Porous polymer containing chalcogenide viologen, synthesis method and photoelectric application based on porous polymer

By preparing porous polymers containing chalcogen elements, the problems of purple essence recovery and toxicity in photocatalysis are solved, and its performance in the fields of photocatalysis and electrochromicity is improved, achieving a more stable free radical state and a stronger Visible light absorption capacity, suitable for photocatalytic and electrochromic applications.

CN119019682AActive Publication Date: 2024-11-26XI AN JIAOTONG UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411115380.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing application of violet essence containing main group in photocatalysis has problems with difficult catalyst recycling and soluble toxicity, and its absorption capacity in the visible light region is weak and the free radical state is not stable enough, resulting in the deactivation of the catalyst, which limits its inactivation in the Applications in the fields of photocatalysis and electrochromicity.

Method used

Using a porous polymer based on chalcogen-containing elements, the SN2 reaction of chalcogen-bridged 4,4'-bipyridine with tetrahedral structure is formed by preparing SN2 of chalcogen-bridged 4,4'-bipyridine with tetrahedral structure. Porous polymers, enhance the stability of the material and the visible light absorption capacity.

Benefits of technology

Improves the electronic cloud state stability and overall material stability of purple essence, enhances visible light absorption capacity, extends the life of excitation state, improves the photocatalytic reaction rate and yield, and shows excellent electrochromic performance, suitable for intelligent windows, monitors and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019682A_ABST
    Figure CN119019682A_ABST
Patent Text Reader

Abstract

The invention discloses a porous polymer containing chalcogenide viologen and a synthesis method thereof based on photoelectric application of the porous polymer, and belongs to the technical field of electrochromic devices and visible light catalysis. The polymer has unique spatial configuration, stable free radical state, prolonged excited state life, narrow band gap width, enhanced visible light absorption capability, and special electron transfer and catalytic performance, so that the catalytic efficiency of the polymer in photocatalytic cross dehydrogenation coupling reaction reaches up to 82%; and excellent hydrogen production efficiency is shown in a visible light catalysis hydrogen production process. Besides, the porous polymer is insoluble in any solvent, has a good cyclic utilization characteristic as a heterogeneous catalyst, and can still maintain relatively high catalytic efficiency after multiple catalytic cycles, so that the porous polymer can be applied to an electrochromic device. Wide application prospects are realized in electrochromic devices, visible light catalysis cross dehydrogenation coupling and visible light catalysis hydrogen production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochromic devices and visible light catalysis, and specifically relates to a porous polymer containing sulfide element viologen, a synthesis method and optoelectronic applications based thereon. Background Art

[0002] As a classic redox species, viologen has shown great application potential in many fields. In particular, viologen has attracted much attention due to its unique properties in photocatalysis, electrocatalysis, electrochromism, photodynamic therapy, organic flow batteries, and host-guest chemistry. Among them, viologen containing main group elements is widely used in photocatalysis, electrochromism, photodynamic therapy and other fields due to its excellent visible light absorption ability, narrower energy gap and stable free radical state.

[0003] However, the applications of main-group element viologens in photocatalysis reported so far are mostly homogeneous catalysis, which has some problems, such as the difficulty in recycling the catalyst after the reaction and the toxicity of the soluble catalyst, thus limiting the further application of main-group element viologens in the field of photocatalysis.

[0004] In order to solve these problems, heterogeneous photocatalysis technology has emerged. Heterogeneous photocatalysis, also known as multiphase photocatalysis, refers to the process in which the photocatalyst and the reaction substrate are completely or partially in different phases during the photocatalytic process. This technology has great potential in solar energy utilization and conversion, and is therefore increasingly favored. Exploring and improving new heterogeneous photocatalysts is a feasible strategy to further optimize the practical application effect of solar energy conversion. Compared with traditional inorganic semiconductor materials, organic photocatalysts have become an important part of promoting the development of new energy technologies due to their light weight, strong structural adaptability, and strong light utilization ability. Inspired by supramolecular chemistry, various two-dimensional / three-dimensional organic photocatalysts have been widely studied and reported, such as supramolecular organic frameworks (SOFs), metal organic frameworks (MOFs), covalent organic frameworks (COFs), and other porous polymers. The emergence of these new organic photocatalysts provides new opportunities for the development of heterogeneous photocatalysis technology. In particular, RV2+-modified multi-cation COFs / POPs materials have attracted much attention in heterogeneous photocatalysis due to their significant redox and free radical stability. This type of material not only has excellent catalytic performance, but also has good stability and recyclability, which provides a new idea for solving the problems existing in homogeneous catalysis of main-group element viologens. Therefore, exploring new heterogeneous photocatalysts based on main-group element viologens has important research value and practical application significance. Summary of the invention

