Luminescent material with adjustable red and green emitting colors as well as preparation method and application of luminescent material
By developing the red-green luminescent material Ca1-yCey (Al1-xMnx)12O19 and using Ce3+ to transmit energy to Mn2+, the problem of color crosstalk in RGB colorimetric temperature measurement is solved, and high-sensitivity temperature detection is achieved.
Patent Information
- Application Number
- CN202411123590.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The existing RGB colorimetric temperature measurement technology reduces the relative sensitivity of temperature measurement due to the color crosstalk caused by broadband emission peaks, making it difficult to achieve high-sensitivity temperature detection.
Develop a luminescent material Ca1-yCey (Al1-xMnx)12O19 with adjustable red and green luminescent colors. The luminescent color is controlled through the doping concentration of Ce4+, and the energy transfer of Ce3+ to Mn2+ is used to achieve efficient luminescence of Mn2+ and reduce color cross-instrument. , improve the sensitivity of RGB colorimetric temperature measurement.
The high color purity emission peak of the red-green luminescent material is achieved, and the color crosstalk is reduced. The RGB colorimetric temperature measurement based on the material has obtained a high sensitivity of 2% K-1, which can be accurately detected at a temperature of 350K.
Smart Images

Figure CN119020027A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to a luminescent material with adjustable red and green luminescent colors, a preparation method and application thereof. Background Art
[0002] Fluorescence intensity ratio temperature measurement has attracted wide attention from researchers as an emerging optical temperature measurement method. This technology usually uses luminescent materials with thermally coupled energy levels or dual-wavelength emission as the medium for temperature sensing, and performs temperature sensing through changes in spectral peak position, peak shape or ratio. However, this temperature measurement method requires the use of a spectrometer for fine spectral detection. Therefore, it is difficult to promote this technology to daily life. In order to solve this problem, a simpler and more convenient three-primary color (RGB) colorimetric temperature measurement method has been proposed. This method also uses luminescent materials as the temperature measurement medium. The luminescent color of such luminescent materials needs to change significantly with temperature changes. Then, the fluorescence photos of the luminescent materials are taken by mobile phones or digital cameras, and the temperature-related information can be obtained by analyzing the values of the RGB channels in the photos. The emission spectrum of traditional luminescent materials of this type usually contains a broadband emission peak and a narrower emission peak, and the different thermal stability of the two realizes the change of luminescent color with temperature. However, the broadband emission peak is not conducive to RGB colorimetric temperature measurement, because the most common camera is a CMOS detector based on a Bayer filter, and the broadband emission will be responded to by multiple color channels, which is called color crosstalk. This color crosstalk will distort the channel intensity ratio, thereby reducing the relative sensitivity of RGB colorimetric temperature measurement. Therefore, although RGB colorimetric temperature measurement provides a simpler and more convenient temperature measurement method, the sensitivity obtained based on this type of temperature measurement technology is always low.
[0003] One way to solve the color crosstalk is to obtain a luminescent material with dual-color narrow-band emission, which requires that the two emission peaks have high color purity and different thermal stability. 4+ With Mn 2+ is a group of ions with great potential. Due to the double prohibition of spin parity, Mn 4+ With Mn 2+ The emission peak of Mn usually has extremely high color purity. In addition, the thermal stability of the two is completely different. 4+ because 4 A2 energy level and 4 The intersection of T2 makes its quenching temperature 4 The position of the T2 energy level is related to the Mn 2+ Because the local phonon vibration leads to the breaking of the forbidden zone, it usually exhibits the behavior of "zero-thermal quenching". Therefore, if it is possible to realize Mn 4+ With Mn 2+ The luminescence of the light makes it possible to achieve high-sensitivity RGB colorimetric temperature measurement. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a luminescent material with adjustable red and green luminescent colors, a preparation method and application thereof.
