Method for investment casting of high-silicon-molybdenum nodular cast iron
By optimizing the investment casting process and raw material ratio, the problems of poor graphite spheroidization quality and unstable matrix structure in high-silicon molybdenum ductile iron products were solved, achieving stable production and performance improvement of high-silicon molybdenum ductile iron.
Patent Information
- Application Number
- CN202411064725.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-26
AI Technical Summary
Existing investment casting high-silicon molybdenum ductile iron products suffer from poor graphite spheroidization quality, unstable matrix structure, and complex production processes, resulting in reduced performance indicators and high surface roughness.
The mold shell is made of medium-temperature wax, and a mixture of silica sol and zircon powder is used as the surface material. A mixture of silica sol and mullite powder is used as the transition layer and back layer material. The mold shell is roasted in a natural gas roasting furnace. During the molten iron smelting process, a specific proportion of furnace charge and inoculant are added for spheroidization and inoculation treatment. Finally, the mold shell is cast at high temperature.
This has enabled the stable production of high-silicon molybdenum ductile iron products, ensuring stable product strength and performance, meeting processing performance requirements, avoiding additional heat treatment, and resulting in products with low surface roughness and minimal dimensional fluctuations.
Smart Images

Figure CN119016685A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of special material ductile iron casting, and in particular to a method for investment casting of high-silicon-molybdenum ductile iron. Background Art
[0002] At present, ductile iron products at home and abroad are basically produced using sand casting technology. The sand molds are cast at room temperature, and the cooling speed can be controlled by measures such as chills. The production process is simple, the product appearance is rough, and the size fluctuates greatly.
[0003] The production process of investment casting products is complex. The mold shell needs to be cast at high temperature and the cooling rate is uncontrollable, which leads to poor quality of investment casting graphite spheroidization, unstable matrix structure, and reduced performance indicators of castings. However, the advantages of investment casting products are small appearance roughness and small dimensional fluctuation. Summary of the invention
[0004] In order to make up for the deficiencies of the prior art, the present invention provides a method for investment casting high-silicon-molybdenum ductile iron with optimized process, precise control of raw material ratio and stable product performance.
[0005] The present invention is achieved through the following technical solutions: A method for investment casting high silicon-molybdenum ductile iron comprises the following steps: (1) Investment casting shell making: Use medium temperature wax to make the wax pattern, use a mixture of silica sol and zircon powder as the surface layer material of the shell, and use fused quartz sand as the sanding material; use a mixture of silica sol and mullite powder as the transition layer and back layer material of the shell, and use mullite sand as the sanding material. After drying and dewaxing, the final shell is obtained; (2) Shell roasting: The shell is roasted in a natural gas roasting furnace; (3) Hot metal smelting: Pig iron, recycled materials, scrap steel, carburizer, ferromolybdenum, ferrosilicon and silicon carbide are selected as the charge materials and added into the smelting furnace for smelting to obtain hot metal; (4) Spheroidizing treatment: The molten iron is spheroidized by the flushing method; (5) Inoculation treatment: secondary inoculation is adopted, inoculant is added during iron tapping, and secondary inoculation is adopted during casting; (6) Shell casting: During the spheroidization process, the molten shell is taken out of the roasting furnace for casting to obtain the product.
[0006] The invention utilizes the investment casting process to produce QTRSi4Mo1 ductile iron, and undergoes the processes of investment casting shell making, shell roasting, molten iron smelting, spheroidizing treatment, inoculation treatment, shell pouring, etc., and under the premise of ensuring that the strength is not reduced, through the optimization of the preparation process and the control of the raw material ratio, the high silicon-molybdenum ductile iron product can be mass-produced by investment casting, and stable application can be achieved.
