High-amorphization halide solid electrolyte material, preparation method thereof and all-solid-state battery

By using OCN- instead of Cl- in the Li2+xZrCl6-xOx system, the ionic conductivity and rate performance of solid electrolytes are improved, and the problem of insufficient conductivity of the existing Li2+xZrCl6-xOx system is solved, the material cost is reduced, and the material cost is promoted. Industrial application of all solid state batteries.

CN119029286APending Publication Date: 2024-11-26CHINA AUTOMOTIVE INNOVATION CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411386495.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The ionic conductivity of the Li2+xZrCl6-xOx system solid electrolyte is not high, and it cannot meet the rate performance requirements of all-solid state batteries. The raw material cost is high, which limits the industrial application of all-solid state batteries.

Method used

The solid electrolyte material of the Li2+yZrCl6-x-y(OCN)xOy system has an ion radius close to Cl-, which improves the room temperature ion conductivity and reduces the Young's mode through amorphization treatment. The contact area between the electrode and the electrolyte is increased.

Benefits of technology

It significantly improves the ionic conductivity and rate performance of solid electrolytes, while reducing the cost of materials, and promoting the industrial application process of all-solid state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029286A_ABST
    Figure CN119029286A_ABST
Patent Text Reader

Abstract

The invention discloses a high-amorphization halide solid electrolyte material, a preparation method thereof and an all-solid-state battery. The high-amorphization halide solid electrolyte material is represented by the following chemical formula: Li < 2 + y > ZrCl6-x-y (OCN) xOy, wherein x and y meet the following relational expression: 0 lt; x is greater than or equal to 0 and less than or equal to 6, y is greater than or equal to 0 and less than or equal to 2, and x + y is less than or equal to 6, and OCN <-> with an ion radius close to and larger than that of Cl <-> is adopted to replace a part of Cl <->, so that the effective ion potential ratio of the solid electrolyte material is increased, the interaction of anions to carriers is weakened, the diffusion potential barrier of Li < + > is reduced, and the ionic conductivity is improved, the highest room-temperature ionic conductivity of the high-amorphization halide solid electrolyte material reaches 5.09 mS / cm, and compared with the melting point (886K) of LiCl and the melting point (648K) of LiOCN, the high-amorphization halide solid electrolyte material is lower in melting point and lattice energy, so that the material keeps lower Young modulus, and the lowest Young modulus of the high-amorphization halide solid electrolyte material reaches 11.09 Gpa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of all-solid-state batteries, and in particular to a highly amorphous halide solid electrolyte material and a preparation method thereof, and an all-solid-state battery. Background Art

[0002] Li 2+x ZrCl 6-x O x The ionic conductivity of the solid electrolyte of the system is an important research direction at present. In addition to the relatively high price of Li element, the only other metal element in this solid electrolyte material is Zr element, and the abundance of Zr in the earth's crust is much greater than that of In, Sc, Y, Tb, Lu and other elements that make up other chloride solid electrolytes. The price of ZrCl4 as a raw material is several orders of magnitude lower than that of other chloride solid electrolyte raw materials. The low cost of raw materials eliminates the important obstacles to the industrial application of inorganic chloride solid electrolytes and further promotes the industrial application process of all-solid-state batteries. In the prior art, Li 2+x ZrCl 6-x O x The ionic conductivity of the solid electrolyte of the system is not high, which cannot meet the rate performance requirements of the all-solid-state battery with its solid electrolyte material. 2+x ZrCl 6-x O x There is still room for improvement in the ionic conductivity of the system's solid electrolyte. Summary of the invention

[0003] In view of the above problems, the present invention aims to provide a method for - Replace part of Cl - , and OCN - The ionic radius of Cl - The ionic radius of Li 2+x ZrCl 6-x O x The room temperature ionic conductivity of the system solid electrolyte also maintains a highly amorphous halide solid electrolyte material with a lower Young's modulus, a preparation method thereof, and an all-solid-state battery.

[0004] In order to solve the above technical problems, the present invention provides a highly amorphous halide solid electrolyte material and a preparation method thereof and an all-solid-state battery. The technical solution is as follows:

[0005] In one aspect, a highly amorphous halide solid electrolyte material is provided, wherein the highly amorphous halide solid electrolyte material is represented by the following chemical formula:

[0006] Li 2+y ZrCl 6-x-y (OCN) xO y ;

[0007] Wherein, x and y satisfy the following relational expressions:

[0008] 0 < x ≤ 6, 0 ≤ y ≤ 2, and x + y ≤ 6.

