Vanadium precipitation method of sodium vanadium solution

By using a composite vanadium deposition agent with melamine, ethylenediamine and glutaraldehyde aqueous solution and vanadium seeds, the problems of excessive ammonium ions in wastewater in the prior art and difficulty in treating vanadium liquid are solved, and high efficiency and low The cost of sodium vanadium liquid vanadium precipitation process is suitable for large-scale industrial production.

CN119020615APending Publication Date: 2024-11-26YANGTZE NORMAL UNIVERSITY +5
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411113775.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing industrial vanadium deposition treatment, commonly used ammonium salts improve the vanadium deposition effect, but it causes excessive ammonium ion content in wastewater, which increases the difficulty and cost of wastewater treatment. It is difficult to effectively treat vanadium liquid containing high concentrations of chromium, which affects industrialization. Sustainability and environmental protection requirements of large-scale production.

Method used

Using a composite vanadium precipitant agent, including a mixture of melamine, ethylenediamine and glutaraldehyde aqueous solution and vanadium-containing seeds, adjust the pH value of vanadium liquid and heat it, induce selective precipitation of vanadium elements, reduce the entrainment of sodium impurities, and achieve efficient deposition. Vanadium and reduce wastewater treatment costs.

Benefits of technology

It improves the purity of vanadium sedimentation products and the density of precipitates of vanadium liquid, reduces the use of ammonium salts in vanadium sedimentation process, reduces the cost of wastewater treatment, and achieves low-cost clean production, which is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020615A_ABST
    Figure CN119020615A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of vanadium precipitation, and discloses a vanadium precipitation method of a sodium vanadium solution, which comprises the following steps: S1, taking the sodium vanadium solution, removing impurities, filtering, and taking filtrate for later use; s2, taking the filtrate, adding a composite vanadium precipitation agent, adjusting the pH value of the filtrate to 2.2-2.5, carrying out a heating reaction, and filtering to obtain a vanadium precipitate; according to the vanadium precipitation method of the sodium vanadium solution, the technological process is more convenient, ammonium-free vanadium precipitation can be achieved, the vanadium precipitation effect is kept level or obviously better than that of an existing vanadium precipitation process, and the vanadium precipitation method is suitable for large-scale industrial production. The problem that more convenient and environment-friendly industrial vanadium precipitation is difficult to realize on the basis of keeping an efficient vanadium precipitation effect in the prior art can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vanadium precipitation, and in particular to a method for vanadium precipitation from sodium vanadium solution. Background Art

[0002] Vanadium slag refers to the solid slag containing vanadium oxide obtained by oxidative blowing of vanadium-containing molten iron in the process of vanadium extraction or by wet vanadium extraction of vanadium-containing iron concentrate. Vanadium slag is the main raw material for the production of vanadium oxide. In the traditional production of vanadium oxide, crude vanadium slag is mostly obtained by blast furnace / converter process, and then sodium carbonate is added as an additive to roast the crude vanadium slag. The roasted product is leached in water to obtain sodium vanadium extraction leachate, and then after further removing impurities such as phosphorus and silicon, ammonium salt is added. Ammonium polyvanadate can be precipitated under acidic conditions, and the obtained ammonium polyvanadate can be used to produce downstream products.

[0003] For the above-mentioned sodium vanadium precipitation process, the vanadium precipitation effect of the sodium vanadium solution is currently mainly improved by a vanadium precipitation agent, thereby improving the efficiency and degree of vanadium precipitation. For example, the patent with publication number CN113800562A provides a method for preparing high-purity vanadium pentoxide by sodium salt vanadium precipitation of a sodium vanadate solution, by adjusting the pH of the sodium vanadate and adding a silicon removal agent, first removing impurities from the sodium vanadate solution to eliminate the influence of silicon on the vanadium precipitation effect, and then adjusting the pH of the solution to precipitate sodium salts, thereby precipitating vanadium precipitation products, and washing, calcining and other treatments to obtain high-purity vanadium pentoxide.

