Mechanochromic fluorescent material as well as preparation method and application thereof

By designing a new fluorescent material based on donor-acceptor (D-A) molecules, the problem of unpredictable force chromatability in the prior art is solved, and the reversible force chromatization effect and high force response sensitivity of fluorescent materials are achieved. Various application areas.

CN119019337APending Publication Date: 2024-11-26SHANTOU VOCATIONAL & TECH COLLEGE
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411128032.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The force-discolorability of existing force-discolored organic small molecule materials is difficult to predict and design, and has limited force-discoloration properties, which limits its application in deformation detectors, mechanical sensors and other fields.

Method used

Using a new fluorescent material design based on donor-acceptor (D-A) molecules, a fluorescent material with significant discoloration characteristics was prepared by adding inorganic salts to an organic solvent and reflux reaction.

Benefits of technology

The reversible force-discoloration effect of fluorescent materials is achieved. The conversion of compounds between crystalline and amorphous forms leads to a reversible change in luminescent colors, with high force response sensitivity, and is suitable for fluorescent inks, pressure sensor materials, information security and anti-counterfeiting fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019337A_ABST
    Figure CN119019337A_ABST
Patent Text Reader

Abstract

The invention discloses a mechanochromic fluorescent material and a preparation method and application thereof.The preparation method comprises the steps that a compound i and a compound ii are dissolved in an organic solvent, inorganic salt is added, reflux is conducted for 2-24 h at the temperature of 60-150 DEG C, a compound of a general formula I is prepared, and an R group in the compound of the general formula I is substituted by one of phenoxazine, phenothiazine, 9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9, 10-dihydro-9 The compound is prepared from 9, 9-dimethyl acridine, carbazole and diphenylamine. The mechanochromic fluorescent material has a reversible mechanochromic effect, the luminescent color is reversibly converted because dye molecules are converted between a crystalline state and an amorphous state, and the material has high force response sensitivity and can make color reaction when the material has obvious force change, so that the material can be applied to the field of luminescent materials. The method is applied to the fields of fluorescent ink, pressure sensor materials, information security, anti-counterfeiting and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorescent dyes, and in particular to a mechanochromic fluorescent material and a preparation method and application thereof. Background Art

[0002] Mechanochromic fluorescent materials have attracted extensive attention due to their promising applications in deformation detectors, mechanical sensors, security systems, and storage devices. The mechanochromic properties of organic conjugated materials largely depend on the molecular stacking associated with intermolecular interactions such as π-π, hydrogen bonding, and dipole-dipole interactions. It seems difficult to predict the mechanochromic behavior of chromophores due to the intrinsic complexity of molecular structural factors and intermolecular forces. Therefore, it is also very challenging to achieve major breakthroughs in the rational molecular design of mechanochromic materials. So far, organic small molecule materials with mechanochromic properties are still limited. The present invention demonstrates a new strategy for the design of mechanochromic luminophores based on donor-acceptor (DA) molecules. Summary of the invention

[0003] The purpose of the present invention is to provide a mechanochromic fluorescent material which is easy to synthesize, belongs to a new type of organic fluorescent dye and has significant mechanochromic properties.

[0004] To achieve the above object, the present invention provides a mechanochromic fluorescent material, the molecular structure of which is shown in Formula I as follows:

[0005]

[0006] Wherein, the R group is substituted by one of the following groups: phenoxazine, phenothiazine, 9,10-dihydro-9,9-dimethylacridine, carbazole, diphenylamine.

[0007] Preferably, the fluorescent material comprises five mechanochromic fluorescent compounds C1-C5, the molecular formulas of which are C1:C 35 H 21 N5O, C2:C 35 H 21 N5S, C3:C 38 H 27 N5, C4:C 35 H 21 N5, C5: C 35 H 23 N5.

[0008] An application of a mechanochromic fluorescent material is applied to the fields of fluorescent ink, pressure sensor material, information security and anti-counterfeiting.

[0009] The above-mentioned method for preparing a mechanochromic fluorescent material comprises the following steps:

[0010] Compound i and compound ii are dissolved in an organic solvent in a certain ratio, an inorganic salt is added, and the mixture is refluxed at 60-150° C. for 2-24 hours to prepare a compound of formula I.

[0011] Preferably, the molecular structure of the compound i is:

[0012]

[0013] The molecular structural formula of the compound ii is:

[0014]

[0015] Wherein, the R group is substituted by one of the following groups: phenoxazine, phenothiazine, 9,10-dihydro-9,9-dimethylacridine, carbazole, and diphenylamine.