[0005] The existing main-group element viologen compounds have weak absorption capacity in the visible light region, and the free radical state is often not stable enough, which easily leads to catalyst deactivation. The traditional external modification method has limited effect on improving the photoelectric performance of the main-group element viologen compounds, thus limiting their application in the fields of photocatalysis, electrochromism, etc. The present invention aims to provide a porous polymer containing sulfide element viologen, a synthesis method and a photoelectric application based thereon.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a type of porous polymer based on viologen containing chalcogen elements, wherein the porous polymer based on viologen containing chalcogen elements includes the following two structural formulas:

[0008]

[0009] Wherein, E is any one of S, Se and Te; n represents the number of anions, which is the same as the number of cations; and X is any one of Cl, Br, I and PF6.

[0010] The above-mentioned method for synthesizing porous polymers based on chalcogen-containing viologen is characterized by comprising:

[0011] (1) Preparation of chalcogen-containing bridged 4,4'-bipyridine;

[0012] The structural formula of the chalcogen-bridged 4,4'-bipyridine is as follows:

[0013] Wherein, E is S, Se or Te;

[0014] (2) Step (1) 4,4'-bipyridine containing a sulfur element is reacted with tetrakis(4-(bromomethyl)phenyl)methane by S N 2. Preparation of porous polymers based on chalcogen-containing viologen.

[0015] The step (1) of preparing the chalcogen-containing bridged 4,4'-bipyridine comprises:

[0016] Under the protection of inert gas, 3,3'-dibromo-4,4'-bipyridine is dissolved in pre-cooled tetrahydrofuran, and after being fully stirred, chalcogen chloride is added to react fully, and then the temperature is raised to room temperature to remove the solvent. The organic phase is collected after washing and extraction, and then dried, filtered, concentrated and purified by silica gel column to obtain chalcogen bridged 4,4'-bipyridine.

[0017] The chalcogenide chloride is any one of S2Cl2, SeCl2 and TeCl4.

[0018] The molar ratio of the 3,3'-dibromo-4,4'-bipyridine to the chalcogen chloride is 1:1-2; and the reaction conditions are -80°C to -90°C.

[0019] Said by S N 2. The reaction preparation of the porous polymer based on the chalcogen-containing viologen includes: under the protection of an inert gas, dissolving the chalcogen-containing bridged 4,4'-bipyridine and tetrakis(4-(bromomethyl)phenyl)methane in a solvent respectively, then slowly adding them into the reaction system, stirring the reaction, cooling to room temperature after the reaction, precipitating, collecting the precipitate, washing, filtering, and vacuum drying to obtain the porous polymer based on the chalcogen-containing viologen.

[0020] The molar ratio of the sulfur-containing element-bridged 4,4'-bipyridine to tetrakis(4-(bromomethyl)phenyl)methane is 2:1, and the reaction solvent is any one of N-methylpyrrolidone, DMSO or DMF.

[0021] The reaction temperature is 100° C. to 150° C., and the reaction time is 6 days to 8 days. The washing adopts solvents of dichloromethane and water.

[0022] The above-mentioned type of porous polymer based on chalcogen-containing viologen is used in the preparation of electrochromic devices.

[0023] The above-mentioned type of porous polymer based on sulfur-containing viologen is applied in visible light-induced cross-dehydrogenation coupling reaction and visible light-induced hydrogen production.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The chalcogen-containing viologen porous polymer disclosed in the present invention is a class of organic porous polymers. A tetrahedron (diamond structure) spatial configuration is formed by introducing a tetraphenylmethane structure. This structure not only stabilizes the electron cloud state of the viologen, but also enhances the overall stability of the material. The introduction of the chalcogen element further adjusts the electronic structure and optical properties of the material, making it have more superior performance. The polymer has the following properties: a more stable free radical state; a narrower band gap width, stronger visible light absorption; and a prolonged excited state lifetime.

[0026] The present invention discloses a method for synthesizing a chalcogen-containing viologen porous polymer, which synthesizes the chalcogen-containing viologen porous polymer through an SN2 reaction. The method has clear steps, simple operation, high synthesis efficiency and yield. In order to compare the property differences between monomers and polymers, regular tetrahedral model compounds and benzyl chalcogen-containing viologen are also synthesized, which provides strong support for subsequent performance research and application.

