclosure, a fundamental mode is selected in a mode supported by a triangular lattice, a tetragonal lattice or a composite lattice arrangement.
[0053] According to an embodiment of the present disclosure, the material of the dielectric film includes silicon oxide or magnesium fluoride.
[0054] In the embodiments of the present disclosure, the emission wavelength can be controlled by adjusting the photonic crystal structure, and the emission wavelength of the photonic crystal laser of the present disclosure is adjustable within the luminescence spectrum of the quasi-two-dimensional perovskite film.
[0055] According to an embodiment of the present disclosure, the photonic crystal layer further includes a substrate, and the dielectric film is disposed on the substrate.
[0056] Figures of the present disclosure Figure 1-12 In the embodiment, the substrate material is quartz, the material of the dielectric film is magnesium fluoride, the thickness of the dielectric film is 100 nm, and the thickness of the gain medium layer is 150 nm.
[0057] Figure 1 A side view of a quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is schematically shown.
[0058] Figure 2 A schematic top view of a quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is schematically shown.
[0059] Figure 3a The photonic band structure of a quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is schematically shown.
[0060] Figure 8 The preparation process of the photonic crystal laser based on quasi-two-dimensional perovskite according to the embodiment of the present disclosure is schematically shown. The embodiment of the present disclosure provides a preparation method of the photonic crystal laser based on quasi-two-dimensional perovskite, including: simulating with the wave optics module of COMSOL and calculating the eigenvalues.
[0061] Among them, physical modeling uses 2D modeling blocks to model the 2D morphology, composition, size and arrangement of the unit. Parameter setting, according to the physical model and purpose, sets the size, refractive index or dielectric constant of the material, wave vector, wavelength and other parameters.
[0062] The substrate material is quartz, the material of the dielectric film is magnesium fluoride, the dielectric film has dielectric holes arranged in a tetragonal lattice, the cross-sectional shape of the dielectric holes is circular, the thickness of the dielectric film is 100nm, the dielectric hole period is 358nm, and the diameter of the dielectric hole is 108nm; the thickness of the gain medium layer is 150nm.
[0063] Grid generation: divide the grid into appropriate sizes according to the size of the physical model and the characteristic wavelength to be scanned; eigenvalue solution: scan the wave vector and solve the eigenvalue, and draw the photonic crystal band structure as shown in Figure 3.
[0064] According to the solved photon energy band, the corresponding period and size are calculated. The method for preparing the photonic crystal layer includes: (1) using a thermal evaporation method to evaporate a magnesium fluoride dielectric layer on a quartz substrate with a thickness of 100 nm;
[0065] (2) Spin-coat PMMA on the magnesium fluoride film at 4000 rpm and bake at 150°C for 3 min;
[0066] (3) Spin-coat the conductive adhesive at 2000 rpm and bake at 90°C for 1 min;
[0067] (4) patterning by electron beam exposure;
[0068] (5) developing with a developer prepared with isopropyl alcohol and methyl isobutyl ketone in a volume ratio of 3:1 for 210 seconds, and then fixing with isopropyl alcohol for 30 seconds;
[0069] (6) etching magnesium fluoride using reactive ion beam etching or inductively coupled plasma etching;
[0070] (7) The electron beam glue is washed away with acetone to obtain a hole array in the magnesium fluoride film.
[0071] like Figure 8 As shown, 50 μL of the precursor solution was first dropped onto the photonic crystal layer by spin coating at a rotation speed of 5000 rpm, and then 100 μL of the anti-solvent-chlorobenzene was dropped to promote growth, and then placed on a hot stage and annealed at 100° C. for 10 min to prepare a quasi-two-dimensional perovskite film. The obtained photonic crystal laser of the present disclosure is as shown in FIG. Figure 1 and Figure 2 As shown;
[0072] The precursor solution is obtained by dissolving phenethylammonium bromide, methylammonium bromide and lead bromide in a molar ratio of 1:4:4 in a 0.4M N,N-dimethylformamide solution.
[0073] The prepared quasi-two-dimensional perovskite-based photonic crystal laser was optically characterized by using a laser confocal system and a femtosecond pulse light source to pump the effective structure of the photonic crystal and measure the spectrum. Figure 7 As shown, the shaded portion in the figure is the effective structure of the photonic crystal structure disclosed in the present invention.