[0016] Preferably, the molar ratio of compound i to compound ii is 1:1-1:1.5.

[0017] Preferably, the inorganic salt is: K2CO3, Na2CO 3、 One of NaHCO3, Cs2CO3, and Na2S2O5.

[0018] Preferably, the organic solvent is one of methanol, ethanol, acetonitrile, DMF, toluene, chloroform and carbon tetrachloride.

[0019] The advantages and positive effects of the mechanochromic fluorescent material and its preparation method and application described in the present invention are:

[0020] The fluorescent dye of the present invention has a reversible force-induced color change effect. The fluorescent colors of compound C5 before and after grinding are yellow-green and red, respectively. After dichloromethane fumigation, the fluorescent color changes back to yellow-green. This process is mainly due to the transformation of dye molecules between crystalline and amorphous states, resulting in reversible change of luminescent color. This type of material has high force response sensitivity and responds in color when a significant force change occurs in the material. It is applied to fluorescent inks, pressure sensor materials, information security, anti-counterfeiting and other fields.

[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a synthetic route diagram of compounds C1-C5 of the present invention;

[0023] Figure 2 is the hydrogen nuclear magnetic resonance spectrum of C1 of the present invention;

[0024] Figure 3 is the hydrogen nuclear magnetic resonance spectrum of C2 of the present invention;

[0025] Figure 4 is the hydrogen nuclear magnetic resonance spectrum of C3 of the present invention;

[0026] Figure 5 is the hydrogen nuclear magnetic resonance spectrum of C4 of the present invention;

[0027] Figure 6 is the hydrogen nuclear magnetic resonance spectrum of C5 of the present invention;

[0028] Figure 7 is the carbon nuclear magnetic resonance spectrum of C1 of the present invention;

[0029] Figure 8 is the carbon nuclear magnetic resonance spectrum of C2 of the present invention;

[0030] Fig. 9 is the carbon nuclear magnetic resonance spectrum of C3 of the present invention;

[0031] Fig.10 is the carbon nuclear magnetic resonance spectrum of C4 of the present invention;

[0032] Fig.11 is the carbon nuclear magnetic resonance spectrum of C5 of the present invention;

[0033] Fig.12 is the high resolution mass spectrum of C1 of the present invention;

[0034] Fig.13 is the high resolution mass spectrum of C3 of the present invention;

[0035] Fig.14 is the high resolution mass spectrum of C4 of the present invention;

[0036] Fig.15 is the high resolution mass spectrum of C5 of the present invention;

[0037] Fig.16 is a single crystal structure diagram of C4 of the present invention;

[0038] Fig.17 is the fluorescence spectrum of compound C1 of the present invention at an excitation wavelength of 380 nm;

[0039] Fig.18 is the fluorescence spectrum of compound C2 of the present invention at an excitation wavelength of 390 nm;

[0040] Fig.19 This is the fluorescence emission graph of the solid 365nm ultraviolet lamp before and after grinding of the compound C3 of the present invention

[0041] Fig. 20 is the fluorescence spectrum of the compound C3 of the present invention before and after grinding at an excitation wavelength of 390 nm;

[0042] Fig.21It is the fluorescence emission diagram of the solid state 365nm ultraviolet lamp of the compound C4 of the present invention before and after grinding;

[0043] Fig. 22 is the fluorescence spectrum of the compound C4 of the present invention before and after grinding at an excitation wavelength of 380 nm;

[0044] Fig.23 It is the fluorescence emission diagram of the solid state 365nm ultraviolet lamp of the compound C5 of the present invention before and after grinding;

[0045] Fig.24 It is the fluorescence spectrum of the compound C5 of the present invention before and after grinding with an excitation wavelength of 390 nm. DETAILED DESCRIPTION

[0046] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0047] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0048] A mechanochromic fluorescent material, the molecular structure of which is generally described as follows:

[0049]

[0050] Wherein, the R group is substituted by one of the following groups: phenoxazine, phenothiazine, 9,10-dihydro-9,9-dimethylacridine, carbazole, diphenylamine.

[0051] The fluorescent materials include five mechanochromic fluorescent compounds C1-C5, with molecular formulas of C1:C 35 H 21 N5O, C2:C 35 H 21 N5S, C3:C 38 H 27 N5, C4:C 35 H 21 N5, C5: C 35 H 23 N5.