[0004] Another example is the patent with publication number CN112239806A, which provides a method for extracting vanadium from acidic high-phosphorus vanadium liquid. First, an oxidant is added to the acidic high-phosphorus vanadium liquid for treatment, and the vanadium liquid is filtered to obtain the vanadium liquid. Then, the vanadium is precipitated by adjusting the pH and adding a vanadium precipitating agent, and then calcined to obtain vanadium pentoxide. This technology first oxidizes the acidic high-phosphorus vanadium liquid before vanadium precipitation, which can reduce the vanadium loss in the subsequent vanadium extraction process, thereby improving the vanadium precipitation effect.

[0005] However, the existing vanadium precipitation process mentioned above is difficult to effectively treat vanadium liquid containing high concentration of chromium, and the ammonium content in the wastewater after vanadium precipitation is relatively high, which makes wastewater treatment difficult and costly. It is not suitable for large-scale industrial production and treatment, which is contrary to the development needs of green sustainability and energy conservation and environmental protection. Summary of the invention

[0006] The technical problems to be solved by the present invention are:

[0007] At present, in the existing industrial vanadium precipitation treatment, ammonium salts are often used to improve the vanadium precipitation effect, but the introduction of ammonium salts will cause the problem of excessively high ammonium ion content in the wastewater, resulting in great difficulty and high cost in wastewater treatment. That is, the present invention aims to reduce the difficulty and cost of treating byproducts such as wastewater, while improving the vanadium precipitation effect of sodium vanadium solution and reducing the content of impurity elements such as sodium in the vanadium precipitation product.

[0008] The technical solution adopted by the present invention is:

[0009] The present invention provides a method for precipitating vanadium from sodium vanadium solution, comprising the following steps:

[0010] S1 takes sodium vanadium solution, removes impurities, filters, and takes the filtrate for later use;

[0011] S2 takes the filtrate, adds a composite vanadium precipitant, adjusts the pH value of the filtrate to 2.2-2.5, heats to 85-95°C for reaction, and filters to obtain a vanadium precipitate;

[0012] The composite vanadium precipitation agent comprises at least one of the following formula a and formula b:

[0013]

[0014]

[0015] Preferably, in step S1, the impurity removal method is: adding an impurity remover to the sodium vanadium solution, stirring the reaction, filtering, and removing impurity precipitation to obtain the filtrate;

[0016] Calculated by mass fraction, the impurity remover includes 10-20wt% of polyaluminium chloride, 50-70wt% of aluminium sulfate and 20-30wt% of magnesium stearate.

[0017] Preferably, the sodium vanadium solution has a vanadium content of 5-50 g / L, a sodium content of 10-100 g / L, a chromium content of 1-30 g / L, a silicon content of 0.2-2 g / L, and a phosphorus content of ≤0.05 g / L;

[0018] The amount of the impurity remover added is 2-3 times the silicon content in the sodium vanadium solution by mass.

[0019] Preferably, before adding the impurity remover, the pH value of the sodium vanadium solution is adjusted to 4-5.

[0020] Preferably, the vanadium precipitate obtained in step S2 is dried, calcined at 500-550° C. for 2-4 hours, and cooled to obtain vanadium pentoxide.

[0021] Preferably, in step S2, the method for preparing the composite vanadium precipitation agent comprises the following steps:

[0022] Melamine, ethylenediamine and glutaraldehyde aqueous solution are mixed and heated to 50-60° C. for reaction; the reaction product is then mixed and stirred with vanadium-containing seed crystals to obtain the composite vanadium precipitation agent.

[0023] Preferably, the ratio of melamine, ethylenediamine and glutaraldehyde aqueous solution is 8-10:2.5-3.5:1 based on molar mass, and the mass concentration of glutaraldehyde aqueous solution is 2-5wt%.

[0024] Preferably, the vanadium-containing seed crystals are selected from one or more of vanadium pentoxide or ammonium polyvanadate.

[0025] Preferably, the ratio of melamine to vanadium-containing seed crystals is 0.04-0.15:1 by mass.

[0026] Preferably, the ratio of the composite vanadium precipitating agent to the vanadium content in the filtrate is 0.1-0.2:1 by mass.

[0027] The beneficial effects of the present invention are as follows:

[0028] In terms of vanadium precipitation products, the present invention uses a mixture of melamine, ethylenediamine and glutaraldehyde, combined with vanadium-containing seed crystals, as a composite vanadium precipitation agent. The formed multi-dentate ligand can selectively complex vanadium. In the subsequent vanadium precipitation reaction, the vanadium element in the vanadium liquid is induced to quickly and selectively precipitate around the seed crystals, so as to reduce the situation in which a large amount of sodium ions are entrained into the precipitation in conventional acid hydrolysis vanadium precipitation, thereby improving the product purity. The obtained precipitate has a large particle density and a high bulk density, and there is almost no flaky precipitation of hydrolysis vanadium precipitation.

