Method for improving structure uniformity and cold upsetting performance of 10B21 cold forging steel
Through billet grinding, low-temperature heating and controlled rolling processes, combined with high-pressure water phosphorus removal and air-cooling cooling, the problem of easy formation of Wei's tissue in 10B21 cold heading steel is solved, significantly improving the tissue uniformity and cold top forging performance, satisfying the satisfaction of Performance requirements of advanced cold heading steel.
Patent Information
- Application Number
- CN202410997635.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
10B21 cold heading steel is prone to form Wei's tissue, resulting in insufficient tissue unevenness and cold top forging performance. It is difficult for the existing technology to completely eliminate Wei's tissue, affecting mechanical properties and fatigue properties.
Through billet grinding, low-temperature heating, controlled rolling and slow cooling processes, the austenite grain size and deformation energy of the billet are reduced, the formation conditions of Wei's tissue are reduced, and the crystal is refined by high-pressure water phosphorus removal and air-cooling cooling. particles to improve tissue uniformity and cold heading performance.
The 10B21 cold heading steel wire produced by Wei's structure ≤1, tensile strength 480-520MPa, elongation 25-35%, cross-section shrinkage 60-75%, meets the requirements of advanced cold heading performance, and the average thickness of the iron oxide sheet is reduced to 14 -27μm, product stability and performance are significantly improved.
Smart Images

Figure CN119020569A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a method for improving the uniformity of 10B21 cold heading steel structure and the cold upsetting performance. Background Art
[0002] Widmanstatten structure refers to the general term for the proeutectoid lamellar (needle) ferrite or lamellar (needle) carbide plus pearlite structure. Under high temperature and large grain state, the proeutectoid structure often preferentially nucleates and grows along certain specific crystal planes of the original austenite structure during its formation, forming a needle-shaped precipitation along a certain crystal plane of austenite. Under an optical microscope, the ferrite or cementite grown from the austenite grain boundary can be observed to be approximately parallel to the microstructure. For cold heading steel, it is generally believed that the Widmanstatten structure increases the heterogeneity of the structure, and the fundamental reason for the formation of the Widmanstatten structure is the coarse original structure formed during the heating process. Although customers have the ability to improve the structure in the subsequent processing, they cannot completely eliminate the serious Widmanstatten structure. It is generally believed that the Widmanstatten structure has a great influence on the mechanical properties (especially impact toughness), fatigue properties and surface coating of cold heading steel.
[0003] Chinese patents CN103572021A and CN110508614A are controlled rolling and controlled cooling processes for eliminating cementite Widmanstatten structure of hypereutectoid tool steel wire rods, which mainly prevents the formation of cementite Widmanstatten structure of hypereutectoid steel by controlling the cooling of rolled materials; Chinese patent CN115896416A is a production method based on eliminating high-quality carbon rounded Widmanstatten structure, which mainly controls the Widmanstatten structure by controlling the heating temperature and rolling speed. Chinese patent CN107326161A is a control method for the Widmanstatten structure of medium-carbon cold heading steel wire rods, which is mainly for medium-carbon cold heading steel without microalloying, and the entire production process is completed at a higher temperature; Chinese patent CN102560253A discloses a method for manufacturing high-quality cold heading steel with uniform organizational properties, which obtains an ideal bainite structure instead of ferrite + pearlite structure by optimizing the composition and rolling process. The factors that often affect the Widmanstatten structure are not only the heating temperature, deformation temperature and cooling rate. For different steel grades, the heating temperature, original structure and cooling rate work together to cause the appearance of the Widmanstatten structure. It is impossible to have a completely covered method to perfectly eliminate the Widmanstatten structure of different steel grades. The 10B21 material involved in the present invention is a hypoeutectoid microalloyed steel with a composition that is very prone to the appearance of the Widmanstatten structure. It is necessary to reduce or eliminate the Widmanstatten structure of the hot-rolled wire through the process parameter control and refined management of the whole process, improve the organizational stability of the product, and improve the cold heading performance. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for improving the uniformity of the structure and the cold forging performance of 10B21 cold heading steel.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a production method for improving the uniformity of the structure and the cold forging performance of 10B21 cold heading steel products, the production method includes billet grinding, billet heating, controlled rolling, and wire cooling processes; in the controlled rolling process, the rolling temperature of the billet in the rough rolling, intermediate rolling and pre-finishing rolling stages is ≥900°C, the temperature entering the finishing mill and reducing the sizing is ≤880°C, and the temperature of the wire laying machine is 790-820°C.