[0052] A mechanochromic fluorescent material is used in fluorescent ink, pressure sensor material, information security and anti-counterfeiting fields.

[0053] A method for preparing a mechanochromic fluorescent material comprises the following steps:

[0054] Compound i and compound ii are dissolved in an organic solvent in a certain ratio, an inorganic salt is added, and the mixture is refluxed at 60-150° C. for 2-24 hours to prepare a compound of formula I.

[0055] The molecular structure of compound i is:

[0056]

[0057] The molecular structure of compound ii is:

[0058]

[0059] Wherein, the R group is substituted by one of the following groups: phenoxazine, phenothiazine, 9,10-dihydro-9,9-dimethylacridine, carbazole, and diphenylamine.

[0060] The molar ratio of compound i to compound ii is 1:1-1:1.5.

[0061] The inorganic salt is one of: K2CO3, Na2CO3, NaHCO3, Cs2CO3, Na2S2O5.

[0062] The organic solvent is one of methanol, ethanol, acetonitrile, DMF, toluene, chloroform and carbon tetrachloride.

[0063] Example 1

[0064] A method for preparing a mechanochromic fluorescent material compound C1 comprises the following steps:

[0065] 20.00 mg of compound i and 26.95 mg of compound ii (R group is phenoxazine) were placed in a reaction bottle with a molar ratio of compound i to compound ii of 1:1.2. 3 mL of ethanol was added, followed by 0.2 mL of 10% (mass concentration) Na2S2O5 aqueous solution. The mixture was heated to reflux for 12 h, cooled and filtered to obtain a pure yellow solid with a yield of 54.5%.

[0066] Example 2

[0067] The molar ratio of compound i to compound ii was changed to 1:1, and the rest was the same as in Example 1, and the product yield was 45.9%.

[0068] Example 3

[0069] The molar ratio of compound i to compound ii was changed to 1:1.5, and the rest was the same as in Example 1, and the product yield was 48.3%.

[0070] Example 4

[0071] A method for preparing a mechanochromic fluorescent material compound C1 comprises the following steps:

[0072] 26.70 mg of compound i and 30.10 mg of compound ii (R group is phenoxazine) were placed in a reaction bottle with a molar ratio of compound i to compound ii of 1:1.2. 2 mL of DMF was added, and then 0.2 mL of 10% Na2S2O5 aqueous solution was added. The solution was heated to reflux for 12 h to obtain a brown turbid solution. The solution was cooled, water was added, and a precipitate was precipitated. The brown solid crude product was obtained by suction filtration. The crude product was subjected to silica gel column chromatography to obtain a yellow solid with a yield of 30.48%.

[0073] Example 5

[0074] A method for preparing a mechanochromic fluorescent material compound C2 comprises the following steps:

[0075] 26.50 mg of compound i and 30.30 mg of compound ii (R group is phenothiazine) were placed in a reaction bottle with a molar ratio of compound i to compound ii of 1:1.2. 2 mL of ethanol was added, and then 0.2 mL of 10% Na2CO3 aqueous solution was added. The solution was heated to reflux for 12 h to obtain a brown turbid solution. The solution was cooled, water was added, and a precipitate was precipitated. The brown solid crude product was obtained by suction filtration. The crude product was subjected to silica gel column chromatography to obtain a yellow solid with a yield of 40.58%.

[0076] Example 6

[0077] A method for preparing a mechanochromic fluorescent material compound C3 comprises the following steps:

[0078] 26.80 mg of compound i and 37.68 mg of compound ii (R group is 9,10-dihydro-9,9-dimethylacridine) were placed in a reaction bottle with a molar ratio of compound i to compound ii of 1:1.2. 2 mL of ethanol was added, and then 0.2 mL of 10% NaHCO3 aqueous solution was added. The solution was heated to reflux for 12 h to obtain a yellow turbid solution. The solution was cooled, water was added, and a precipitate was precipitated. The solution was filtered to obtain a brown solid crude product. The crude product was chromatographed on a silica gel column to obtain a yellow solid with a yield of 73.93%.