[0074] In the embodiment of the present disclosure, the photonic crystal laser based on quasi-two-dimensional perovskite is optically characterized, and the characterization results are as follows: Fig. 9 As shown, it is the photoluminescence spectrum of the quasi-two-dimensional perovskite film of the embodiment of the present disclosure, the central wavelength is around 540nm, and the full width at half maximum is about 25nm; Fig.12The figure shows the photoluminescence spectrum of the quasi-two-dimensional perovskite-based photonic crystal laser of the embodiment of the present disclosure, with a central wavelength of about 543nm. It shows that the quasi-two-dimensional perovskite-based photonic crystal laser of the present disclosure achieves single-mode laser emission, the emission band is in the green band, and the quality factor is higher than 200; at the same time, the emission wavelength of the quasi-two-dimensional perovskite-based photonic crystal laser of the present disclosure is adjustable within the photoluminescence spectrum of the quasi-two-dimensional perovskite film.
[0075] like Fig.11 As shown in the figure, the emission spectrum of the photonic crystal laser based on quasi-two-dimensional perovskite of the embodiment of the present disclosure at different pump powers, the results show that it is fluorescence at first, then single-mode laser appears, and as the pump power increases further, the luminescence intensity increases, and other modes appear. This is because within the gain spectrum range of the quasi-two-dimensional perovskite, multiple modes can be supported. At low pump power, the mode with low loss and large gain appears first. As the pump power increases, other modes with relatively high loss can also be generated under high pump conditions.
[0076] According to an embodiment of the present disclosure, phenethylammonium bromide can be replaced by tetrabutylammonium bromide; methylamidinium bromide can be replaced by methylaminoammonium bromide or cesium bromide.
[0077] In the embodiments of the present disclosure, the quasi-two-dimensional perovskite film prepared by using the precursor solution prepared by the above raw materials can effectively gain the output in the green light band.
[0078] According to an embodiment of the present disclosure, when the material of the dielectric film is silicon oxide, the method further includes subjecting the photonic crystal layer to ultraviolet ozone treatment before preparing the quasi-two-dimensional perovskite film.
[0079] In the embodiment of the present disclosure, when the material of the dielectric film is silicon oxide, the photonic crystal layer is subjected to ultraviolet ozone treatment for 15 minutes to improve the wettability of silicon oxide, which is beneficial to the coating of the quasi-two-dimensional perovskite film.
[0080] Figure 4 A scanning electron microscope image of a tetragonal lattice dielectric column photonic crystal structure according to an embodiment of the present disclosure is schematically shown.
[0081] like Figure 4 As shown, an embodiment of the present disclosure provides a method for preparing a dielectric column arranged in a tetragonal lattice, comprising:
[0082] (1) Spin-coat PMMA on a quartz substrate at 4000 rpm and bake at 150 °C for 3 min;
[0083] (2) Spin-coat the conductive adhesive at 2000 rpm and bake at 90°C for 1 min;
[0084] (3) Patterning by electron beam exposure;
[0085] (4) developing with a developer prepared with isopropyl alcohol and methyl isobutyl ketone in a volume ratio of 3:1 for 210 seconds, and then fixing with isopropyl alcohol for 30 seconds;
[0086] (5) using a thermal evaporation method to deposit a magnesium fluoride dielectric layer with a thickness of 100 nm on the patterned electron beam gel;
[0087] (6) The electron beam glue is washed off with acetone and peeled off to obtain dielectric columns with a tetragonal lattice arrangement.
[0088] Figure 5 A scanning electron microscope image of a tetragonal lattice dielectric hole photonic crystal structure according to an embodiment of the present disclosure is schematically shown.
[0089] like Figure 5 As shown, the embodiment of the present disclosure provides a photonic crystal structure of a tetragonal lattice dielectric hole, wherein the shape of the dielectric hole is elliptical.
[0090] Figure 6 A scanning electron microscope image of a triangular lattice dielectric hole photonic crystal structure according to an embodiment of the present disclosure is schematically shown.
[0091] like Figure 6 As shown, the embodiments of the present disclosure provide a photonic crystal structure of triangular lattice dielectric holes.