[0007] A better technical solution of the present invention is: In step (1), the specific process of investment casting shell making is as follows: a) slowly add wetting agent and defoamer to silica sol in sequence, then add zircon sand powder in batches, and continue stirring until uniform. The viscosity of the final silica sol slurry is measured with a No. 4 James cup to measure 30-45s; b) Soak the wax model in wax model cleaning agent and silica sol in sequence, then immerse it in silica sol slurry, take it out after it is completely immersed, blow the bubbles on the surface with compressed air, immerse it in silica sol slurry again, take it out after it is completely immersed, and then send it to the sand spraying machine to be covered with molten quartz sand. Hang the wax model covered with sand and dry it at a temperature of 23±3℃ and a breeze of 0.5-1m / s for 3-8h to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of 1430 type silica sol and 180-250 mesh mullite powder. In the transition layer slurry, the weight ratio of mullite powder to silica sol is 1.2-2:1, and the drying time is 8-12h; in the back layer slurry, the weight ratio of mullite powder to silica sol is 1-1.5:1, and 0.15-0.25% of carbon fiber by weight of silica sol is added at the same time, and the drying time is 10-24h; in the sealing layer slurry, the weight ratio of mullite powder to silica sol is 0.8-1.2:1, and the drying time is 10-14h; the transition layer, back layer and sealing layer are all dried at a temperature of 23±3℃ and a breeze of 3-5m / s; Ductile iron products undergo graphitization and expansion during solidification, increasing their volume and easily cracking the mold shell, causing molten iron to escape or product surface swelling. Therefore, carbon fiber is added to the back layer as a reinforcing agent to improve the mold shell strength. d) In steps b)-c), the surface layer is made 1-2 times, the transition layer is made 1-2 times, the back layer is made 2-8 times, the sealing layer is made once, and finally the formwork is obtained; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell. The dewaxing time is 15-30 minutes, the dewaxing temperature is 150-170°C, the dewaxing pressure is 0.6-0.7MPa, and the time from closing the dewaxing kettle door to increasing the pressure to the dewaxing pressure is less than 10 seconds.
[0008] Further preferably, in step a), the silica sol is 830 type silica sol, which is used directly without adjusting the content; the fineness of the zircon sand powder is 270-325 mesh, the volume ratio of the wetting agent, the defoaming agent and the silica sol is 1.2-1.7:0.7-1:1000; the mass ratio of the zircon sand powder to the silica sol is 3-4.2:1, and stirring is continued for more than 8 hours until it is uniform.
[0009] Further preferably, in step b), the silica sol is 830 type silica sol, the wax mold is soaked in wax mold cleaning agent for 5-15s, hung up to drip off the liquid and then soaked in silica sol for 3-5s, hung up to drip off the liquid and then immersed in silica sol slurry until it is completely immersed and then taken out, 0.1-0.3MPa compressed gas is used to blow the surface bubbles, immersed in silica sol slurry again until it is completely immersed, then taken out and controlled for 5-10s, and then sent to a sand spraying machine to be covered with 80-120 mesh fused quartz sand. Compared with zircon sand, the use of fused quartz sand powder can reduce the sand powder cost by 2 / 3.
[0010] In step (2), the natural gas roasting temperature is 1050-1150°C, and the roasting time is greater than 45 minutes.
[0011] In step (3), the pig iron is Q10 pig iron; the recycled materials are die heads or scrap materials of the same brand as QTRSi4Mo1, and other recycled materials are not used; the scrap steel is high-quality carbon steel scraps, the carbon content of the carburizer is more than 99%, the ferrosilicon is 75 ferrosilicon, and the silicon carbide content is more than 95%; The above-mentioned raw materials must not have any oil stains, mud, plastic or other debris on the surface, and must be shot blasted, derusted, dehydrated and dried before use; Further preferably, the weight ratio of the above raw materials is 20-30% pig iron, 35-50% recycled materials, 20-30% scrap steel, 0.5-1% recarburizer, 0.7-1.2% ferromolybdenum, 0.5-1.2% ferrosilicon, and 0.5-1% silicon carbide.
[0012] Further preferably, part of the recarburizer is placed in the furnace body, and pig iron, scrap steel, remaining recarburizer and recycled materials are added in sequence. When the molten iron is melted to 60-80% of the capacity of the furnace and the temperature reaches 1400-1450°C, silicon carbide, ferromolybdenum and ferrosilicon are added to melt and samples are taken for component detection. When the component detection is qualified and the charge is fully melted, the molten iron temperature reaches 1550-1600°C and is allowed to stand for slag removal for 3-5 minutes. After the standing period is over, the molten iron is discharged from the furnace at 1450-1530°C.