[0027] The application of the porous polymer containing chalcogen viologen disclosed in the present invention has a narrower band gap width, enhanced visible light absorption capacity, and longer excited state lifetime due to the formation of a regular tetrahedral structure, which is beneficial to the accumulation of more energy and charge in the photocatalytic process, thereby improving the reaction rate and yield, making it have broad application prospects in the field of photocatalysis, especially in visible light catalytic cross-dehydrogenation coupling reaction and visible light catalytic hydrogen production. At the same time, the polymer also exhibits excellent electrochromic performance, and a reversible color change can be achieved by adjusting the voltage, which provides a new option for the preparation of electrochromic devices and can be used in smart windows, displays, sensors and other fields, with broad application prospects and important research value. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The reaction diagram of the selenium-containing viologen porous polymer and the model compound prepared by the present invention;

[0029] Figure 2 The thermogravimetric curves of the porous polymer and monomer containing selenium viologens of the present invention are shown in FIG. 2+ As a monomer, POP-SeV 2+ It is a porous polymer containing selenium viologen;

[0030] Figure 3 is the diffuse reflection UV / visible absorption spectrum of the selenium-containing viologen porous polymer and monomer of the present invention; wherein Bn-SeV 2+ As a monomer, POP-SeV 2+ Selenium-containing viologen porous polymer

[0031] Figure 4 The electron paramagnetic resonance spectra of the selenium-containing viologen porous polymer, monomer and model compound of the present invention are shown in FIG. 2+ As a monomer, TBn-SeV 2+ As a model compound, POP-SeV 2+ It is a porous polymer containing selenium viologen;

[0032] Figure 5 The fluorescence quantum yield and fluorescence lifetime comparison diagram of the selenium-containing viologen porous polymer and monomer compound of the present invention; wherein Bn-SeV 2+ As a monomer, POP-SeV 2+ It is a porous polymer containing selenium viologen;

[0033] Figure 6 It is the two-dimensional transient absorption spectrum of the regular tetrahedron model compound containing selenium viologen of the present invention;

[0034] Figure 7The ultraviolet-visible absorption spectrum and color change result of the electrochromic device based on the porous polymer containing selenium viologen and the model compound after the voltage is cut off; wherein TBn-SeV 2+ As a model compound, POP-SeV 2+ It is a porous polymer containing selenium viologen;

[0035] Figure 8 The photocatalytic cross-dehydrogenation coupling effect of different systems of the present invention is compared; Bn-SeV 2+ As a monomer, POP-SeV 2+ It is a porous polymer containing selenium viologen;

[0036] Fig. 9 The effect comparison of the photocatalytic cross-dehydrogenation coupling of the selenium-containing viologen porous polymer of the present invention after multiple cycles;

[0037] Fig.10 The graph is a graph showing the change of the photocatalytic hydrogen production of the selenium-containing viologen porous polymer over time;

[0038] Fig.11 This is a diagram showing the effect of multiple cycles of photocatalytic hydrogen production by the selenium-containing viologen porous polymer of the present invention;

[0039] Fig.12 This is a diagram showing the effect of the selenium-containing viologen porous polymer of the present invention performing photocatalytic hydrogen production after the photocatalytic cross-dehydrogenation coupling reaction;

[0040] Fig.13 This is the visible light catalytic mechanism of the selenium-containing viologen porous polymer of the present invention. DETAILED DESCRIPTION

[0041] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0042] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0043] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0044] Example 1

[0045] The selenium-containing viologen porous polymer and model compound prepared by the present invention are shown in the attached Figure 1 As shown, it is prepared by the steps of the following reaction equation, which specifically includes the following steps:

[0046] Preparation of Chalcogen-Containing Bridged 4,4'-Bipyridine (Compound 2)

[0047] (a) Specific steps of the reaction: Under argon protection, 628 mg of 3,3'-dibromo-4,4'-bipyridine (Compound 1) was dissolved in tetrahydrofuran (60 mL), and after being fully stirred, 4.2 mmol of n-butyl lithium was added at -85°C. After reacting for 1 hour, SeCl2 (2.1 mmol) was added. After sufficient reaction, the temperature was raised to room temperature to remove the solvent, and the organic phase was collected after washing and extraction, and then dried, filtered, concentrated and purified by silica gel column to obtain selenium-bridged 4,4'-bipyridine.

[0048]

[0049] Specific steps for preparing compound 3 using compound 2

[0050] (b) Specific steps of the reaction: 0.7 mmol of compound 2 was dissolved in 30 mL of dichloromethane at 60° C., iodomethane (142 mg, 1 mmol) was added, and after sufficient reaction, the mixture was washed with dichloromethane to obtain compound 3.