[0029] In terms of process effect, the vanadium precipitation method of sodium vanadium liquid proposed by the present invention does not need to introduce ammonium salt for treatment, and first removes silicon and phosphorus, which can realize the efficient utilization of vanadium and chromium resources and solve the problem of high cost of ammonia nitrogen wastewater treatment; and compared with the traditional acidic ammonium salt vanadium precipitation process, the amount of precipitant is significantly reduced, and the vanadium precipitation rate is significantly faster, and the vanadium precipitation treatment can reach more than 98% of the vanadium precipitation rate in 30 minutes. In actual industrial applications, the vanadium precipitation method of the present invention has low process cost and simple process route, can realize low-cost clean production, and can be applied to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the hydrogen spectrum of the composite vanadium precipitation agent in Example 1. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0032] The present invention provides a method for vanadium precipitation from sodium vanadium solution, which can achieve higher purity vanadium precipitation from sodium vanadium solution through a simpler process and a more efficient vanadium precipitation process. The specific process is as follows:

[0033] (1) taking sodium vanadium solution, wherein the pH value of the solution is about ≥9, the vanadium content is 5-50 g / L, the sodium content is 10-100 g / L, the chromium content is 1-30 g / L, the silicon content is 0.2-2 g / L, and the phosphorus content is ≤0.05 g / L; adjusting the pH value of the sodium vanadium solution to 4-5 with sulfuric acid, adding an impurity remover, reacting at room temperature for 20-30 minutes, filtering to remove impurities and precipitates, and taking the filtrate for standby use.

[0034] The impurity remover is a mixture of polyaluminium chloride, aluminium sulfate and magnesium stearate, wherein the content of polyaluminium chloride is 10-20wt%, the content of aluminium sulfate is 50-70wt% and the content of magnesium stearate is 20-30wt%; the amount of the impurity remover added is 2-3 times the silicon content in the sodium vanadium solution. The above soluble aluminium salts are added to the sodium vanadium solution in the form of saturated aqueous solution to achieve the best dispersion effect and save water.

[0035] (2) Adding a composite vanadium precipitant to the filtrate after impurity removal, adjusting the pH value of the solution to 2.2-2.5 with sulfuric acid, heating to 85-95° C. for reaction for 50-80 minutes, filtering, and obtaining a vanadium precipitate.

[0036] The preparation method of the composite vanadium precipitation agent comprises the following steps:

[0037] Melamine, ethylenediamine and 2-5wt% glutaraldehyde aqueous solution are mixed in a molar mass ratio of 8-10:2.5-3.5:1, and reacted at 50-60°C for 0.75-1.5h, and then the reaction product is mixed and stirred with vanadium-containing seed crystals for 5min to carry out complexation, thereby obtaining a composite vanadium precipitation agent;

[0038] The main effective substances in the composite vanadium precipitation agent include the following formula a and / or formula b:

[0039]

[0040] The vanadium-containing seed crystals can be vanadium pentoxide or ammonium polyvanadate, the mass ratio of melamine to the vanadium-containing seed crystals is controlled to be 0.04-0.15:1, and the mass ratio of the composite vanadium precipitator to the vanadium content in the filtrate is 0.1-0.2:1.

[0041] In the preparation process of composite vanadium precipitation agent, the main chemical reaction processes involved are as follows:

[0042]

[0043] (3) drying the vanadium precipitate, calcining it at 500-550° C. for 2-4 hours, and cooling it to obtain a vanadium pentoxide product.

[0044] The vanadium precipitation method of the sodium vanadium liquid of the present invention uses glutaraldehyde to slightly cross-link the organic amine, thereby increasing the complexing ability of the amino group to the vanadium element and providing hydrophilic groups such as hydroxyl groups to improve the water solubility of the organic amine. The organic amine can capture polyvanadate and act on vanadium-containing seed crystals. When the mixed vanadium precipitation agent acts on the vanadium-containing seed crystals, the polyvanadate ions in the vanadium liquid can be induced to be rapidly and selectively precipitated around the seed crystals, and the vanadium-containing seed crystals can ensure that the precipitation grows uniformly, thus achieving a corresponding or even more significant vanadium precipitation effect under the condition of omitting the ammonium salt reagent and extraction steps required by the traditional vanadium precipitation process.