[0006] The steel billet grinding process of the present invention grinds the steel billet to a grinding depth of 0.8-1.6 mm to remove surface defects of the steel billet.
[0007] In the steel billet heating process of the present invention, the ground steel billet is heated in a heating furnace, the soaking temperature is 1000-1030° C., and the heating time is ≤100 min.
[0008] In the wire cooling process of the present invention, the speed of the first roller is 0.20-0.25m / s, the first insulation cover is opened, and the other insulation covers are all closed, so that the wire is in a slow cooling state in the subsequent cooling process, the cooling speed is controlled to be ≤0.8℃ / s, the coiling temperature is ≤550℃, and the wire is coiled on the PF chain for natural air cooling after passing through the coiler.
[0009] The 10B21 cold heading steel wire produced by the method of the present invention has a Widmanstatten structure of ≤1 level, a ferrite+pearlite structure, and meets the high-level cold heading performance requirement of 1 / 4 cold heading without cracking.
[0010] The control method of the present invention is suitable for producing 10B21 cold heading steel wire with a specification of Φ5.5-14mm.
[0011] The 10B21 cold heading steel wire produced by the method of the invention has a tensile strength of 480-520 MPa, an elongation of 25-35%, and a cross-sectional shrinkage of 60-75%.
[0012] The average thickness of the oxide scale of the 10B21 cold heading steel wire produced by the method of the present invention is 14-27 μm.
[0013] The design idea of the present invention is as follows: remove the surface defects of the steel billet by grinding to reduce the impact on the surface quality of the wire rod; reduce the driving force of the organization growth during the heating process of the steel billet by low temperature heating and short time heating, and reduce the austenite grain size of the steel billet under the premise of meeting the requirements of the steel rolling process. Then, dephosphorization is carried out by high-pressure water, and temperature control is not performed in the rough rolling and pre-finishing rolling stages to ensure that the rolled material can fully recover and recrystallize after each deformation during the rolling process, and the austenite grains are refined to the greatest extent. When entering the finishing and sizing units, the temperature of the rolled material is reduced to below 880°C, and the wire drawing temperature is reduced to 790-820°C, so that a large amount of deformation energy accumulated after rapid deformation of the material can be stored. Combined with the lower temperature after wire drawing and the faster cooling rate at the front end of the air cooling line, the grain nucleation position is increased, the driving force of grain growth is reduced, the ratio of nucleation rate to grain growth rate is increased, the austenite grains are refined, and the conditions for the appearance of Widmanstätten structure are reduced. In the subsequent phase transformation process, the cooling is carried out at a slow cooling rate, so that the phase transformation can be fully carried out, the uniformity of the organization is improved, and the cold heading performance is increased. At the same time, the thickness of the oxide scale is reduced to 14-27μm, and the efficiency of removing the scale by shot blasting and pickling is improved.
[0014] The beneficial effect of adopting the above technical scheme is that the Φ5.5-14mm 10B21 cold heading steel wire produced by the method of the present invention has a Widmanstatten structure ≤ level 1, a structure of ferrite + pearlite, the product wire rod has good stability, low tensile strength, and good cross-sectional shrinkage, meeting the high-level cold heading performance requirements of 1 / 4 cold forging without cracking. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is the microstructure diagram of comparative example 1; Figure 2 It is the microstructure diagram of comparative example 2; Figure 3 is the microstructure diagram of Example 1; Figure 4 is the microstructure diagram of Example 2; Figure 5 This is the microstructure diagram of Example 3. DETAILED DESCRIPTION
[0016] The present invention will be further described in detail below in conjunction with specific embodiments.
[0017] Comparative Example 1 This comparative example is a conventional production process, and most manufacturers currently implement similar processes. It is mainly used to compare the organization and performance of the improved and innovative process to clarify the advantages of the improved process in terms of organization uniformity and performance optimization. It involves grinding, heating, rolling, spinning and controlled cooling processes, specifically: Billet grinding process: single-side grinding of billet 1.2mm; Billet heating process: preheating temperature <750℃, heating section temperature 950-1100℃, soaking temperature set at 1100℃, the whole heating process is 105min; Controlled rolling process: rough rolling and intermediate rolling temperature 980℃, finishing rolling and sizing temperature 950℃, wire laying temperature 910℃; Wire cooling process: The speed of the first roller is 0.220m / s, the first insulation cover is opened, and the other insulation covers are all closed. The cooling process is in a slow cooling state, and the cooling speed is controlled to be ≤0.8℃ / s. The coiling temperature is about 600℃. After passing through the coiler, it is coiled on the PF chain for natural air cooling.