[0092] Fig.10 The photoluminescence spectrum of a quasi-two-dimensional perovskite-based photonic crystal laser according to an embodiment of the present disclosure is schematically shown.
[0093] like Fig.10 As shown, an embodiment of the present disclosure provides a photonic crystal laser based on quasi-two-dimensional perovskite, wherein the medium hole diameter is 115 nm and the central wavelength is 549 nm. The present disclosure can control the output wavelength by adjusting the size of the unit.
[0094] The embodiments of the present disclosure are described above. However, these embodiments are only for the purpose of illustration and are not intended to limit the scope of the present disclosure. Although the embodiments are described above separately, this does not mean that the measures in the various embodiments cannot be used in combination to advantage. The scope of the present disclosure is defined by the attached claims and their equivalents. Without departing from the scope of the present disclosure, those skilled in the art may make various substitutions and modifications, which should all fall within the scope of the present disclosure.
Claims
1. A photonic crystal laser based on quasi-two-dimensional perovskite, characterized in that: include: The photonic crystal layer comprises a dielectric film having dielectric holes or dielectric columns arranged in an array; A gain medium layer is located on the photonic crystal layer, and the gain medium layer is a quasi-two-dimensional perovskite film; the luminescence spectrum of the quasi-two-dimensional perovskite film covers a range of 510nm-560nm.
2. The quasi-two-dimensional perovskite-based photonic crystal laser according to claim 1, characterized in that: The thickness of the dielectric film is 10nm-200nm, the periods of the dielectric holes and the dielectric columns are both 100nm-800nm, the diameters of the dielectric holes and the dielectric columns are both 50nm-300nm; the thickness of the gain dielectric layer is 50nm-200nm.
3. The quasi-two-dimensional perovskite-based photonic crystal laser according to claim 1, characterized in that: The array arrangement includes a triangular lattice, a tetragonal lattice or a composite lattice.
4. The quasi-two-dimensional perovskite-based photonic crystal laser according to claim 3, characterized in that: The overall size of the arrayed dielectric pores or dielectric columns is greater than 5 μm×5 μm.
5. The quasi-two-dimensional perovskite-based photonic crystal laser according to any one of claims 1 or 2, characterized in that: The material of the dielectric film includes silicon oxide or magnesium fluoride.
6. The quasi-two-dimensional perovskite-based photonic crystal laser according to claim 1, characterized in that: The photonic crystal layer also includes a substrate, and the dielectric film is arranged on the substrate.
7. A method for preparing a quasi-two-dimensional perovskite-based photonic crystal laser according to any one of claims 1 to 6, characterized in that: include: Use optical simulation software to simulate the photonic crystal structure, design the photonic crystal structure, and calculate the photonic band gap; According to the simulation results, a dielectric film having dielectric holes or dielectric columns arranged in an array is generated on the substrate to obtain a photonic crystal layer; The precursor solution is first dripped onto the photonic crystal layer by a spin coating method, and then chlorobenzene is dripped, and annealing treatment is performed to prepare a quasi-two-dimensional perovskite film, thereby obtaining the quasi-two-dimensional perovskite-based photonic crystal laser; The precursor solution is obtained by dissolving phenethylammonium bromide, methylammonium bromide and lead bromide in N,N-dimethylformamide solution.
8. The method for preparing a quasi-two-dimensional perovskite-based photonic crystal laser according to claim 7, characterized in that: The method for preparing the array-arranged dielectric holes comprises: firstly plating a dielectric film on a substrate, and then performing photolithography, etching and cleaning on the dielectric film to obtain the array-arranged dielectric holes.
9. The method for preparing a quasi-two-dimensional perovskite-based photonic crystal laser according to claim 7, characterized in that: The method for preparing the array-arranged dielectric pillars comprises: firstly performing photolithography on a substrate, then coating a dielectric film on the photolithographic substrate, and then cleaning and peeling off to obtain the array-arranged dielectric pillars.
10. The method for preparing a quasi-two-dimensional perovskite-based photonic crystal laser according to claim 9, characterized in that: When the material of the dielectric film is silicon oxide, the method also includes subjecting the photonic crystal layer to ultraviolet ozone treatment before preparing the quasi-two-dimensional perovskite film.