[0045] Example 1

[0046] After testing, the sodium vanadium solution to be treated has a total vanadium content of 48.73 g / L, a Na content of 53.62 g / L, a Cr content of 5.27 g / L, a Si content of 1.63 g / L, a P content of 0.023 g / L, and a pH value of 12.1. The sodium vanadium solution is treated as follows:

[0047] Step 1: Mix 12 g of melamine, 1.9 g of ethylenediamine and 50 mL of 2 wt% glutaraldehyde aqueous solution, stir, heat to 50° C. and react for 1 h, then add 51 g of ammonium polyvanadate and stir for 5 min to obtain a composite vanadium precipitator for later use.

[0048] Step 2: Take 160g of aluminum sulfate 18hydrate, 30g of polyaluminum chloride and 50g of magnesium stearate respectively, add deionized water, and dilute to 400mL to obtain an impurity remover solution for later use.

[0049] Step 3: Take 5L of sodium vanadium solution to be treated, adjust the pH value of the solution to about 4 with sulfuric acid, add 400mL of impurity remover solution, react at room temperature for 20 minutes, then filter to remove the precipitate, take the filtrate and set aside.

[0050] Step 4: Add the mixed vanadium precipitant prepared in step 1 to the filtrate obtained in step 3, heat to 90°C for reaction, add sulfuric acid during the reaction to keep the pH value of the solution at about 2.2, react for 60 minutes, filter and obtain a vanadium precipitate.

[0051] Step 5: Dry the vanadium precipitate and calcine it in a furnace at 500℃ for 3h to obtain vanadium pentoxide, whose bulk density is about 0.69g / cm 3 .

[0052] Example 2

[0053] After testing, the sodium vanadium solution to be treated has a total vanadium content of 55.71 g / L, a Na content of 61.60 g / L, a Cr content of 7.32 g / L, a Si content of 2.52 g / L, a P content of 0.027 g / L, and a pH value of 12.7. The sodium vanadium solution is treated as follows:

[0054] Step 1: 13.8 g of melamine, 2.2 g of ethylenediamine and 58 mL of 2 wt% glutaraldehyde aqueous solution were mixed, stirred, heated to 50° C. for reaction for 1 h, and then 53 g of ammonium polyvanadate was added and stirred for 5 min to obtain a composite vanadium precipitator for standby use.

[0055] Step 2: Take 156 g of aluminum sulfate 18hydrate, 25 g of polyaluminum chloride and 57 g of magnesium stearate respectively, add deionized water, and dilute to 400 mL to obtain an impurity remover solution for later use.

[0056] Step 3: Take 5L of sodium vanadium solution to be treated, adjust the pH value of the solution to about 4 with sulfuric acid, add 400mL of impurity remover solution, react at room temperature for 20 minutes, then filter to remove the precipitate, take the filtrate and set aside.

[0057] Step 4: Add the mixed vanadium precipitant prepared in step 1 to the filtrate obtained in step 3, heat to 93°C for reaction, add sulfuric acid during the reaction to keep the pH value of the solution at about 2.1, react for 70 minutes, filter and obtain a vanadium precipitate.

[0058] Step 5: Dry the vanadium precipitate and calcine it in a furnace at 540°C for 3 hours to obtain vanadium pentoxide, whose bulk density is about 0.65 g / cm 3 .

[0059] Example 3

[0060] After testing, the sodium vanadium solution to be treated has a total vanadium content of 51.58 g / L, a Na content of 58.16 g / L, a Cr content of 5.59 g / L, a Si content of 1.92 g / L, a P content of 0.034 g / L, and a pH value of 11.6. The sodium vanadium solution is treated as follows:

[0061] Step 1: Mix 12.8 g of melamine, 2 g of ethylenediamine and 53 mL of 2 wt% glutaraldehyde aqueous solution, stir, heat to 50° C. and react for 1 h, then add 52 g of ammonium polyvanadate and stir for 5 min to obtain a composite vanadium precipitator for later use.