[0018] Wire rod structure and performance: Wire rod specification Φ8mm, comparative metallographic structure as Figure 1 As shown. Figure 1 It can be seen that the product obtained in Comparative Example 1 has an obvious Widmanstatten structure, which is level 3, and the structure is ferrite + pearlite, which meets the requirements of no cracking in 1 / 3 cold heading and cracking in 1 / 4 cold heading. The tensile strength is 496MPa, the elongation is 29%, the cross-sectional shrinkage is 66%, and the average thickness of the oxide scale is 38μm.
[0019] Comparative Example 2 This comparative example involves grinding, heating, rolling, spinning and controlled cooling processes, specifically: Billet grinding process: single-side grinding of billet 1.2mm; Billet heating process: preheating temperature <750℃, heating section temperature 950-1100℃, soaking temperature set at 1100℃, the whole heating process is 105min; Controlled rolling process: Rough rolling and intermediate rolling temperature 980℃, finishing rolling and sizing temperature 930℃, wire laying temperature 870℃; Wire cooling process: The speed of the first roller is 0.220m / s, the first insulation cover is opened, and the other insulation covers are all closed. The cooling process is in a slow cooling state, and the cooling speed is controlled to be ≤0.8℃ / s. The coiling temperature is about 600℃. After passing through the coiler, it is coiled on the PF chain for natural air cooling.
[0020] Wire rod structure and performance: Wire rod specification Φ8mm, the metallographic structure of this comparative example is as follows Figure 2 As shown. Figure 2 It can be seen that the product obtained in Comparative Example 2 has an obvious Widmanstatten structure, which is level 2, and the structure is ferrite + pearlite, which meets the requirements of high-grade cold heading steel without cracking in 1 / 4 cold heading. The tensile strength is 501MPa, the elongation is 27%, the cross-sectional shrinkage is 69%, and the average thickness of the oxide scale is 33μm. Example 1
[0021] The present embodiment provides a production method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel products, which involves grinding, heating, rolling, spinning and controlled cooling processes, specifically: Billet grinding process: single-side grinding of billet 1.2mm; Billet heating process: preheating temperature <750℃, heating section temperature 950-1000℃, soaking temperature set at 1020℃, the whole heating process takes 95min; Controlled rolling process: rough rolling and intermediate rolling temperature 955℃, finishing rolling and sizing temperature 850℃, wire laying temperature 800℃; Wire cooling process: The speed of the first roller is 0.22m / s, the first insulation cover is opened, and the other insulation covers are all closed. The cooling process is in a slow cooling state, the cooling speed is controlled at 0.6℃ / s, the coiling temperature is about 510℃, and after passing through the coiler, it is coiled on the PF chain for natural air cooling.
[0022] Wire rod structure and performance: Wire rod specification Φ8mm, the metallographic structure of this embodiment is as follows Figure 3 As shown. Figure 3 It can be seen that the product obtained in this embodiment has no Widmanstatten structure, and the structure is ferrite + pearlite structure, which meets the performance requirements of high-grade cold heading steel without cracking in 1 / 4 cold heading. The tensile strength is 494MPa, the elongation is 31%, the cross-sectional shrinkage is 70%, and the average thickness of the oxide scale is 22μm. Example 2
[0023] The present embodiment provides a production method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel products, which involves grinding, heating, rolling, spinning and controlled cooling processes, specifically: Billet grinding process: single-side grinding of billet 0.8mm; Billet heating process: preheating temperature <750℃, heating section temperature 950-1000℃, soaking temperature set at 1000℃, the whole heating process is 100min; Controlled rolling process: Rough rolling and intermediate rolling temperature 900℃, finishing rolling temperature 835℃, wire laying temperature 805℃; Wire cooling process: The speed of the first roller is 0.23m / s, the first insulation cover is opened, and the other insulation covers are all closed. The cooling process is in a slow cooling state, the cooling speed is controlled at 0.7℃ / s, the coiling temperature is 520℃, and after passing through the coiler, it is coiled on the PF chain for natural air cooling.