[0013] In step (4), the spheroidization is carried out by the flushing method. First, a rare earth magnesium spheroidizer is placed on the bottom of the inner side of the dam. The amount of rare earth magnesium spheroidizer added is 0.8-1.3% of the weight of the molten iron. The rare earth magnesium spheroidizer is covered with an inoculant, then covered with iron beans, and finally covered with a layer of slag remover. After each layer of covering material is compacted with a tool such as a wooden stick.
[0014] In step (5), the inoculation in the ladle uses a silicon-barium inoculant with a specification of 2-10 mm and an inoculation amount of 0.5-0.8%; the in-stream inoculation uses a silicon-strontium inoculant with a specification of 0.2-0.7 mm and an inoculation amount of 0.1-0.2%; in order to prevent the spheroidization inoculation decay of the molten iron after the spheroidization inoculation treatment from causing waste, the molten iron must be cast within 10 minutes, and the casting temperature is 1350-1450°C.
[0015] In step (6), the final casting temperature of the molten model shell is controlled at 1000-1100°C. During casting, a layer of slag cleaning agent is sprinkled on the surface of the molten iron in the spheroidizing ladle for slag cleaning and heat preservation. At the same time, slag blocking cotton is placed on the surface of the slag cleaning agent to intercept slag. During the casting process, a 15-30 mesh ceramic filter is placed at the gate position of the molten model shell to filter and block slag, thereby reducing impurities from entering the product.
[0016] The patented technology of the present invention utilizes the investment casting process to produce high silicon-molybdenum ductile iron. Through the optimization of the preparation process and the control of the raw material ratio, the element content (%) of the obtained product QTRSi4Mo1 ductile iron is as follows: C: 2.7-3.5, Si: 4.0-4.5, Mn≤0.3, P≤0.05, S≤0.015, Mo: 1.0-1.5, Mg: 0.01-0.05.
[0017] The present invention optimizes the process and precisely controls the raw material ratio, while ensuring the product spheroidization rate, matrix structure stability, and mechanical properties meet the standards. The product pearlite is less than 15%, and no additional heat treatment is required to eliminate carbides, thereby meeting the product processing performance and product use requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described below in conjunction with the accompanying drawings.
[0019] Figure 1 This is a schematic diagram of the metallographic detection results of the ductile iron obtained in Example 1; Figure 2 This is a schematic diagram of the metallographic detection results of the ductile iron obtained in Example 2; Figure 3 This is a schematic diagram of the metallographic detection results of the ductile iron obtained in Example 3; Figure 4 This is a schematic diagram of the metallographic detection results of the ductile iron obtained in Example 4; Figure 5 This is a schematic diagram of the shell product after casting without adding carbon fiber in Example 4; Figure 6 This is a schematic diagram of the shell product after casting with carbon fiber added in Example 3. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Embodiment 1: A method for investment casting high silicon-molybdenum ductile iron, comprising the following steps: (1) Investment casting shell making: Use medium temperature wax to make wax pattern, use a mixture of silica sol and zircon powder as the surface layer material of the shell, and use fused quartz sand as the sanding material; use a mixture of silica sol and mullite powder as the transition layer and back layer material of the shell, and use mullite sand as the sanding material. After drying and dewaxing, the final shell is obtained. Among them, the silica sol is 830 type silica sol, which is used directly without adjusting the content. The specific process is as follows: a) Slowly add 331 mL of wetting agent (purchased product, main components are polyether-modified siloxane copolymer mixture and modifier) and 276 mL of defoamer (purchased product, main components are dimethyl silicone oil and modifier) to 275 L of silica sol, then add 965 kg of 270-325 mesh zircon sand powder in batches, continue stirring for more than 8 hours until it is uniform, and measure the viscosity of the final silica sol slurry with a No. 4 James cup for 30 seconds; b) Soak the wax model in wax