[0062] Step 2: Take 148 g of aluminum sulfate 18hydrate, 35 g of polyaluminum chloride and 60 g of magnesium stearate respectively, add deionized water, and dilute to 400 mL to obtain an impurity remover solution for later use.

[0063] Step 3: Take 5L of sodium vanadium solution to be treated, adjust the pH value of the solution to about 4 with sulfuric acid, add 400mL of impurity remover solution, react at room temperature for 20 minutes, then filter to remove the precipitate, take the filtrate and set aside.

[0064] Step 4: Add the mixed vanadium precipitant prepared in step 1 to the filtrate obtained in step 3, heat to 90°C for reaction, add sulfuric acid during the reaction to keep the pH value of the solution at about 2.1, react for 75 minutes, filter and obtain a vanadium precipitate.

[0065] Step 5: Dry the vanadium precipitate and calcine it in a furnace at 550°C for 2.5 hours to obtain vanadium pentoxide, whose bulk density is about 0.68 g / cm 3 .

[0066] Example 4

[0067] After testing, the sodium vanadium solution to be treated has a total vanadium content of 42.36 g / L, a Na content of 50.48 g / L, a Cr content of 3.73 g / L, a Si content of 2.07 g / L, a P content of 0.032 g / L, and a pH value of 11.3. The sodium vanadium solution is treated as follows:

[0068] Step 1: Mix 10.5 g of melamine, 1.65 g of ethylenediamine and 43 mL of 2 wt% glutaraldehyde aqueous solution, stir, heat to 50° C. and react for 1 h, then add 50 g of ammonium polyvanadate and stir for 5 min to obtain a composite vanadium precipitator for later use.

[0069] Step 2: Take 150 g of aluminum sulfate 18hydrate, 42 g of polyaluminum chloride and 67 g of magnesium stearate respectively, add deionized water, and dilute to 400 mL to obtain an impurity remover solution for later use.

[0070] Step 3: Take 5L of sodium vanadium solution to be treated, adjust the pH value of the solution to about 4 with sulfuric acid, add 400mL of impurity remover solution, react at room temperature for 20 minutes, then filter to remove the precipitate, take the filtrate and set aside.

[0071] Step 4: Add the mixed vanadium precipitant prepared in step 1 to the filtrate obtained in step 3, heat to 90°C for reaction, add sulfuric acid during the reaction to keep the pH value of the solution at about 2.2, react for 75 minutes, filter and obtain a vanadium precipitate.

[0072] Step 5: Dry the vanadium precipitate and calcine it in a furnace at 550°C for 3 hours to obtain vanadium pentoxide, whose bulk density is about 0.67 g / cm 3 .

[0073] Comparative Example 1

[0074] After testing, the sodium vanadium solution to be treated has a total vanadium content of 48.73 g / L, a Na content of 53.62 g / L, a Cr content of 5.27 g / L, a Si content of 1.63 g / L, a P content of 0.023 g / L, and a pH value of 12.1. The following treatment is performed:

[0075] Step 1: Take 150g of aluminum sulfate 18hydrate, 42g of polyaluminum chloride and 67g of magnesium stearate respectively, add deionized water, and dilute to 400mL to obtain an impurity remover solution for later use.

[0076] Step 2: Take 5L of sodium vanadium solution to be treated, adjust the pH value of the solution to about 4 with dilute sulfuric acid, add 400mL of impurity remover solution, react at room temperature for 20 minutes, then filter to remove the precipitate, take the filtrate and set aside.

[0077] Step 3: Control the temperature of the reaction system to 90°C, add 20g of melamine to the filtrate obtained in step 2, and add sulfuric acid to keep the pH value of the solution at about 2.0, continue stirring at 300rpm, react for 120min, filter, and obtain vanadium precipitate.

[0078] Step 4: Place the vanadium precipitate in 300 mL of pure water, add dilute sulfuric acid to adjust the pH value of the solution to about 2, stir for 30 minutes, filter, and take the vanadium precipitate; dry the vanadium precipitate, place it in a furnace at 550°C and calcine it for 4 hours to obtain vanadium pentoxide, whose bulk density is about 0.23 g / cm 3 .

