Method for improving undercut phenomenon at bottom of crystal ball
Through innovative methods of dry etching and mask plate design, the problem of bottom cutting in wafer packaging is solved, the stability and reliability of the packaging are improved, and the isotropic etching problems caused by wet etching are avoided.
Patent Information
- Application Number
- CN202411133489.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
In wafer packaging technology, the undercut phenomenon at the bottom of the crystal sphere leads to instability and reliability problems in the packaging process, and the bumps are mainly suspended due to isotropic etching caused by H2O2 wet etching.
Using dry etching, plasma etching replaces H2O2 wet etching, and in the mask plate design, the bump pattern size of the mask plate is expanded to bump size + undercut width, combining wet etching and secondary Au layer etching , eliminate the undercut phenomenon.
The undercut phenomenon is eliminated through dry etching, which improves the mechanical strength of the package and the reliability of the electrical connection, avoids unnecessary etching caused by isotropic etching, and achieves a more stable crystal ball packaging.
Smart Images

Figure CN119028833A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wafer packaging, and in particular relates to a method for improving the undercut phenomenon at the bottom of a crystal ball. Background Art
[0002] In the field of wafer packaging technology, undercutting at the bottom of the crystal ball is a common problem, which will lead to instability of the crystal ball and affect the quality and reliability of the entire packaging process. Undercutting usually occurs in the manufacturing process of the bump. When the size of the UBM (Under Bump Metallurgy) layer is smaller than the size of the bump, undercutting will occur, making the bump suspended, which will reduce the mechanical strength of the package and the reliability of the electrical connection.
[0003] In the existing process technology, undercutting is mainly caused by wet etching (Wet Etch) using H2O2 (hydrogen peroxide) at the TiW (titanium tungsten) etching station. Wet etching is a chemical reaction process that has no selectivity for the etching direction, so it usually manifests as isotropic etching (Isotropic Etching). This isotropic etching not only etches on the top of the bump, but also etches on the sidewalls of the bump, resulting in undercutting. . Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention proposes an improved mask design scheme and adopts a dry etching method to improve the undercut phenomenon at the bottom of the crystal ball.
[0005] In order to achieve the above object, the following technical solution is adopted: The present invention provides a method for improving the undercut phenomenon at the bottom of the crystal ball, comprising the following steps:
[0006] providing a substrate;
[0007] sputtering a TiW / Au layer on the substrate;
[0008] coating a photoresist on the TiW / Au layer;
[0009] To develop,
[0010] The substrate is exposed, and during the exposure, the size of the bump pattern on the mask is consistent with the size of the bump or is enlarged to the size of the bump + the undercut width;
[0011] Curing the photoresist by hardening baking;
[0012] performing plasma treatment on the photoresist;
[0013] An Au layer is plated in the opening area of the photoresist pattern by electroplating to form an Au bump;
[0014] The Au layer is removed by etching;
[0015] The TiW layer is etched to remove the TiW layer to eliminate the undercut phenomenon;
[0016] Performing annealing treatment;
[0017] Carry out final quality inspection on the product and obtain the packaged product.
[0018] Furthermore, when the size of the mask is consistent with the size of the bump pattern during exposure, the specific method for etching the TiW / Au layer is as follows:
[0019] Plasma etching is performed. Further, when the size of the mask is expanded to the size of the bump pattern + the undercut width, the specific method for etching the TiW / Au layer is:
[0020] The TiW layer is wet etched, and the Au layer is etched a second time.
[0021] The beneficial effects of the present invention are:
[0022] (1) The present invention adopts plasma etching, a dry etching method, to replace H2O2 wet chemical etching. Since the ions in dry etching physically collide with the target and have no selectivity, it is anisotropic etching, so no undercut phenomenon occurs.
[0023] (2) When designing the mask, the present invention enlarges the size of the bump pattern of the mask to the bump size + the undercut width, and according to the principle that wet etching is isotropic etching, an Au layer etching process is added after the TiW layer etching. By controlling the etching amount, the size of the bump is etched to be consistent with the size of the TiW layer, which is equivalent to no undercut, thereby eliminating the undercut phenomenon. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the process of sputtering TiW / Au layer on a substrate;
[0025] Figure 2 Schematic diagram of the process of coating photoresist on the TiW / Au layer;
[0026] Figure 3 is a schematic diagram of the development process;
[0027] Figure 4 Schematic diagram of the process of exposure, hardening baking and plasma treatment;
[0028] Figure 5 Schematic diagram of the process of electroplating Au bumps;
[0029] Figure 6A schematic diagram of the process of photoresist stripping;
[0030] Figure 7 Schematic diagram of the process of etching and removing the Au layer;
[0031] Figure 8 A schematic diagram of the process of removing the TiW layer, annealing, and performing final quality inspection to obtain a packaged product in Example 1 and Example 2;
[0032] Fig. 9 This is a schematic diagram of plasma etching in Example 1;
[0033] Fig.10 A schematic diagram of the dimensions of the mask and the bump pattern in Example 2;
[0034] Fig.11 This is a schematic diagram of the structure of the packaged product obtained in Comparative Example 1.
[0035] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.
[0036] Legend: 1. Al pad; 2. passivation layer; 3. PI layer; 4. TiW layer; 5. Au layer; 6. photoresist; 7. mask; 8. Au bump; 9. processing chamber; 10. microwave plasma source; 11. nozzle; 12. electrons; 13. ions; 14. free radicals; 15. undercut; 16. bump pattern. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0038] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0039] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0040] Example 1
[0041] Method for improving undercutting phenomenon at the bottom of crystal ball
[0042] The steps include:
[0043] providing a substrate;
[0044] like Figure 1 As shown, a TiW / Au layer is sputtered on the substrate;
[0045] like Figure 2 As shown, a photoresist is coated on the TiW / Au layer;
[0046] like Figure 3 As shown, development is performed.