model cleaning agent for 5 seconds, hang it up to drip off the liquid and soak it in 830 type silica sol for 3 seconds, hang it up to drip off the liquid and then immerse it in silica sol slurry until it is completely immersed and then take it out, blow the bubbles on the surface with 0.1Pa compressed gas, immerse it in silica sol slurry again until it is completely immersed and then take it out to control the slurry for 5 seconds, then send it to the sand spraying machine to be covered with 80-120 mesh fused quartz sand, hang up the wax model covered with sand, dry it at 26℃ and 0.5m / s breeze for 3 hours to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of 1430 type silica sol and 180-250 mesh mullite powder. In the transition layer slurry, there are 480kg of mullite powder and 400kg of silica sol, and the drying time is 8h; in the back layer slurry, there are 400kg of mullite powder and 400kg of silica sol, and 0.0015kg of carbon fiber is added at the same time, and the drying time is 10h; in the sealing layer slurry, there are 200kg of mullite powder and 250kg of silica sol, and the drying time is 10h; the transition layer, back layer and sealing layer are all dried at a temperature of 26℃ and a breeze of 3m / s; d) In steps b) to c), the surface layer is made once, the transition layer is made once, the backing layer is made twice, and the sealing layer is made once, and finally the formwork is obtained; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell. The dewaxing time is 15 minutes, the dewaxing temperature is 170°C, the dewaxing pressure is 0.6 MPa, and the time from closing the dewaxing kettle door to increasing the pressure to the dewaxing pressure is less than 10 seconds; (2) Shell roasting: The shell is roasted in a natural gas roasting furnace at a temperature of 1050°C for 46 minutes. (3) Hot metal smelting: 2 kg of recarburizer is placed in the furnace body, and 100 kg of pig iron, 135 kg of scrap steel, 2 kg of recarburizer, and 250 kg of recycled materials are added in sequence. When the hot metal is melted to 70% of the furnace capacity and the temperature reaches 1400°C, 5 kg of silicon carbide, 3.5 kg of ferromolybdenum, and 2.5 kg of ferrosilicon are added to melt and samples are taken for component testing. When the component test is qualified and the furnace charge is fully melted, the hot metal temperature reaches 1600°C and is allowed to stand for 3 minutes to remove slag. After the standing period is over, the hot metal is taken out of the furnace at 1480°C to obtain hot metal; Among them, the pig iron is Q10 pig iron; the recycled materials are die heads or scrap materials of the same brand as QTRSi4Mo1, the carbon content of the carburizer is more than 99%, the ferrosilicon is 75 ferrosilicon, and the silicon carbide content is more than 95%; (4) Spheroidization: Spheroidization adopts the flushing method. First, rare earth magnesium spheroidizer is placed on the bottom of the inner side of the dam. The addition amount of rare earth magnesium spheroidizer is 0.8% of the weight of molten iron. The rare earth magnesium spheroidizer is covered with inoculant, then covered with iron beans, and finally covered with a layer of slag cleaning agent. After each layer of covering materials, it is compacted with a wooden stick or other tools; (5) Inoculation treatment: The secondary inoculation method is adopted. The inoculation in the ladle uses a silicon-barium inoculant with a specification of 2-10mm and an inoculation amount of 0.8%; the inoculation in the flow uses a silicon-strontium inoculant with a specification of 0.2-0.7mm and an inoculation amount of 0.1%; In order to prevent the molten iron from being scrapped due to the decline of spheroidization after spheroidization treatment, the molten iron must be cast within 10 minutes at a casting temperature of 1450°C. (6) Shell casting: During the spheroidizing treatment, the molten shell is taken out of the roasting furnace for casting. The final casting temperature of the molten shell is controlled at 1000°C. During casting, a layer of slag remover is sprinkled on the surface of the molten iron in the spheroidizing ladle for slag removal and heat preservation. At the same time, slag blocking cotton is placed on the surface of the slag remover to intercept slag. During the casting process, a 30-mesh ceramic filter is placed at the gate of the molten shell to filter and block the slag, and finally the product is obtained.