[0079] Example 7

[0080] A method for preparing a mechanochromic fluorescent material compound C4 comprises the following steps:

[0081] 27.21 mg of compound i and 34.50 mg of compound ii (R group is carbazole) were placed in a reaction bottle with a molar ratio of compound i to compound ii of 1:1.2. 2 mL of ethanol was added, and then 0.2 mL of 10% Na2S2O5 aqueous solution was added. The solution was heated to reflux for 12 h to obtain a yellow-brown turbid solution. The solution was cooled, water was added, and a precipitate was precipitated. The brown solid crude product was obtained by suction filtration. The crude product was subjected to silica gel column chromatography to obtain a yellow solid with a yield of 86.32%.

[0082] Example 8

[0083] A method for preparing a mechanochromic fluorescent material compound C5 comprises the following steps:

[0084] 57.40 mg of compound i and 65.80 mg of compound ii (R group is diphenylamine) were placed in a reaction bottle with a molar ratio of compound i to compound ii of 1:1.2. 2 mL of ethanol was added, and then 0.2 mL of 10% Na2S2O5 aqueous solution was added. The solution was heated to reflux for 12 h to obtain an orange turbid solution. The solution was cooled, water was added, and a precipitate was precipitated. The solution was filtered to obtain a brown solid crude product. The crude product was purified by silica gel column chromatography to obtain a yellow solid with a yield of 61.62%.

[0085] Example 9

[0086] The C4 compound prepared in Example 7 was recrystallized in ethanol to obtain crystals of the target compound, and its crystal data are shown in Table 1.

[0087] Table 1 Crystal data

[0088]

[0089]

[0090] like Figure 2-15 As shown, the obtained compounds C1-C5 are 1 HNMR, 13 CNMR and mass spectrometry detection, its structural data are:

[0091] C1: 1 H NMR (400MHz, DMSO-d6) δ13.55 (s, 1H), 8.48 (d, J = 7.6Hz, 2H),

[0092] 7.92(s,1H),7.78(d,J=7.7Hz,1H),7.67-7.56(m,7H),7.25(d,J=8.1Hz,1H),6.88-6.63(m,6H),5.98(d,J=5.9Hz,2H). 13 C NMR(100MHz,DMSO-d6)δ175.3,143.7,140.9,137.2,134.0,132.8,131.8,1 30.9,130.2,130.0,129.2,124.3,122.2,115.9,115.5,115.2,113.8,80.5.

[0093] C2: 1H NMR(400MHz,DMSO-d6)δ8.35(d,J=8.4Hz,2H),7.92-7.70(m,

[0094] 2H),7.67(t,8Hz,1H),7.60-7.48(m,6H),7.24(d,J=7.3Hz,2H),7.15-6.98(m,4H),6.64(s,2H). 13 C NMR(101MHz,DMSO-d6)δ142.49,136.59,132.16,130.28,128.96,128.59,127.39,127.22,123.82,114.88,114.62,79.68.

[0095] C3: 1 H NMR(400MHz,DMSO-d6)δ13.58(s,1H),8.52(d,J=8.4Hz,2H),

[0096] 7.93(d,1H),7.77(d,J=8Hz,1H),7.68(t,J=7.1Hz,1H),7.65–7.54(m,6H),7.52(dd,J=7.7,1.1Hz,2H),7.26(d,J=8.2Hz,1H),7.06–6.90(m,4H),6.26(d,J=8.2Hz,2H),1.63(s,6H). 13 C NMR(100MHz,DMSO-d6)δ143.22,140.56,137.21,132.81,132.23,130.91,130.35,130.09,129.75,129.24,127.02,125.96,121.27,115.49,115.24,114.22,80.48,36.07,31.67.

[0097] C4: 1 H NMR(400MHz,DMSO-d6)δ13.57(s,1H),8.51(d,J=8.5Hz,2H),

[0098] 8.28(d,J=7.7Hz,2H),7.93(m,1H),7.89(d,J=7.7Hz,2H),7.79(d,J=8.2Hz,1H),7.68(t,J=7.1Hz,1H),7.65–7.42(m,8H),7.33(t,J=7.3Hz,2H),7.25(d,J=8.4Hz,1H). 13C NMR(100MHz,DMSO-d6)δ175.39,140.23,139.32,137.21,132.81,130.91,130.18,129.23, 129.10,128.62,127.47,126.90,123.51,121.08,120.93,115.50,115.23,110.32,80.41.