[0009] In an exemplary embodiment, the highly amorphous halide solid electrolyte material is an amorphous compound.

[0010] On the one hand, the present invention also provides a method for preparing the above-mentioned solid electrolyte material, and the method includes:

[0011] Providing a lithium raw material and a zirconium raw material, wherein the lithium raw material includes at least one of Li2O, Li2O2, LiOCN, and LiCl, the zirconium raw material includes at least one of ZrCl4, ZrOCl2, and Zr(OCN)4, and at least one of the lithium raw material and the zirconium raw material contains cyanate;

[0012] Performing an amorphization reaction on the lithium raw material and the zirconium raw material to obtain the highly amorphous halide solid electrolyte material.

[0013] In an exemplary embodiment, the performing an amorphization reaction on the lithium raw material and the zirconium raw material to obtain the highly amorphous halide solid electrolyte material includes:

[0014] Placing the lithium raw material and the zirconium raw material in a ball milling container and performing ball milling through ball milling balls to obtain a first amorphization reaction product; the first amorphization reaction product includes the highly amorphous halide solid electrolyte material and the ball milling balls;

[0015] Based on the obtained first amorphization reaction product, using a sieve to remove the ball milling balls to obtain the highly amorphous halide solid electrolyte material.

[0016] In an exemplary embodiment, the mass ratio of the total mass of the lithium raw material and the zirconium raw material to the mass of the ball milling balls is 1:(1 - 50).

[0017] In an exemplary embodiment, the ball milling time is 2 - 60 h.

[0018] In an exemplary embodiment, the ball milling speed is 200 - 600 rpm.

[0019] In an exemplary embodiment, the performing an amorphization reaction on the lithium raw material and the zirconium raw material to obtain the highly amorphous halide solid electrolyte material includes:

[0020] Place the lithium raw material and the zirconium raw material in a dispersion medium for an amorphization reaction to obtain a second amorphization reaction product; the amorphization reaction product includes the highly amorphous halide solid electrolyte material and the dispersion medium;

[0021] The dispersion medium includes one or more of saturated alkane solvents or benzene solvents;

[0022] Based on the obtained second amorphization reaction product, use a vacuum filtration device to remove the dispersion medium to obtain the highly amorphous halide solid electrolyte material.

[0023] In an exemplary embodiment, the mass ratio of the total mass of the lithium raw material and the zirconium raw material to the mass of the dispersion medium is 1:(0 to 50).

[0024] On the other hand, a all-solid-state battery is provided, including any one of the above highly amorphous halide solid electrolyte materials.

[0025] The present invention discloses a highly amorphous halide solid electrolyte material, which is represented by the following chemical formula: Li 2+y ZrCl 6-x-y (OCN) x O y ; wherein, x and y satisfy the following relationship: 0 < x ≤ 6, 0 ≤ y ≤ 2, and x + y ≤ 6. By using OCN - with an ionic radius close to and larger than that of Cl - to replace part of Cl - , the effective ion potential ratio of the solid electrolyte is increased, thereby weakening the interaction between anions and carriers, reducing the Li + diffusion barrier, improving the ionic conductivity. At the same time, compared with the melting point of LiCl (886K), the melting point of LiOCN (648K) is lower and the lattice energy is lower, so that the material maintains a lower Young's modulus. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the present invention, the following will briefly introduce the drawings required for the description of the embodiments or the prior art. Obviously, the following drawings are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative efforts.

[0027] Figure 1 is the Lewis structure diagram of OCN - provided by the embodiment of the present invention;

[0028] Figure 2 is different Cl provided by the embodiment of the present invention- / OCN - Proportion of Li 2+y ZrCl 6-x-y (OCN) x O y Electrolyte conductivity trend chart;

[0029] Figure 3 It is a flowchart of a preparation method of a highly amorphous halide solid electrolyte material provided by an embodiment of the present invention;

[0030] Figure 4 It is a schematic diagram of the structure of a all-solid-state battery provided by an embodiment of the present invention;

[0031] Figure 5 It is an XRD diffraction pattern of Li2Zr(OCN)6 solid electrolyte provided by an embodiment of the present invention;

[0032] Figure 6 It is Li provided by an embodiment of the present invention 2.5 ZrCl2(OCN) 3.5 O 0.5 XRD diffraction pattern of solid electrolyte;

[0033] Figure 7 It is an XRD diffraction pattern of Li2ZrCl6 solid electrolyte provided by an embodiment of the present invention. Specific embodiments

[0034] Next, the technical solutions in the embodiments of the present invention will be clearly and completely described in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.