[0005] The first object of the present invention is to provide a luminescent material with adjustable red and green luminescent colors. The chemical formula of the luminescent material with adjustable red and green luminescent colors is: Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 ; Wherein, x and y are mole fractions, and their value ranges are 0.0001≤x≤0.1 and 0.0001≤y≤0.1 respectively.
[0006] Preferably, the value ranges of x and y are 0.0001≤x≤0.05 and 0.0001≤y≤0.06, respectively.
[0007] Preferably, the value range of y is 0.01≤y≤0.03.
[0008] Preferably, the luminescent color coordinates of the luminescent material with adjustable red and green luminescent colors are (a, b); wherein a and b are both coordinate positions of the color coordinates, the value range of a is 0.15≤a≤0.72, and b=-0.84a+0.88.
[0009] Preferably, the red light color purity of the luminescent material with adjustable red and green light colors is 100%, and the green light color purity is 88%.
[0010] The second object of the present invention is to provide a method for preparing a luminescent material having adjustable red and green luminescence, comprising the following steps:
[0011] S1. Using CaCO3, Al2O3, MnO2 and CeO2 as raw materials, according to the chemical formula Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 The stoichiometric ratio of each substance in the mixture is weighed; wherein the molar ratio of CaCO3, Al2O3, MnO2 and CeO2 is 1-y:12(1-x):12x:y;
[0012] S2. Mix and grind the raw materials evenly, sinter at 1100-1700° C. in an air atmosphere for 4-8 hours; grind after naturally cooling to room temperature to obtain the luminescent material with adjustable red and green luminescent colors.
[0013] Preferably, the sintering temperature in step S2 is 1500-1600°C.
[0014] The first purpose of the present invention is to provide a luminescent material with adjustable red and green luminescence for application in the field of RGB colorimetric temperature measurement.
[0015] Compared with the prior art, the present invention can achieve the following beneficial effects:
[0016] 1. The luminescent material with adjustable red and green luminescent colors provided by the present invention has two high color purity emission peaks of red and green, which can reduce color crosstalk. The color of the luminescent material can be adjusted by Ce 4+ The doping concentration of Ce is controlled and can be adjusted continuously from red to green. 4+ Can self-restore to Ce 3+ , Ce 3+ To Mn 2+ Effective energy transfer makes Mn 2+ It exhibits efficient UV absorption in the range of 200-300nm.
[0017] 2. Mn provided by the present invention 2+ With Mn 4+ The luminescent color of the co-activated luminescent material changes significantly with temperature. Based on the three primary colors (RGB) of the material, a 2% K -1 High sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The red and green luminescent color adjustable luminescent materials of Comparative Example 1 and Examples 1 to 6 of the present invention and CaAl 12 O 19 Comparison data of X-ray diffraction patterns of international standard card PDF#84-1613.
[0019] Figure 2 This is a data graph comparing the emission spectra of the red and green luminescent color-adjustable luminescent materials of Comparative Example 1 and Examples 1 to 6 of the present invention; (a) is Comparative Example 1; (b) to (g) are Examples 1 to 6, respectively.
[0020] Figure 3 It is a CIE color coordinate data diagram of the red and green luminescent color adjustable luminescent materials of Comparative Example 1 and Examples 1 to 6 of the present invention.
[0021] Figure 4 Yes Ce 3+ With Mn 2+ Data plot of spectral evidence for energy transfer.
[0022] Figure 5 This is a data diagram of the relationship between RG intensity variation with temperature provided in Example 1 of the present invention.
[0023] Figure 6 It is a data diagram of absolute sensitivity and relative sensitivity based on RGB colorimetric temperature measurement provided according to Example 1 of the present invention. DETAILED DESCRIPTION
[0024] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In the following description, the same modules are represented by the same reference numerals. In the case of the same reference numerals, their names and functions are also the same. Therefore, the detailed description thereof will not be repeated.
[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.