[0022] Embodiment 2: A method for investment casting high silicon-molybdenum ductile iron, the specific steps are the same as those in Embodiment 1, and the parameters different from those in Embodiment 1 are: (1) The specific process of investment casting shell making is as follows: a) Slowly add 324 mL of wetting agent and 151 mL of defoamer to 216 L of silica sol, then add 1036 kg of 270-325 mesh zircon sand powder in batches, and continue stirring for more than 8 hours until it is uniform. The viscosity of the final silica sol slurry is measured by a No. 4 James cup at 45 seconds; b) Soak the wax model in wax model cleaning agent for 15 seconds, hang it up to drip off the liquid and soak it in 830 type silica sol for 5 seconds, hang it up to drip off the liquid and then immerse it in silica sol slurry until it is completely immersed and then take it out, blow the bubbles on the surface with 0.3MPa compressed air, immerse it in silica sol slurry again until it is completely immersed and then take it out to control the slurry for 10 seconds, then send it to the sand spraying machine to be covered with 80-120 mesh fused quartz sand, hang up the wax model covered with sand, dry it at 20℃ and 1m / s breeze for 8 hours to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of 1430 type silica sol and 180-250 mesh mullite powder. In the transition layer slurry, there are 800kg of mullite powder and 400kg of silica sol, and the drying time is 12h; in the back layer slurry, there are 600kg of mullite powder and 400kg of silica sol, and 1kg of carbon fiber is added at the same time, and the drying time is 24h; in the sealing layer slurry, there are 300kg of mullite powder and 250kg of silica sol, and the drying time is 14h; the transition layer, back layer and sealing layer are all dried at a temperature of 20℃ and a breeze of 5m / s; d) In steps b)-c), the surface layer is made 2 times, the transition layer is made 2 times, and the back layer is made 8 times; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell, the dewaxing time is 30 minutes, the dewaxing temperature is 150°C, and the dewaxing pressure is 0.7MPa; (2) Shell roasting: The shell is roasted in a natural gas roasting furnace at a temperature of 1150°C for 50 minutes. (3) Hot metal smelting: 2.5 kg of recarburizer is placed in the furnace body, and 150 kg of pig iron, 150 kg of scrap steel, 2.5 kg of recarburizer and 180.5 kg of recycled materials are added in sequence. When the hot metal is melted to 60% of the furnace capacity and the temperature reaches 1400°C, 2.5 kg of silicon carbide, 6 kg of ferromolybdenum and 6 kg of ferrosilicon are added to melt and samples are taken for component testing. When the component test is qualified and the furnace charge is fully melted, when the hot metal temperature reaches 1550°C, the hot metal is allowed to stand for 5 minutes to remove slag. After the standing period is over, the hot metal is taken out of the furnace at 1450°C to obtain hot metal; (4) Spheroidizing treatment: The amount of rare earth magnesium spheroidizing agent added is 1.3% of the weight of molten iron; (5) Inoculation treatment: The inoculation in the ladle uses a silicon-barium inoculant with a specification of 2-10 mm and an inoculation amount of 0.5%; the in-stream inoculation uses a silicon-strontium inoculant with a specification of 0.2-0.7 mm and an inoculation amount of 0.2%; the molten iron casting temperature is 1350°C; (6) Mold shell casting: The final casting temperature of the molten mold shell is controlled at 1100°C. During the casting process, a 15-mesh ceramic filter is placed at the gate position of the molten mold shell to filter out slag.