[0079] Comparative Example 2

[0080] After testing, the sodium vanadium solution to be treated has a total vanadium content of 48.73 g / L, a Na content of 53.62 g / L, a Cr content of 5.27 g / L, a Si content of 1.63 g / L, a P content of 0.023 g / L, and a pH value of 12.1. The following treatment is performed:

[0081] Step 1: Take 150g of aluminum sulfate 18hydrate, 42g of polyaluminum chloride and 67g of magnesium stearate respectively, add deionized water, and dilute to 400mL to obtain an impurity remover solution for later use.

[0082] Step 2: Take 5L of sodium vanadium solution to be treated, adjust the pH value of the solution to about 4 with dilute sulfuric acid, add 400mL of impurity remover solution, react at room temperature for 20 minutes, then filter to remove the precipitate, take the filtrate and set aside.

[0083] Step 3: Control the temperature of the reaction system to 95°C, add 390g of ammonium sulfate to the filtrate obtained in step 2, and add sulfuric acid to keep the pH value of the solution at about 2.0, continue stirring at 300rpm, react for 90min, filter, and obtain vanadium precipitate.

[0084] Step 4: Place the vanadium precipitate in 300 mL of pure water, add dilute sulfuric acid to adjust the pH value of the solution to about 2, stir for 30 minutes, filter, and take the vanadium precipitate; dry the vanadium precipitate, place it in a 550° C. furnace and calcine it for 4 hours to obtain vanadium pentoxide.

[0085] After testing, the waste liquid filtered in step 4 has an ammonium ion concentration of 2.7 g / L and a bulk density of about 0.30 g / cm 3 .

[0086] Test example

[0087] (1) Figure 1 As shown, 1g of the composite vanadium precipitating agent prepared in Example 1 is taken, dissolved in 2mL of deuterated chloroform, and the synthetic compound hydrogen spectrum (1H NMR) is obtained by testing with a Brook full digital nuclear magnetic resonance spectrometer (300MHz), and the peak attribution at each chemical shift is shown in the figure, with a peak area of ​​1 at 3.32ppm, a peak area of ​​4.3 at 6.94ppm, a peak area of ​​1.2 at 5.95ppm, a peak area of ​​1.3 at 5.95ppm, a peak area of ​​2.3 at 5.31ppm, a peak area of ​​2.4 at 4.63ppm, and a peak area of ​​3.9 at 2.8ppm, thereby verifying that the compound structure of the actual composite vanadium precipitating agent is substantially consistent with the theoretical reaction structure, and the partial peak area is larger due to containing two main effective substances, formula a and formula b. In addition, by the relationship between the mass of the composite vanadium precipitating agent and the total mass of the raw materials melamine, ethylenediamine and glutaraldehyde, the yield of the composite vanadium precipitating agent is calculated to be about 86.05%.

[0088] (2) The vanadium precipitation effects in Examples 1 to 4 and Comparative Examples 1 to 2 were measured respectively, specifically the content of each substance or element in the product. The results are summarized in Table 1 below:

[0089] Table 1 Component content of vanadium precipitation products in different tests (unit: wt%)

[0090] <![CDATA[V2O5]]> Na Si P YB / T 5304-2017 98.0 1.0 0.2 0.03 Example 1 98.6 0.3 0.09 <0.01 Example 2 98.3 0.33 0.08 <0.01 Example 3 98.6 0.32 0.09 <0.01 Example 4 98.7 0.33 0.11 <0.01 Comparative Example 1 95.3 2.5 0.11 0.03 Comparative Example 2 98.8 0.8 0.11 0.02

[0091] The vanadium precipitation rates of the vanadium precipitation methods in Examples 1 to 4 and Comparative Examples 1 to 2 were also measured, and the results are summarized in Table 2 below:

[0092] Table 2 Effects of vanadium precipitation in different tests

[0093] Vanadium precipitation rate (%) Example 1 99.2 Example 2 99.1 Example 3 99.2 Example 4 99.1 Comparative Example 1 96.2 Comparative Example 2 99.0

[0094] Through the above experiments, it can be seen that Examples 1 to 4 achieve non-ammonium vanadium precipitation treatment, and the purity of vanadium pentoxide in the product is equivalent to or significantly higher than that of the product in Comparative Examples 1 to 2, and the vanadium precipitation rate of Examples 1 to 4 is also significantly higher than that of Comparative Examples 1 to 2. In addition, in Comparative Example 1, an equal amount of melamine is used for treatment, and it is obvious that its product is difficult to meet the quality requirements, and the vanadium precipitation rate is also significantly low; while the product in Comparative Example 2 basically meets the quality requirements, but due to the use of ammonium salt treatment, the ammonium ion concentration in the wastewater is too high, resulting in difficulty and high cost in subsequent wastewater treatment.