[0026] In the examples, CaCO3, Al2O3, MnO2 and CeO2 are used as raw materials to prepare the luminescent materials with adjustable red and green luminescent colors in each example of the present invention. 4+ Anovalent substitution of Ca 2+ Ca vacancies can be generated, which effectively reduce the Mn 2+ The formation energy of Mn 4+ To Mn 2+ The valence state changes, causing the emission color to change from red Mn 4+ The luminescence gradually changes to green Mn 2+ Many other elements can also generate Ca vacancies and make Mn 4+ To Mn 2+ Valence state transitions, such as La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Ti and Zr. But Ce 4+ In changing Mn 4+ The valence state will also be reduced to Ce 3+ Thus, Mn 2+ Energy transfer. 2+ Due to the double forbiddenness of self-selected parity, the absorption efficiency of excitation light is low, and Ce 3+ Due to the parity-allowed transition, the absorption efficiency of the excitation light is higher (compared to Mn 2+ The absorption efficiency is more than 10 times higher). Therefore, through Ce 3+ To Mn 2+ Energy transfer, i.e. Ce 3+ Sensitized Mn 2+ Can effectively enhance Mn 2+ Based on the discussion of the above inventive concept, the following comparative examples and embodiments are provided.
[0027] Comparative Example 1
[0028] This comparative example prepared Ca(Al 0.998 Mn 0.002 ) 12 O 19 (i.e. Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 When x=0.002 and y=0), the luminescent material powder is prepared as follows:
[0029] S1. First, weigh CaCO3, Al2O3 and MnO2 according to the stoichiometric ratio (molar ratio) of 1:11.976:0.024, grind and mix them evenly to obtain a mixture;
[0030] S2. The obtained mixture was sintered at 1600°C in air atmosphere for 6 hours, and then ground after naturally cooling to room temperature to obtain a Ca(Al 0.998 Mn 0.002 ) 12 O 19 The luminescent material powder exhibits red luminescence under 254nm excitation.
[0031] Example 1
[0032] In this example, Ca 0.99 Ce 0.01 (Al 0.998 Mn 0.002 ) 12 O 19 (i.e. Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 When x=0.002 and y=0.01), the luminescent material powder is prepared as follows:
[0033] S1. First, weigh CaCO3, Al2O3, MnO2 and CeO2 according to the stoichiometric ratio (molar ratio) of 0.99:11.964:0.024:0.01, grind and mix them evenly to obtain a mixture;
[0034] S2. The mixture was sintered at 1600℃ in air atmosphere for 6h, cooled to room temperature naturally and then ground and tested to obtain a compound with the chemical formula of Ca 0.99 Ce 0.01 (Al 0.998 Mn 0.002 ) 12 O 19The luminescent material powder exhibits orange luminescence under 254nm excitation.
[0035] Example 2
[0036] In this example, Ca 0.98 Ce 0.02 (Al 0.998 Mn 0.002 ) 12 O 19 (i.e. Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 When x=0.002 and y=0.02), the luminescent material powder is prepared as follows:
[0037] S1. First, weigh CaCO3, Al2O3, MnO2 and CeO2 according to the stoichiometric ratio (molar ratio) of 0.98:11.964:0.024:0.02, grind and mix them evenly to obtain a mixture;
[0038] S2. The mixture was sintered at 1500℃ in air atmosphere for 6h, cooled to room temperature naturally and then ground and tested to obtain a compound with the chemical formula of Ca 0.98 Ce 0.02 (Al 0.998 Mn 0.002 ) 12 O 19 The luminescent material powder exhibits yellow luminescence under 254nm excitation.