[0024] Wire rod structure and performance: Wire rod specification Φ14mm, the metallographic structure of this embodiment is as follows Figure 4 As shown. Figure 4It can be seen that the product obtained in this embodiment has no Widmanstatten structure, and the structure is ferrite + pearlite structure, which meets the performance requirements of high-grade cold heading steel without cracking in 1 / 4 cold heading. The tensile strength is 503MPa, the elongation is 28%, the cross-sectional shrinkage is 68%, and the average thickness of the oxide scale is 24μm. Example 3
[0025] The present embodiment provides a production method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel products, which involves grinding, heating, rolling, spinning and controlled cooling processes, specifically: Billet grinding process: single-side grinding of billet 1.5mm; Billet heating process: preheating temperature <750℃, heating section temperature 950-1000℃, soaking temperature set at 1030℃, the whole heating process takes 90min; Controlled rolling process: Rough rolling and intermediate rolling temperature 970℃, finishing rolling temperature 880℃, wire laying temperature 800℃; Wire cooling process: The speed of the first roller is 0.24m / s, the first insulation cover is opened, and the other insulation covers are all closed. The cooling process is in a slow cooling state, the cooling speed is controlled at 0.5℃ / s, the coiling temperature is 535℃, and after passing through the coiler, it is coiled on the PF chain for natural air cooling.
[0026] Wire rod structure and performance: Wire rod specification Φ14mm, the metallographic structure of this embodiment is as follows Figure 5 As shown. Figure 5 It can be seen that there is no Widmanstatten structure, and the structure is ferrite + pearlite, which meets the performance requirements of high-grade cold heading steel without cracking in 1 / 4 cold heading. The tensile strength is 491MPa, the elongation is 27%, the cross-sectional shrinkage is 67%, and the average thickness of the oxide scale is 19μm. Example 4
[0027] The present embodiment provides a production method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel products, which involves grinding, heating, rolling, spinning and controlled cooling processes, specifically: Billet grinding process: single-side grinding of billet 1.4mm; Billet heating process: preheating temperature <750℃, heating section temperature 950-1000℃, soaking temperature set at 1010℃, the whole heating process takes 98min; Controlled rolling process: rough rolling and intermediate rolling temperature 950℃, finishing rolling and sizing temperature 870℃, wire laying temperature 820℃; Wire cooling process: The speed of the first roller is 0.20m / s, the first insulation cover is opened, and the other insulation covers are all closed. The cooling process is in a slow cooling state, and the cooling speed is controlled at 0.8℃ / s. The coiling temperature is about 500℃. After passing through the coiler, it is coiled on the PF chain for natural air cooling.
[0028] Wire rod structure and performance: The wire rod specification is Φ5.5mm, and the metallographic structure diagram of this embodiment is similar to that of Example 2. The product obtained in this embodiment has no Widmanstatten structure, and the structure is ferrite + pearlite structure, which meets the performance requirements of high-grade cold heading steel without cracking in 1 / 4 cold heading. The tensile strength is 507MPa, the elongation is 28%, the cross-sectional shrinkage is 69%, and the average thickness of the oxide scale is 17μm. Example 5
[0029] The present embodiment provides a production method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel products, which involves grinding, heating, rolling, spinning and controlled cooling processes, specifically: Billet grinding process: single-side grinding of billet 1.6mm; Billet heating process: preheating temperature <750℃, heating section temperature 950-1000℃, soaking temperature set at 1025℃, the whole heating process takes 85min; Controlled rolling process: Rough rolling and intermediate rolling temperature 945℃, finishing rolling temperature 835℃, wire laying temperature 795℃; Wire cooling process: The speed of the first roller is 0.25m / s, the first insulation cover is opened, and the other insulation covers are all closed. The cooling process is in a slow cooling state, the cooling speed is controlled at 0.57℃ / s, the coiling temperature is 550℃, and after passing through the coiler, it is coiled on the PF chain for natural air cooling.