[0051]

[0052] Preparation of Compound 6 Tetrakis(4-(bromomethyl)phenyl)methane

[0053] (d) The specific steps of the reaction: Under argon protection, 320 mg 5 (1.00 mmol) and 1.10 g titanium bromide (3.00 mmol) were placed in 5 ml of dry dichloromethane, and then 1.08 g of bromomethyl methyl ether (8.00 mmol) was added dropwise at 0°C and heated under reflux for 48 hours. After the reaction was completed, 5 mL of water was added dropwise to the reaction system, the liquid was separated, the aqueous phase was extracted with dichloromethane 3-5 times, the organic phase was collected, washed with water and saturated brine 3-5 times, and then dried over anhydrous magnesium sulfate. The solvent was then removed under reduced pressure, and the mixture was separated and purified using a silica gel column (PE:DCM=1:2) to obtain a white solid 6.

[0054]

[0055] Preparation of compound 6b

[0056] Compound 6 (3.50 g, 5.50 mmol) and triphenylphosphine (462 mg, 1.76 mmol) were placed in a 250 ml round-bottom flask. Diisopropylamine (100 mL) was added and the solution was purged with nitrogen for 30 min. Then bis(triphenylphosphine)palladium dichloride (618 mg, 0.88 mmol), copper iodide (168 mg, 0.88 mmol) and trimethylsilylacetylene (6.2 ml, 44.0 mmol) were added. Cool to -78 ° C and reflux under nitrogen for 24 h. After removing volatile substances in vacuo, the residue was redissolved in chloroform (100 mL), filtered, and the filter paper was washed with 50 mL of chloroform, and then the combined filtrate was washed with distilled water (2×25 mL) and sodium chloride aqueous solution (25 mL), dried over anhydrous magnesium sulfate, and evaporated to dryness under vacuum. The crude product was subjected to flash column chromatography on silica gel with pure n-hexane and n-hexane / ethyl acetate (4:1) as eluent to obtain intermediate compound 6'.

[0057] Compound 6' (2.50 g, 3.54 mmol) was added to a 250 mL round-bottom flask, and 150 ml of acetonitrile was added. The flask was wrapped with aluminum foil, and then silver fluoride (2.70 g, 21.3 mmol) and N-bromosuccinimide (3.79 g, 21.3 mmol) were added. Vacuum was evacuated while stirring, nitrogen was re-injected, and stirred at room temperature for 24 h. Distilled water (200 mL) was added, and the resulting mixture was extracted with ether (4×50 mL). The combined organic layer was washed with saturated sodium bisulfite (40 mL), distilled water (40 mL) and saturated brine (40 mL), and dried over anhydrous magnesium sulfate. The solvent was evaporated under reduced pressure to obtain an orange residue. Further purification was performed by column chromatography (silica gel, hexane / ethyl acetate = 9:1) to obtain the desired compound 6b as a yellow solid.

[0058]

[0059] 1. Preparation of Selenium Viologen-Containing Porous Polymer 7a

[0060] Under argon protection, 200 mg of selenium-containing bipyridine (0.86 mmol) and 300 mg of compound 6 tetrakis(4-(bromomethyl)phenyl)methane (0.43 mmol) were placed in 10 mL of dry N-methylpyrrolidone to obtain a reaction system, which was reacted at 110 °C for 7 days and slowly cooled to room temperature. The precipitate was collected by filtration under reduced pressure, washed with dichloromethane and water several times, and then dried in vacuo to obtain a light yellow solid 7a.

[0061] The reaction equation is as follows:

[0062]

[0063] 2. Preparation of Selenium-containing Viologen Tetrahedral Model Compound 8a

[0064] Under argon environment, 180 mg of unilaterally methylated selenium-containing viologen of compound 3 (0.48 mmol) and 80 mg of tetrakis(4-(bromomethyl)phenyl)methane of compound 6 (0.11 mmol) were placed in 5 mL of dry DMF to obtain a reaction system, which was reacted at 100 °C for 20 h and slowly cooled to room temperature; the precipitate was collected by filtration under reduced pressure, washed with dichloromethane and acetone several times, and then dried in vacuo to obtain a yellow-brown solid 8a.

[0065] The reaction equation is as follows:

[0066]

[0067] 3. Preparation of Selenium-containing Viologen Porous Polymer 7b

[0068] Under argon protection, 200 mg of compound 2 containing selenium bipyridine (0.86 mmol) and 340 mg of compound 6b (0.43 mmol) were placed in 10 mL of dry N-methylpyrrolidone to obtain a reaction system, which was reacted at 110 °C for 7 days and then slowly cooled to room temperature; the precipitate was collected by filtration under reduced pressure, washed with dichloromethane and water several times, and then dried in vacuo to obtain a light yellow solid 7b.