[0099] C5: 1 H NMR (400MHz, DMSO-d6) δ13.22 (s, 1H), 8.07 (d, J = 8.7Hz, 2H),

[0100] 7.80(s,1H),7.71–7.64(m,2H),7.62–7.50(m,4H),7.38(t,J=7.7Hz,4H),7.16(dd,J=19.7,8.8Hz,7H),7.04(d,J=8.7Hz,2H). 13 C NMR(100MHz,DMSO-d6)δ149.97,146.87,137.27,132.73,130.91,130.30,129 .62,129.19,128.60,125.76,124.77,121.42,115.57,115.30,100.00,79.88.

[0101] Figure 2-15 This indicates that compounds C1-C5 were successfully synthesized.

[0102] Example 10

[0103] The yellow-green dye molecule C5 prepared in Example 8 was put into a mortar and ground for 2 hours to obtain a red dye molecule. The ground red dye was fumigated with dichloromethane to obtain a yellow-green dye (such as Fig.23 As shown). The fluorescence colors of compound C5 before and after grinding were yellow-green and red, respectively. After dichloromethane fumigation, the fluorescence color returned to yellow-green. This process is mainly due to the conversion of dye molecules between crystalline and amorphous states, resulting in reversible changes in luminescent color; given that this type of material has a high force response sensitivity, it can respond in color when the material undergoes a significant force change. Therefore, it is used in fluorescent inks, pressure sensor materials, information security, anti-counterfeiting and other fields. Solid fluorescence spectrum detection was performed with 390nm as the excitation wavelength, and the results are shown in Fig.24 As shown in the figure, it can be seen that after grinding, the maximum absorption peak of compound C5 red-shifted from 583nm to 660nm.

[0104] Depend on Figure 16-22It can be seen that C3 and C4 will also produce changes similar to C5 before and after grinding and after fluorescence spectrum detection with an excitation wavelength. Therefore, the fluorescent materials of C3 and C4 of the present invention have a reversible mechanochromic effect and can respond in color when the material undergoes a significant force change.

[0105] Therefore, the present invention adopts the above-mentioned mechanochromic fluorescent material, which has a reversible mechanochromic effect, mainly due to the transformation of dye molecules between crystalline and amorphous states, resulting in reversible change of luminescent color; this type of material has a high force response sensitivity and can respond in color when the material undergoes obvious force changes, and is used in fluorescent inks, pressure sensor materials, information security, anti-counterfeiting and other fields.

[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A mechanochromic fluorescent material, characterized in that: The molecular structure formula I of the fluorescent material is as follows: Wherein, the R group is substituted by one of the following groups: phenoxazine, phenothiazine, 9,10-dihydro-9,9-dimethylacridine, carbazole, diphenylamine.

2. The mechanochromic fluorescent material according to claim 1, characterized in that: The fluorescent material comprises five mechanochromic fluorescent compounds C1, C2, C3, C4 and C5, and the molecular formulas are C1:C 35 H 21 N5O, C2:C 35 H 21 N5S, C3:C 38 H 27 N5, C4:C 35 H 21 N5, C5: C 35 H 23 N5.

3. The use of a mechanochromic fluorescent material according to any one of claims 1 to 2, characterized in that: Used in fluorescent inks, pressure sensor materials, information security, and anti-counterfeiting fields.

4. The method for preparing a mechanochromic fluorescent material according to any one of claims 1 to 2, characterized in that: The following steps are involved: The compound i and the compound ii are dissolved in an organic solvent, an inorganic salt is added, and the mixture is refluxed at 60-150° C. for 2-24 hours to prepare a compound of the general formula I.

5. The method for preparing a mechanochromic fluorescent material according to claim 4, characterized in that: The molecular structure of the compound i is: The molecular structural formula of the compound ii is: Wherein, the R group is substituted by one of the following groups: phenoxazine, phenothiazine, 9,10-dihydro-9,9-dimethylacridine, carbazole, and diphenylamine.

6. The method for preparing a mechanochromic fluorescent material according to claim 4, characterized in that: The molar ratio of the compound i to the compound ii is 1:1-1:1.

5.

7. The method for preparing a mechanochromic fluorescent material according to claim 4, characterized in that: The inorganic salt is K2CO3, Na2CO 3、 One of NaHCO3, Cs2CO3, and Na2S2O5.

8. The method for preparing a mechanochromic fluorescent material according to claim 4, characterized in that: The organic solvent is one of methanol, ethanol, acetonitrile, DMF, toluene, chloroform and carbon tetrachloride.

Citation Information

Cited By

  • Mechanical force-induced fluorescent discoloration sensor material as well as preparation method and application thereof

    CN120518546A