[0023] Embodiment 3: A method for investment casting high silicon-molybdenum ductile iron, the specific steps are the same as those in Embodiment 1, and the parameters different from those in Embodiment 1 are: (1) The specific process of investment casting shell making is as follows: a) Slowly add 415 mL of wetting agent and 195 mL of defoamer to 244.5 L of silica sol, then add 1002 kg of 270-325 mesh zircon sand powder in batches, and continue stirring for more than 8 hours until it is uniform. The viscosity of the final silica sol slurry is measured with a No. 4 James cup at 38 seconds; b) Soak the wax model in wax model cleaning agent for 10 seconds, hang it up to drip off the liquid and soak it in 830 type silica sol for 4 seconds, hang it up to drip off the liquid and then immerse it in silica sol slurry until it is completely immersed and then take it out, blow the bubbles on the surface with 0.2MPa compressed gas, immerse it in silica sol slurry again until it is completely immersed and then take it out to control the slurry for 8 seconds, then send it to the sand spraying machine to be covered with 80-120 mesh fused quartz sand, hang up the wax model covered with sand, dry it at 23℃ and 0.8m / s breeze for 5 hours to complete the surface layer production; c) The transition layer, back layer and sealing layer are made of 1430 type silica sol and 180-250 mesh mullite powder. In the transition layer slurry, there are 640kg of mullite powder and 400kg of silica sol, and the drying time is 10h; in the back layer slurry, there are 520kg of mullite powder and 400kg of silica sol, and 8kg of carbon fiber is added at the same time, and the drying time is 15h; in the sealing layer slurry, there are 250kg of mullite powder and 250kg of silica sol, and the drying time is 12h; the transition layer, back layer and sealing layer are all dried at a temperature of 23℃ and a breeze of 4m / s; d) In steps b)-c), the surface layer is applied twice, the transition layer is applied once, and the backing layer is applied five times; e) Place the mold shell in a dewaxing kettle for dewaxing to obtain a cavity shell, the dewaxing time is 25 minutes, the dewaxing temperature is 160°C, and the dewaxing pressure is 0.65MPa; (2) Shell roasting: The shell is roasted in a natural gas roasting furnace at a temperature of 1100°C for 55 minutes. (3) Hot metal smelting: 1.75 kg of recarburizer is placed at the bottom of the furnace, and 125 kg of pig iron, 125 kg of scrap steel, 1.75 kg of recarburizer, and 233 kg of recycled materials are added in sequence. When the hot metal is melted to 70% of the furnace capacity and the temperature reaches 1430°C, 4 kg of silicon carbide, 5 kg of ferromolybdenum, and 4.5 kg of ferrosilicon are added to melt and samples are taken for component testing. When the component test is qualified and the furnace charge is fully melted, the hot metal temperature reaches 1570°C and is allowed to stand for 4 minutes to remove slag. After the standing period is over, the hot metal is taken out of the furnace at 1500°C to obtain hot metal; (4) Spheroidizing treatment: The amount of rare earth magnesium spheroidizing agent added is 1% of the weight of molten iron; (5) Inoculation treatment: The inoculation in the ladle uses a silicon-barium inoculant with a specification of 2-10 mm and an inoculation amount of 0.7%; the inoculation in the stream uses a silicon-strontium inoculant with a specification of 0.2-0.7 mm and an inoculation amount of 0.15%; the molten iron casting temperature is 1400°C; (6) Mold shell casting: The final casting temperature of the molten mold shell is controlled at 1050°C. During the casting process, a 20-mesh ceramic filter is placed at the gate of the molten mold shell to filter out slag.
[0024] Example 4: A method for investment casting high silicon molybdenum ductile iron The specific steps of this embodiment are the same as those of Embodiment 3, except that: (1) in step c) of the specific process of investment casting shell making, no carbon fiber is added to the backing slurry, and molten iron leaks during the casting process, with a ratio of 1.32%.
[0025] The composition of the QTRSi4Mo1 ductile iron obtained in Examples 1-4 was tested, and the results were as follows: It can be seen from the above test results that the high silicon-molybdenum ductile iron product prepared by the method of the present invention has excellent high temperature strength, thermal fatigue performance, excellent oxidation resistance, growth and good creep resistance.
[0026] The performance parameters of the silicon-molybdenum ductile iron obtained in Examples 1-4 were tested, and the results were as follows: It can be seen from the above test results that the QTRSi4Mo1 silicon-molybdenum ductile iron prepared by the method of the present invention fully meets the performance requirements of the GB / T9437-2009 standard, and its specific requirements are as follows: Tensile strength>550Mpa, hardness 200-240HB.