[0069] The reaction equation is as follows:

[0070]

[0071] 4. Preparation of Selenium-containing Viologen Tetrahedral Model Compound 8b

[0072] Under argon protection, 180 mg of unilaterally methylated selenium-containing viologen of compound 3 (0.48 mmol) and 80 mg of compound 6b (0.11 mmol) were placed in 5 mL of dry DMF to obtain a reaction system, which was reacted at 100 °C for 20 h and then slowly cooled to room temperature; the precipitate was collected by filtration under reduced pressure, washed with dichloromethane and acetone several times, and then dried in vacuo to obtain a yellow-brown solid 8b.

[0073] The reaction equation is as follows:

[0074]

[0075] 5. Preparation of Selenium-containing Viologen Porous Polymer Monomer 4

[0076] Under argon environment, 100 mg of selenium-containing bipyridine (0.43 mmol) was placed in 5 mL of benzyl bromide, and the reaction system was reacted at 60 °C for 12 h, then cooled to room temperature, and the precipitate was collected by filtration under reduced pressure. The precipitate was washed several times with dichloromethane and dried under vacuum to obtain a light yellow solid compound 4.

[0077]

[0078] The physical properties and structural analysis of some of the selenium-containing viologen porous polymers prepared in the present invention are as follows:

[0079] Yield, NMR and mass spectrometry of porous polymers, monomers and model compounds containing selenium viologen

[0080] Compound 4, yellow powder, yield: 46%, 1 H NMR (400MHz, DMSO-d6): δ10.31(s,2H),9.58(d,J=6.6Hz,2H),9.48(d,J=6.5Hz,2H),7.67-7.61(m,4H),7.52-7.43(m,6H),6.10(s,4H). 13 C NMR (100MHz, DMSO-d6): δ146.10,145.53,144.19,140.26,133.92,129.67,129.45,129.38,124.40,64.22.HRMS(ESI+)m / z:calculated for C 24 H 20 N2S 2+ ,208.03904,found,208.03884.

[0081] Compound 8a, yellow powder, yield: 33%, 1H NMR (400MHz, DMSO-d6): δ10.44(s,4H),10.16(s,4H),9.57(d,J=4.9Hz,4H),9.52-9.35(m,8H), 9.30(d,J=5.3Hz,4H),7.58(d,J=6.4Hz,8H),7.37(d,J=6.0Hz,8H),6.06(s,8H),4.58(s,12H). 13 C NMR(101MHz,DMSO-d6):147.64,147.03,146.53,145.57,144.34,143.91,141.32,140.67 ,132.02,131.48,129.57,124.74,124.07,64.75,63.98,49.63.HRMS(ESI+)m / z:[M+NH4] + calculated for C 73 H 60 N8Se4 7+ ,231.61449,found,231.64761.

[0082] Compound 7a, yellow powder, 13 C CP / MAS NMR: δ 64.5 (-CH2), 131.1 (benzene ring), 146.1 (pyridine ring).

[0083] Example 2

[0084] (1) Electrochromic devices based on the selenium-containing viologen porous polymer

[0085] An electrochromic device is prepared using the selenium-containing viologen porous polymer prepared in Example 1: two ITO conductive films are bonded together with double-sided tape to form a device substrate having a cavity with a thickness of 50 μm to 100 μm, the selenium-containing viologen porous polymer is dissolved or dispersed in DMSO, and then injected into the cavity of the prepared device substrate, and sealed to obtain an electrochromic device.

[0086] (2) Photocatalytic cross-dehydrogenation coupling reaction based on the selenium-containing viologen porous polymer

[0087] The porous polymer containing selenium viologen prepared in Example 1 was used for photocatalytic cross-dehydrogenation coupling: 20.9 mg (0.1 mmol) of N-phenyl-tetrahydroisoquinoline, (1 mmol, 10 eq) of nitromethane and the porous polymer containing selenium viologen (SeV 2+The molar weight of the molecule is 2 mmol%) in 2 mL of methanol, stirred with a magnetic stirring bar, and the solvent was removed by rotary evaporation. The target product was purified by column chromatography on silica gel using petroleum ether / ethyl acetate (10:1) as the eluent.