[0030] Wire rod structure and performance: The wire rod specification is Φ8mm, and the metallographic structure diagram of this embodiment is similar to that of Example 2. The product obtained in this embodiment has no Widmanstatten structure, and the structure is ferrite + pearlite structure, which meets the performance requirements of high-grade cold heading steel without cracking in 1 / 4 cold heading. The tensile strength is 499MPa, the elongation is 27%, the cross-sectional shrinkage is 69%, and the average thickness of the oxide scale is 21μm. Example 6
[0031] The present embodiment provides a production method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel products, which involves grinding, heating, rolling, spinning and controlled cooling processes, specifically: Billet grinding process: single-side grinding of billet 1.2mm; Billet heating process: preheating temperature <750℃, heating section temperature 950-1000℃, soaking temperature set at 1015℃, the whole heating process takes 95min; Controlled rolling process: Rough rolling and intermediate rolling temperature 960℃, finishing rolling temperature 840℃, wire laying temperature 790℃; Wire cooling process: The speed of the first roller is 0.2m / s, the first insulation cover is opened, and the other insulation covers are all closed. The cooling process is in a slow cooling state, the cooling speed is controlled at 0.65℃ / s, the coiling temperature is 480℃, and after passing through the coiler, it is coiled on the PF chain for natural air cooling.
[0032] Wire rod structure and performance: The wire rod specification is Φ8mm, and the metallographic structure diagram of this embodiment is similar to that of Example 2. The product obtained in this embodiment has no Widmanstatten structure, and the structure is ferrite + pearlite structure, which meets the performance requirements of high-grade cold heading steel without cracking in 1 / 4 cold heading. The tensile strength is 486MPa, the elongation is 30%, the cross-sectional shrinkage is 70%, and the average thickness of the oxide scale is 18μm.
[0033] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A method for improving the uniformity of the structure and cold forging performance of 10B21 cold heading steel, characterized in that: The production method includes billet grinding, billet heating, controlled rolling, and wire cooling processes; in the controlled rolling process, the rolling temperature of the billet in the rough rolling, intermediate rolling and pre-finishing rolling stages is ≥900°C, the temperature of entering the finishing mill and reducing the diameter is ≤880°C, and the temperature of the laying head is 790-820°C.
2. The method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel according to claim 1, characterized in that: The steel billet grinding process grinds the steel billet to a grinding depth of 0.8-1.6 mm.
3. The method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel according to claim 1, characterized in that: In the steel billet heating process, the ground steel billet is heated in a heating furnace, the soaking temperature is 1000-1030° C., and the heating time is ≤100 min.
4. The method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel according to claim 1, characterized in that: In the wire cooling process, the speed of the first roller is 0.20-0.25m / s, the first insulation cover is opened, and the other insulation covers are all closed, so that the wire is in a slow cooling state in the subsequent cooling process, the cooling speed is controlled to be ≤0.8℃ / s, the coiling temperature is ≤550℃, and the wire is coiled on the PF chain for natural air cooling after passing through the coiler.
5. A method for improving the uniformity of the structure and the cold forging performance of 10B21 cold heading steel according to any one of claims 1 to 4, characterized in that: The 10B21 cold heading steel wire produced by the method has a Widmanstatten structure of ≤1 level, a structure of ferrite+pearlite, and meets the high-level cold heading performance requirement of 1 / 4 cold heading without cracking.
6. A method for improving the uniformity of the structure and the cold forging performance of 10B21 cold heading steel according to any one of claims 1 to 4, characterized in that: The control method is suitable for producing 10B21 cold heading steel wire with a specification of Φ5.5-14mm.
7. A method for improving the uniformity of the structure and the cold upsetting performance of 10B21 cold heading steel according to any one of claims 1 to 4, characterized in that: The 10B21 cold heading steel wire produced by the method has a tensile strength of 480-520 MPa, an elongation of 25-35%, and a cross-sectional shrinkage of 60-75%.
8. A method for improving the uniformity of the structure and the cold forging performance of 10B21 cold heading steel according to any one of claims 1 to 4, characterized in that: The average thickness of the oxide scale of the 10B21 cold heading steel wire produced by the method is 14-27 μm.
Citation Information
Patent Citations
Method for manufacturing high-quality high-strength cold forging steel with uniform texture performance
CN102808131A
Pearlite spheroidizing method based on high-speed wire production line
CN111659731A
Annealing-free cold heading steel with high cold heading performance and high plasticity, manufacturing method of annealing-free cold heading steel and fastener
CN117403127A
Dehumidification system with gas separating membrane
KR102566489B1