[0039] Example 3
[0040] In this example, Ca 0.97 Ce 0.03 (Al 0.998 Mn 0.002 ) 12 O 19 (i.e. Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 When x=0.002 and y=0.03), the luminescent material powder is prepared as follows:
[0041] S1. First, weigh CaCO3, Al2O3, MnO2 and CeO2 according to the stoichiometric ratio (molar ratio) of 0.97:11.964:0.024:0.03, grind and mix them evenly to obtain a mixture;
[0042] S2. The mixture was sintered at 1500℃ in air atmosphere for 4h, cooled to room temperature naturally and then ground and tested to obtain a compound with the chemical formula of Ca 0.97 Ce 0.03 (Al 0.998 Mn 0.002 ) 12 O 19 The luminescent material powder exhibits light green light under 254nm excitation.
[0043] Example 4
[0044] In this example, Ca 0.96 Ce 0.04 (Al 0.998 Mn 0.002 ) 12 O 19 (i.e. Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 When x=0.002 and y=0.04), the luminescent material powder is prepared as follows:
[0045] S1. First, weigh CaCO3, Al2O3, MnO2 and CeO2 according to the stoichiometric ratio (molar ratio) of 0.96:11.964:0.024:0.04, grind and mix them evenly to obtain a mixture;
[0046] S2. The mixture was sintered at 1400℃ in air atmosphere for 6h, cooled to room temperature naturally and then ground and tested to obtain a compound with the chemical formula of Ca 0.96 Ce 0.04 (Al 0.998 Mn 0.002 ) 12 O 19 The luminescent material powder exhibits green luminescence under 254nm excitation.
[0047] Example 5
[0048] In this example, Ca 0.95 Ce 0.05 (Al 0.998 Mn 0.002 ) 12 O 19 (i.e. Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 When x=0.002 and y=0.05), the luminescent material powder is prepared as follows:
[0049] S1. First, weigh CaCO3, Al2O3, MnO2 and CeO2 according to the stoichiometric ratio (molar ratio) of 0.95:11.964:0.024:0.05, grind and mix them evenly to obtain a mixture;
[0050] S2. The mixture was sintered at 1400℃ in air atmosphere for 4h, cooled to room temperature naturally and then ground and tested to obtain a compound with the chemical formula of Ca 0.95 Ce 0.05 (Al 0.998 Mn 0.002 ) 12 O 19 The luminescent material powder exhibits green luminescence under 254nm excitation.
[0051] Example 6
[0052] In this example, Ca 0.94 Ce 0.06 (Al 0.998 Mn 0.002 ) 12 O 19 (i.e. Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 When x=0.002 and y=0.06), the luminescent material powder is prepared as follows:
[0053] S1. First, weigh CaCO3, Al2O3, MnO2 and CeO2 according to the stoichiometric ratio (molar ratio) of 0.94:11.964:0.024:0.06, grind and mix them evenly to obtain a mixture;
[0054] S2. The mixture was sintered at 1300℃ in air atmosphere for 6h, cooled to room temperature naturally and then ground and tested to obtain a compound with the chemical formula of Ca 0.94 Ce 0.06 (Al 0.998 Mn 0.002 ) 12 O 19 The luminescent material powder exhibits green luminescence under 254nm excitation.
[0055] Embodiment 7-14
[0056] The preparation process is the same as that of Examples 1-6. The raw material ratios, sintering conditions, and color coordinates of the luminescent materials of each example are shown in Table 1.
[0057]
[0058] The RGB colorimetric relative sensitivity comparison between Comparative Example 1 and Examples 1-14 is shown in Table 2.
[0059] Relative sensitivity (%K-1) Comparative Example 1 0 Example 1 2 Example 2 1.5 Example 3 0.8 Example 4 0.01 Example 5 0.02 Example 6 0.01 Example 7 0.3 Example 8 0.5 Example 9 0.03 Example 10 0.05 Embodiment 11 0.5 Example 12 0.01 Example 13 0.01 Embodiment 14 0.02
[0060] Figure 1 The red and green luminescent color adjustable luminescent materials of Comparative Example 1 and Examples 1-6 and CaAl 12 O 19 Comparison results of X-ray diffraction patterns of international standard card PDF#84-1613. Figure 1 It can be seen that changing the raw material ratio does not affect the synthesis of the material, and the diffraction peak shape and peak position do not change significantly and are similar to those of Comparative Example 1.