[0088] (3) Photocatalytic hydrogen production based on the selenium-containing violet porous polymer

[0089] The selenium-containing viologen porous polymer prepared in Example 1 was used for photocatalytic hydrogen production: the selenium-containing viologen porous polymer 7a (2 mg), PVP-Pt (4 mg) and EDTA (160 mg) were placed in 5 mL of deionized water, bubbled with argon for 30 min, irradiated under a xenon lamp (λ>400 nm) with a light power of 100 mW, and then the hydrogen content was detected by gas chromatography.

[0090] The test results are shown in the attached Figure 2 ~Attached Fig.13 .

[0091] Attached Figure 2 The thermogravimetric curves of the selenium-containing viologen porous polymer compound 7a and the monomer compound 4 of the present invention are shown in FIG. Figure 2 The data show that the monomer begins to lose weight significantly at a lower temperature compared to the selenium-containing viologen porous polymer 7a. The porous polymer maintains its structural integrity at a higher temperature due to its complex cross-linked network structure, thereby delaying the occurrence of mass loss. This indicates that after the polymer is formed, the thermal stability of the system is improved.

[0092] Attached Figure 3 The diffuse reflectance UV / visible absorption spectra of the selenium-containing viologen porous polymer compound 7a and the monomer compound 4 of the present invention are shown in FIG. Figure 3 The data show that due to the formation of a regular tetrahedral structure, the maximum absorption wavelength of the selenium-containing violet porous polymer is red-shifted and the energy gap is significantly reduced, indicating that electrons in the selenium-containing violet porous polymer are more likely to jump from the valence band to the conduction band, thereby increasing the conductivity of the material or making it exhibit more obvious semiconductor properties, providing a basis for its application in optoelectronic materials, photocatalysts and other fields.

[0093] Attached Figure 4 The electron paramagnetic resonance spectra of the selenium-containing viologen porous polymer compound 7a, compound 4 and model compound 8a of the present invention are shown in FIG. Figure 4 The data show that after the formation of the selenium-containing viologen porous polymer, the signal in the EPR spectrum changed significantly compared with the monomer and the model compound, which indicates that the free radical generation ability in the polymer system has been enhanced.

[0094] Attached Figure 5The fluorescence quantum yield and fluorescence lifetime comparison diagram of the selenium-containing viologen porous polymer compound 7a and the monomer compound 4 of the present invention are two important parameters for measuring the fluorescence performance of materials. They reflect the efficiency of the material in converting the absorbed light energy into fluorescence emission and the duration of the fluorescence emission state. Figure 5 The data show that compared with monomer compounds, selenium-containing viologen porous polymers have excellent performance in fluorescence quantum yield and fluorescence lifetime. The unique porous structure not only improves the interaction between molecules and the efficiency of energy transfer, but also prolongs the fluorescence lifetime by reducing non-radiative transitions and fluorescence quenching. This shows that after the formation of selenium-containing viologen porous polymers, the fluorescence lifetime of the system is extended and the quantum yield is increased.

[0095] Attached Figure 6 The two-dimensional transient absorption spectrum of the tetrahedral model compound 8a containing selenium viologen of the present invention is shown in FIG. Figure 6 The data show that under visible light excitation, the selenium-containing viologen tetrahedral model compound 8a exhibits an obvious charge separation state, and the lifetime of the charge separation state is longer than that of the monomer, which is beneficial for its application in photocatalysis.

[0096] Attached Figure 7 The color change and absorption spectrum of the electrochromic device based on the selenium-containing viologen porous polymer compound 7a and the model compound 8a of the present invention are shown in FIG. Figure 7 The data show that when a voltage of -0.8 V is applied, the electrochromic device based on the selenium-containing viologen porous polymer compound 7a turns green, and the absorption at 650 nm in the absorption spectrum gradually increases, which has excellent application potential in the field of electrochromism.

[0097] Attached Figure 8 The effect comparison diagram of different catalytic systems in the cross dehydrogenation coupling reaction of the present invention is shown in the attached figure. Figure 8The data show that the catalytic efficiency of the selenium-containing violet porous polymer compound 7a can reach 82%, which is significantly higher than its monomer form. The polymer porous structure provides abundant adsorption sites and reaction channels for reactant molecules, promotes the enrichment and contact of reactants on the catalyst surface, and thus accelerates the reaction rate; the selenium-containing violet in the polymer acts as an active center, and promotes the key steps in the CDC reaction through its unique redox properties; the interaction between polymer chains further stabilizes the reaction intermediates, reduces the reaction energy barrier, and improves the catalytic efficiency; this shows the advantages of the polymer structure in improving catalytic performance, and also proves that catalysts and light are indispensable for the catalytic process. In the CDC reaction catalyzed by the selenium-containing violet porous polymer, light further improves the catalytic efficiency by synergizing with the catalyst; the CDC reaction, as an important method for constructing carbon-carbon bonds and carbon-heteroatom bonds, is of great significance in the synthesis of complex organic molecules. As an efficient and recyclable catalyst, the selenium-containing violet porous polymer is expected to replace traditional transition metal catalysts and realize a greener and more economical organic synthesis process.