[0027] Combined with Figure 1-4 It can be seen that the metallographic test results of the ductile iron obtained in Examples 1-4 show that the ductile iron graphite prepared by the present invention is spherical, with a small amount of flocculent, a spheroidization rate of 1-3, a graphite ball size of 5-8, a ferrite matrix, a small amount of pearlite and carbide, and fully meets the requirements of GB / T9437-2009 standard.
[0028] Combined with Figure 5-6 It can be seen that Example 4 and Example 3 are the shell conditions after casting without adding carbon fiber and with adding carbon fiber respectively. The shell without adding carbon fiber is partially broken during the casting process, and the molten iron flows out, causing the product to be scrapped. The shell with added carbon fiber is compact and there is no leakage of molten iron.
[0029] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for investment casting of high silicon-molybdenum ductile iron, characterized in that it comprises the following steps: (1) using medium-temperature wax to make a wax mold, using a mixture of silica sol and zircon powder as the surface layer material of the mold shell, and using molten quartz sand as the sanding material; using a mixture of silica sol and mullite powder as the transition layer and back layer material of the mold shell, and using mullite sand as the sanding material, and obtaining the final mold shell after drying and dewaxing; (2) using a natural gas roasting furnace to roast the mold shell; (3) selecting pig iron, recycled materials, scrap steel, carburizer, ferromolybdenum, ferrosilicon, and silicon carbide as furnace materials, adding them into a smelting furnace for smelting to obtain molten iron; (4) using a flushing method to spheroidize the molten iron; (5) using a secondary inoculation method, adding an inoculant when tapping, and using a secondary inoculation with the flow during casting; (6) when the spheroidization treatment is being carried out, the molten mold shell is taken out of the roasting furnace for casting to obtain a product.
2. The method for investment casting high silicon-molybdenum ductile iron according to claim 1, characterized in that: In step (1), the specific process of making the shell of the investment casting mold is as follows: a) slowly adding a wetting agent and a defoaming agent to the silica sol in sequence, and then adding zircon sand powder in batches, and continuously stirring until uniform. The viscosity of the finally prepared silica sol slurry is measured by a No. 4 James cup for 30-45s; b) soaking the wax mold in a wax mold cleaning agent and silica sol in sequence, and then immersing it in the silica sol slurry, taking it out after it is completely immersed, blowing the bubbles on the surface with compressed air, and immersing it in the silica sol slurry again, taking it out after it is completely immersed, and then sending it to a sand spraying machine to be covered with molten quartz sand, hanging the wax mold covered with sand, and drying it at a temperature of 23±3°C and a breeze of 0.5-1m / s for 3-8h to complete the surface layer production; c) the transition layer, back layer, and sealing slurry layer are prepared with 1430 type silica sol and 180-250 mesh mullite powder. In the transition layer slurry, the weight ratio of mullite powder to silica sol is 1.2-2:
1. Drying time is 8-12h; in the backing layer slurry, the weight ratio of mullite powder and silica sol is 1-1.5:1, and 0.15-0.25% of the weight of silica sol is added with carbon fiber, and the drying time is 10-24h; in the sealing layer slurry, the weight ratio of mullite powder and silica sol is 0.8-1.2:1, and the drying time is 10-14h; the transition layer, backing layer, and sealing layer are all at a temperature of 23±3℃, 3-5m / s Dry in a breeze; d) In steps b)-c), the surface layer is made 1-2 times, the transition layer is made 1-2 times, the back layer is made 2-8 times, and the sealing layer is made once to finally obtain the mold shell; e) The mold shell is placed in a dewaxing kettle for dewaxing to obtain a cavity shell, the dewaxing time is 15-30min, the dewaxing temperature is 150-170℃, the dewaxing pressure is 0.6-0.7MPa, and the time from closing the dewaxing kettle door to increasing the pressure to the dewaxing pressure is less than 10s.
3. The method for investment casting high silicon-molybdenum ductile iron according to claim 2, characterized in that: In step a), the silica sol is 830 type silica sol, the fineness of zircon sand powder is 270-325 mesh, the volume ratio of wetting agent, defoaming agent and silica sol is 1.2-1.7:0.7-1:1000; the mass ratio of fused quartz sand powder to silica sol is 3-4.2:1, and stirring is continued for more than 8 hours until uniform.