[0047] like Figure 4 As shown, the substrate is exposed, and the size of the bump pattern is consistent with the size of the bump;
[0048] Curing the photoresist by hardening baking;
[0049] performing plasma treatment on the photoresist;
[0050] like Figure 5 As shown, an Au layer is plated in the opening area of the photoresist pattern by electroplating to form an Au bump;
[0051] like Figure 6 As shown, photoresist stripping is performed;
[0052] like Figure 7 As shown, the Au layer is removed by etching;
[0053] like Figure 8 As shown, the TiW layer is etched to remove the TiW layer to eliminate the undercut phenomenon, and the specific method is plasma etching;
[0054] Performing annealing treatment;
[0055] Carry out final quality inspection on the product to obtain the packaged product, such as Figure 8 as shown in .
[0056] The schematic diagram of plasma etching is as follows: Fig. 9 shown.
[0057] Example 2
[0058] Method for improving undercutting phenomenon at the bottom of crystal ball
[0059] The steps include:
[0060] providing a substrate;
[0061] like Figure 1 As shown, a TiW / Au layer is sputtered on the substrate;
[0062] like Figure 2 As shown, a photoresist is coated on the TiW / Au layer;
[0063] like Figure 3 As shown, development is performed.
[0064] like Figure 4 As shown, the substrate is exposed, and the size of the bump pattern is enlarged to the bump size + the undercut width;
[0065] Curing the photoresist by hardening baking;
[0066] performing plasma treatment on the photoresist;
[0067] like Figure 5 As shown, an Au layer is plated in the opening area of the photoresist pattern by electroplating to form an Au bump;
[0068] like Figure 6 As shown, photoresist stripping is performed;
[0069] like Figure 7 As shown, the Au layer is removed by etching;
[0070] like Figure 8 As shown, the TiW layer is etched to remove the TiW layer to eliminate the undercut phenomenon, specifically: the TiW layer is wet-etched, and then the Au layer is etched twice;
[0071] Performing annealing treatment;
[0072] Carry out final quality inspection on the product to obtain the packaged product, such as Figure 8 as shown in .
[0073] The size of the mask and the bump pattern during exposure is as follows: Fig.10 As shown, the size of the bump pattern of the mask is enlarged to the bump size + the undercut width.
[0074] Comparative Example 1
[0075] Conventional Bumping Process
[0076] The steps include:
[0077] providing a substrate;
[0078] like Figure 1 As shown, a TiW / Au layer is sputtered on the substrate;
[0079] like Figure 2 As shown, a photoresist is coated on the TiW / Au layer;
[0080] like Figure 3As shown, development is performed.
[0081] like Figure 4 As shown, the substrate is exposed, and during the exposure, the size of the mask is expanded to the size of the bump pattern + the undercut width;
[0082] Curing the photoresist by hardening baking;
[0083] performing plasma treatment on the photoresist;
[0084] like Figure 5 As shown, an Au layer is plated in the opening area of the photoresist pattern by electroplating to form an Au bump;
[0085] like Figure 6 As shown, photoresist stripping is performed;
[0086] like Figure 7 As shown, the Au layer is removed by etching;
[0087] The TiW layer is etched to remove the TiW layer, specifically: using H2O2 wet chemical etching;
[0088] Performing annealing treatment;
[0089] Carry out final quality inspection on the product to obtain the packaged product. The product structure is as follows Fig.11 As shown, there is undercut in the packaged product.
[0090] Results Analysis
[0091] By comparing Example 1 with Comparative Example 1, it can be seen that by using plasma etching, a dry etching method, to replace H2O2 wet chemical etching, since the ions in dry etching physically collide with the target and have no selectivity, it is anisotropic etching, so no undercutting phenomenon occurs.
[0092] By comparing Example 1 and Comparative Example 1, it can be seen that when designing the mask, the size of the bump pattern of the mask is enlarged to the bump size + the undercut width, and according to the principle that wet etching is isotropic etching, an Au layer etching process is added after the TiW layer etching. By controlling the etching amount, the size of the bump is etched to be consistent with the size of the TiW layer, which is equivalent to no undercut, thereby eliminating the undercut phenomenon.
[0093] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0094] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. Methods to improve the undercut phenomenon at the bottom of the crystal ball, Features: The steps include: providing a substrate; sputtering a TiW / Au layer on the substrate; coating a photoresist on the TiW / Au layer; To develop, The substrate is exposed, and during the exposure, the size of the bump pattern on the mask is consistent with the size of the bump or is enlarged to the size of the bump + the undercut width; Curing the photoresist by hardening baking; performing plasma treatment on the photoresist; An Au layer is plated in the opening area of the photoresist pattern by electroplating to form an Au bump; The Au layer is removed by etching; The TiW layer is etched to remove the TiW layer to eliminate the undercut phenomenon; Performing annealing treatment; Carry out final quality inspection on the product and obtain the packaged product.
2. The method for improving the undercut phenomenon at the bottom of the crystal ball according to claim 1, Features: When the size of the mask is consistent with the size of the bump pattern during exposure, the specific method for etching the TiW layer is as follows: Plasma etching is performed.
3. The method for improving the undercut phenomenon at the bottom of the crystal ball according to claim 2, Features: The wet etching comprises the following steps: When the size of the mask is expanded to the size of the bump pattern + the undercut width, the specific method of etching the TiW layer is: The TiW layer is wet etched, and the Au layer is etched a second time.