[0098] Attached Fig. 9 The results of the photocatalytic cross-dehydrogenation coupling reaction of the selenium-containing viologen porous polymer compound 7a after multiple cycles are compared. This is an important data for evaluating the stability and reusability of the catalyst. Fig. 9 The data show that even after multiple cycles of catalytic processes, the selenium-containing viologen porous polymer of the present invention can still maintain a high catalytic efficiency, indicating that the catalyst has excellent stability. This stability stems from the protection of the active center by its porous structure, which prevents the loss or inactivation of the active center during the reaction; in addition, the interaction between polymer chains may also enhance the overall structural stability of the catalyst, enabling it to maintain catalytic activity in multiple cycles; this means that the catalyst can be recycled and reused in the same catalytic reaction multiple times, thereby reducing production costs and waste generation. This is of great significance for achieving green chemistry and sustainable development.

[0099] Attached Fig.10 The graph of the photocatalytic hydrogen production of the selenium-containing viologen porous polymer 7a according to the present invention changes with time is shown in FIG. Fig.10 The data shows that the amount of hydrogen produced gradually increases with time, which indicates that the selenium-containing violet porous polymer can continuously and effectively catalyze the decomposition of water molecules into hydrogen under continuous light; the hydrogen production rate is fastest within the first 6 hours, indicating that the catalyst has high activity and stability, and its excellent performance in photocatalytic hydrogen production provides broad prospects for its application in the field of renewable energy.

[0100] Attached Fig.11The photocatalytic hydrogen production effect diagram of the porous polymer 7a containing selenium viologen in the present invention is shown in Figure 1. The performance stability of the catalyst in multiple cycles is one of the key factors for its wide promotion in practical applications. Fig.11 The data show that the selenium-containing violet porous polymer can still maintain a high catalytic effect after multiple cycles. After four cycles, the catalytic effect of the catalyst has hardly decreased, showing excellent catalytic performance, which fully proves the stability and reusability of the catalytic performance of the catalyst in multiple cycles. These excellent properties not only provide strong support for the application of the catalyst in photocatalytic hydrogen production reactions, but also lay a solid foundation for its promotion and application in other related fields.

[0101] Attached Fig.12 The effect diagram of the photocatalytic cross-dehydrogenation coupling reaction of the selenium-containing viologen porous polymer 7a of the present invention and the subsequent photocatalytic hydrogen production is shown in FIG. Fig.12 The data show that after one, two, and three cross-dehydrogenation coupling reactions, the catalyst can continue to produce hydrogen through photocatalysis, which proves that the selenium-containing violet porous polymer of the present invention can be reused in multiple catalytic reactions. The catalyst can not only be reused in CDC reactions, but also be switched between different types of catalytic reactions without significantly affecting its catalytic effect. This characteristic makes the catalyst have a wide range of application prospects in industrial production, can significantly reduce production costs and waste generation, and provides broad prospects for its application in chemical synthesis, drug synthesis, energy conversion and other fields.

[0102] Attached Fig.13 The photocatalytic mechanism of the selenium-containing viologen porous polymer 7a of the present invention is as follows: Fig.13 The results show that the photocatalytic mechanism of the selenium-containing viologen porous polymer of the present invention is:

[0103] Photoexcitation process: The selenium-containing viologen porous polymer of the present invention is irradiated with visible light, and the energy of this part of the photons is absorbed by the polymer, causing its electrons to transition from the ground state to the excited state. This is the initial step of the photocatalytic reaction, which enables the polymer to have the energy and activity required for subsequent chemical reactions;

[0104] Free radical generation: When a polymer is excited to an excited state, the electron distribution inside it changes, forming free radicals. Free radicals are highly active molecules or atomic groups that have unpaired electrons and are therefore able to participate in a variety of chemical reactions.