[0095] In summary, the vanadium precipitation method of sodium vanadium liquid proposed in the present invention not only has a more convenient process flow, but also can achieve ammonium-free vanadium precipitation. Its vanadium precipitation effect is the same as or significantly better than the existing vanadium precipitation process. This means that the present invention can solve the problem in the prior art that it is difficult to achieve more convenient and environmentally friendly industrial vanadium precipitation while maintaining a high-efficiency vanadium precipitation effect.

[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for precipitating vanadium from sodium vanadium solution, It is characterized in that The steps include: S1 takes sodium vanadium solution, removes impurities, filters, and takes the filtrate for later use; S2 takes the filtrate, adds a composite vanadium precipitant, adjusts the pH value of the filtrate to 2.2-2.5, heats to 85-95°C for reaction, and filters to obtain a vanadium precipitate; The composite vanadium precipitation agent comprises at least one of the following formula a and formula b:

2. The vanadium precipitation method of sodium vanadium solution according to claim 1, It is characterized in that In step S1, the impurity removal method is: adding an impurity remover to the sodium vanadium solution, stirring the reaction, filtering, removing impurity precipitation, and obtaining the filtrate; Calculated by mass fraction, the impurity remover includes 10-20wt% of polyaluminium chloride, 50-70wt% of aluminium sulfate and 20-30wt% of magnesium stearate.

3. The vanadium precipitation method of sodium vanadium solution according to claim 2, It is characterized in that The sodium vanadium solution has a vanadium content of 5-50 g / L, a sodium content of 10-100 g / L, a chromium content of 1-30 g / L, a silicon content of 0.2-2 g / L, and a phosphorus content of ≤0.05 g / L; The amount of the impurity remover added is 2-3 times the silicon content in the sodium vanadium solution by mass.

4. The vanadium precipitation method of sodium vanadium solution according to claim 2, It is characterized in that Before adding the impurity remover, adjust the pH value of the sodium vanadium solution to 4-5.

5. The vanadium precipitation method of sodium vanadium solution according to claim 1, It is characterized in that The vanadium precipitate obtained in step S2 is dried, calcined at 500-550° C. for 2-4 hours, and cooled to obtain vanadium pentoxide.

6. The method for precipitating vanadium from sodium vanadium solution according to any one of claims 1 to 5, It is characterized in that In step S2, the preparation method of the composite vanadium precipitation agent comprises the following steps: Melamine, ethylenediamine and glutaraldehyde aqueous solution are mixed and heated to 50-60° C. for reaction; the reaction product is then mixed and stirred with vanadium-containing seed crystals to obtain the composite vanadium precipitation agent.

7. The method for precipitating vanadium from sodium vanadium solution according to claim 6, It is characterized in that According to the molar mass, the dosage ratio of melamine, ethylenediamine and glutaraldehyde aqueous solution is 8-10: 2.5-3.5:1, and the mass concentration of the glutaraldehyde aqueous solution is 2-5wt%.

8. The method for precipitating vanadium from sodium vanadium solution according to claim 6, It is characterized in that The vanadium-containing seed crystals are selected from one or more of vanadium pentoxide and ammonium polyvanadate.

9. The method for precipitating vanadium from sodium vanadium solution according to claim 8, It is characterized in that The ratio of melamine to vanadium-containing seed crystals is 0.04-0.15:1 by mass.

10. The method for precipitating vanadium from sodium vanadium solution according to claim 6, It is characterized in that The usage ratio of the composite vanadium precipitator to the vanadium content in the filtrate is 0.1-0.2:1 by mass.

Citation Information

Patent Citations

  • Method for extracting vanadium from acidic high-phosphorus vanadium liquid

    CN112239806A

  • Method for preparing high-purity vanadium pentoxide through sodium salt vanadium precipitation of sodium vanadate solution

    CN113800562A