[0061] Figure 2 The emission spectra of the luminescent materials with adjustable red and green luminescent colors of Comparative Example 1 and Examples 1-6 are shown. Figure 2 It can be seen that Ce 4+ Can effectively change the ratio of the emission spectrum and precisely control Ce 4+ The doping concentration can accurately control the emission color.
[0062] Figure 3 The CIE color coordinates of the luminescent materials with adjustable red and green luminescent colors of Comparative Example 1 and Examples 1-6 are shown. Figure 3 It can be seen that with the 4+ With the increase of doping, the luminescent color gradually changes from red to green.
[0063] Figure 4 Shows Ce 3+ With Mn 2+ Spectroscopic evidence for energy transfer. Figure 4 It can be seen that monitoring Mn 2+ When the emission spectrum of Ce is observed in the excitation spectrum, 3+ The characteristic excitation peak of Ce 3+ Can effectively 2+ Energy transfer.
[0064] Figure 5 The figure shows the relationship between the RG intensity of Example 1 and the temperature. Figure 5 It can be seen that as the temperature increases, the luminescent color of Example 1 gradually changes from red to green.
[0065] Figure 6 The absolute sensitivity and relative sensitivity of Example 1 based on RGB colorimetric temperature measurement are shown. Figure 6 It can be seen that the RGB colorimetric temperature measurement based on Example 1 reached 2%K -1 relative sensitivity.
[0066] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the disclosure of the present invention can be performed in parallel, sequentially or in different orders, as long as the desired results of the technical solution disclosed in the present invention can be achieved, and this document does not limit this.
[0067] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A luminescent material with adjustable red and green luminescent colors, characterized in that: The chemical formula of the luminescent material with adjustable red and green luminescent colors is: Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 ; Wherein, x and y are mole fractions, and their value ranges are 0.0001≤x≤0.1 and 0.0001≤y≤0.1 respectively.
2. The luminescent material with adjustable red and green luminescent colors according to claim 1, characterized in that: The value ranges of x and y are 0.0001≤x≤0.05 and 0.0001≤y≤0.06 respectively.
3. The luminescent material with adjustable red and green luminescent colors according to claim 2, characterized in that: The value range of y is 0.01≤y≤0.
03.
4. The luminescent material with adjustable red and green luminescent colors according to claim 3, characterized in that: The luminescent color coordinates of the luminescent material with adjustable red and green luminescent colors are (a, b); wherein a and b are both coordinate positions of the color coordinates, the value range of a is 0.15≤a≤0.72, and b=-0.84a+0.
88.
5. The luminescent material with adjustable red and green luminescent colors according to claim 4, characterized in that: The red light color purity of the luminescent material with adjustable red and green luminescent colors is 100%, and the green light color purity is 88%.
6. The method for preparing the luminescent material with adjustable red and green light emission according to any one of claims 1 to 5, characterized in that: The steps include: S1. Using CaCO3, Al2O3, MnO2 and CeO2 as raw materials, according to the chemical formula Ca 1-y Ce y (Al 1-x Mn x ) 12 O 19 Weigh the stoichiometric ratio of each substance in the mixture; Wherein, the molar ratio of CaCO3, Al2O3, MnO2 and CeO2 is 1-y:12(1-x):12x:y; S2. Mix and grind the raw materials evenly, sinter at 1100-1700° C. in an air atmosphere for 4-8 hours; grind after naturally cooling to room temperature to obtain the luminescent material with adjustable red and green luminescent colors.
7. The method for preparing the luminescent material with adjustable red and green luminescence according to claim 6, characterized in that: The sintering temperature in step S2 is 1500-1600°C.
8. Application of the red-green luminescent tunable luminescent material according to any one of claims 1 to 5 in the field of RGB colorimetric temperature measurement.