4. The method for investment casting high silicon-molybdenum ductile iron according to claim 2, characterized in that: In step b), the silica sol is 830 type silica sol, the wax mold is soaked in wax mold cleaning agent for 5-15s, hung up to drip off the liquid and then soaked in silica sol for 3-5s, hung up to drip off the liquid and then immersed in silica sol slurry until it is completely immersed and then taken out, 0.1-0.3MPa compressed gas is used to blow the surface bubbles, immersed in silica sol slurry again until it is completely immersed, then taken out and controlled for 5-10s, and then sent to the sand spraying machine to be covered with 80-120 mesh fused quartz sand.
5. The method for investment casting high silicon-molybdenum ductile iron according to claim 1, characterized in that: In step (2), the natural gas roasting temperature is 1050-1150°C, and the roasting time is greater than 45 minutes.
6. The method for investment casting high silicon-molybdenum ductile iron according to claim 1, characterized in that: In step (3), the pig iron is Q10 pig iron, the recycled material is a die head or scrap material of the same grade as QTRSi4Mo1, the scrap steel is high-quality carbon steel scraps, the carbon content of the recarburizer is more than 99%, the ferrosilicon is 75 ferrosilicon, and the silicon carbide content is more than 95%; the weight ratio of the above raw materials is 20-30% of pig iron, 35-50% of recycled material, 20-30% of scrap steel, 0.5-1% of recarburizer, 0.7-1.2% of ferromolybdenum, 0.5-1.2% of ferrosilicon, and 0.5-1% of silicon carbide.
7. The method for investment casting high silicon-molybdenum ductile iron according to claim 1 or 6, characterized in that: In step (3), part of the recarburizer is placed in the furnace body, and pig iron, scrap steel, remaining recarburizer and recycled materials are added in sequence. When the molten iron is melted to 60-80% of the capacity in the furnace and the temperature reaches 1400-1450°C, silicon carbide, ferromolybdenum and ferrosilicon are added to melt and samples are taken for component detection. After the component detection is qualified and the furnace charge is fully melted, the molten iron is allowed to stand for 3-5 minutes to remove slag when the temperature reaches 1550-1600°C. After the standing is completed, the molten iron is discharged from the furnace at 1450-1530°C.
8. The method for investment casting high silicon-molybdenum ductile iron according to claim 1, characterized in that: In step (4), the spheroidization is carried out by flushing method. First, a rare earth magnesium spheroidizer is placed on the bottom of the inner side of the dam. The amount of rare earth magnesium spheroidizer added is 0.8-1.3% of the weight of the molten iron. The rare earth magnesium spheroidizer is covered with an inoculant, then covered with iron beans, and finally covered with a layer of slag cleaning agent. Each layer of covering material is compacted.
9. The method for investment casting high silicon-molybdenum ductile iron according to claim 1, characterized in that: In step (5), the inoculation in the bag uses a silicon-barium inoculant with a specification of 2-10 mm and an inoculation amount of 0.5-0.8%; The flow inoculation uses a silicon strontium inoculant with a specification of 0.2-0.7mm and an inoculation amount of 0.1-0.2%. The molten iron is cast within 10 minutes and the casting temperature is 1350-1450℃.
10. The method for investment casting high silicon-molybdenum ductile iron according to claim 1, characterized in that: In step (6), the final casting temperature of the molten model shell is controlled at 1000-1100°C. During casting, a layer of slag cleaning agent is sprinkled on the surface of the molten iron in the spheroidizing ladle, and slag blocking cotton is placed on the surface of the slag cleaning agent to intercept slag. During the casting process, a 15-30 mesh ceramic filter is placed at the gate position of the molten model shell to filter and block slag.
Citation Information
Cited By
High-spheroidization-rate spheroidal graphite cast iron for silicon carbide auxiliary spheroidization inoculation and preparation method thereof
CN119332042A