[0105] Electron transfer process: The generated free radicals then transfer electrons to the catalytic substrate, which is the core step in the photocatalytic reaction and determines the reaction rate and the type of product. In the system of selenium violet porous polymer, electrons are quickly transferred to the catalytic substrate and PVP-Pt through the polymer chain or pore structure;

[0106] Function of PVP-Pt: PVP-Pt acts as a co-catalyst. When the polymer in the free radical state transfers electrons to PVP-Pt, PVP-Pt can further promote the transfer and conversion of electrons and accelerate the catalytic reaction.

[0107] Completion of the catalytic process: During the transfer and conversion of electrons, the catalytic substrate undergoes a redox reaction to generate the desired product, thus completing the entire catalytic process.

[0108] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A porous polymer based on chalcogen-containing viologen, characterized in that: The porous polymer based on chalcogen-containing viologen includes the following two structural formulas: Wherein, E is any one of S, Se and Te; n represents the number of anions, which is the same as the number of cations; and X is any one of Cl, Br, I and PF6.

2. The method for synthesizing a porous polymer based on chalcogen-containing viologen according to claim 1, characterized in that: include: (1) Preparation of chalcogen-containing bridged 4,4'-bipyridine; The structural formula of the chalcogen-bridged 4,4'-bipyridine is as follows: Wherein, E is S, Se or Te; (2) Step (1) 4,4'-bipyridine containing a sulfur element is reacted with tetrakis(4-(bromomethyl)phenyl)methane by S N 2. Preparation of porous polymers based on chalcogen-containing viologen.

3. The method for synthesizing a porous polymer based on chalcogen-containing viologen according to claim 2, characterized in that: The step (1) of preparing the chalcogen-containing bridged 4,4'-bipyridine comprises: Under the protection of inert gas, 3,3'-dibromo-4,4'-bipyridine is dissolved in pre-cooled tetrahydrofuran, and after being fully stirred, chalcogen chloride is added to react fully, and then the temperature is raised to room temperature to remove the solvent. The organic phase is collected after washing and extraction, and then dried, filtered, concentrated and purified by silica gel column to obtain chalcogen bridged 4,4'-bipyridine.

4. The method for synthesizing a porous polymer based on chalcogen-containing viologen according to claim 3, characterized in that: The chalcogenide chloride is any one of S2Cl2, SeCl2 and TeCl4.

5. The method for synthesizing a porous polymer based on chalcogen-containing viologen according to claim 3, characterized in that: The molar ratio of the 3,3'-dibromo-4,4'-bipyridine to the chalcogen chloride is 1:1-2; and the reaction conditions are -80°C to -90°C.

6. The method for synthesizing a porous polymer based on chalcogen-containing viologen according to claim 2, characterized in that: The method for preparing a porous polymer based on chalcogen-containing viologen by SN2 reaction comprises: under the protection of an inert gas, dissolving chalcogen-containing viologen-bridged 4,4'-bipyridine and tetrakis(4-(bromomethyl)phenyl)methane in a solvent respectively, then slowly adding them into a reaction system, stirring the reaction, cooling to room temperature after the reaction, precipitating, collecting the precipitate, washing, filtering, and vacuum drying to obtain a porous polymer based on chalcogen-containing viologen.

7. The method for synthesizing a porous polymer based on chalcogen-containing viologen according to claim 6, characterized in that: The molar ratio of the sulfur-containing element-bridged 4,4'-bipyridine to tetrakis(4-(bromomethyl)phenyl)methane is 2:1, and the reaction solvent is any one of N-methylpyrrolidone, DMSO or DMF.

8. The method for synthesizing a porous polymer based on chalcogen-containing viologen according to claim 6, characterized in that: The reaction temperature is 100° C. to 150° C., and the reaction time is 6 days to 8 days. The washing adopts solvents of dichloromethane and water.

9. Use of the porous polymer based on chalcogen-containing viologen as claimed in claim 1 in the preparation of electrochromic devices.

10. Use of the porous polymer based on chalcogen-containing viologen as claimed in claim 1 in visible light-induced cross-dehydrogenation coupling reaction and visible light-induced hydrogen production.

Citation Information

Patent Citations

  • Polymer memristor made of poly (chalcogenide viologen-triphenylamine) material and used for biological synaptic simulation and neuromorphic calculation and preparation of polymer memristor

    CN114300617A

  • Water-soluble positive ion type supramolecular organic framework covalent nano bionic drug delivery system

    CN114796514A

  • Chalcogenide element-containing 2, 2 '-viologen derivative, synthesis method thereof, composite material based on chalcogenide element-containing 2, 2'-viologen derivative and photoelectric application thereof

    CN118324777A

  • Tetraphenylmethane derivative and light-emitting element containing the same

    JP2003206278A

  • Display device and method of testing the same

    KR1020200120781A