[0035] The embodiments of the present application provide a highly amorphous halide solid electrolyte material,

[0036] The highly amorphous halide solid electrolyte material is represented by the following chemical formula:

[0037] Li 2+y ZrCl 6-x-y (OCN) x O y ;

[0038] Among them, x and y satisfy the following relationship:

[0039] 0 < x ≤ 6, 0 ≤ y ≤ 2, and x + y ≤ 6.

[0040] Among them, OCN -is a linear anion, see Figure 1 , OCN - The carbon atoms and nitrogen atoms in the structure form a carbon-nitrogen triple bond. The structural characteristics of the carbon-nitrogen triple bond determine OCN - The atoms are on the same line, OCN - and Cl - Similar in structure; on the one hand, OCN - The ionic radius (197 pm) and Cl - The radius (181pm) is close to and larger, and the surface charge distribution density is low. - Replace part of Cl - This increases the effective ion potential ratio of the solid electrolyte, thereby weakening the interaction between anions and carriers, reducing the Li+ diffusion barrier, and thus improving the ionic conductivity.

[0041] On the other hand, increasing the amount of O in the solid electrolyte 2- Content allows connection [MXO] - Unit and adjacent [MXO] - The polarizability of the bridging oxygen of the unit increases, and the charge is further delocalized, where M represents the central cation and X represents the halogen. Therefore, the highly amorphous halide solid electrolyte material is formed by a linear structure OCN. - The incorporation of relatively improves the ionic conductivity of the solid electrolyte.

[0042] At the same time, compared with the melting point of LiCl (886K), the melting point of LiOCN (648K) is lower and the lattice energy is lower, which enables the material to maintain a lower Young's modulus, helping to increase the contact area between the electrode and the electrolyte, thereby improving the battery's rate performance.

[0043] Specifically, 6-yz, y and z can be decimals or integers, which are used to represent the molar ratio of ions in the highly amorphous halide solid electrolyte material components. The molar ratios of ions in highly amorphous halide solid electrolyte materials of different components are different, and have different room temperature conductivities. For example, please refer to Figure 2 , Figure 2 For different Cl - / OCN - Proportional Li 2+y ZrCl 6-x-y (OCN) x O y The trend of electrolyte conductivity shows that within a certain range, as OCN - To Cl - The room temperature ionic conductivity of the highly amorphous halide solid electrolyte material changes positively with the increase of the substitution amount of Li 2.5ZrCl2(OCN) 3.5 O 0.5 The room temperature ionic conductivity is the highest.

[0044] In the embodiment of the present application, the highly amorphous halide solid electrolyte material is an amorphous compound.

[0045] Specifically, the solid form of highly amorphous halide solid electrolyte materials is amorphous, which is the key to improving the ionic conductivity of the highly amorphous halide solid electrolyte materials. Amorphous means disorder, a longer distance between carriers and anion skeletons, isotropy, no periodic potential barriers, low lattice energy and high compaction density.

[0046] The present application also provides a method for preparing a highly amorphous halide solid electrolyte material. For a preparation flow chart of the highly amorphous halide solid electrolyte material, please refer to Figure 3 , the method comprises the following steps:

[0047] Step S1: providing a lithium raw material and a zirconium raw material, wherein the lithium raw material includes at least one of Li2O, Li2O2, LiOCN, and LiCl, and the zirconium raw material includes at least one of ZrCl4, ZrOCl2, and Zr(OCN)4, and at least one of the lithium raw material and the zirconium raw material contains cyanate.

[0048] Among them, the lithium raw material and zirconium raw material used in the preparation method are low in cost, which is conducive to the large-scale production of materials.

[0049] Step S2: subjecting the lithium raw material and the zirconium raw material to an amorphization reaction to obtain the highly amorphous halide solid electrolyte material.

[0050] Specifically, the amorphization reaction is a process of transforming the solid crystalline phase into an amorphous phase through the interface movement of the raw materials during the solid-state reaction.

[0051] In the embodiment of the present application, the lithium raw material and the zirconium raw material are subjected to an amorphization reaction to obtain a highly amorphous halide solid electrolyte material comprising:

[0052] Placing a lithium raw material and a zirconium raw material in a ball milling container and ball milling them with ball milling balls to obtain a first amorphization reaction product; the first amorphization reaction product includes a highly amorphized halide solid electrolyte material and ball milling balls;

[0053] Based on the obtained first amorphization reaction product, the ball milling balls are removed using a screen to obtain a highly amorphous halide solid electrolyte material.

[0054] The ball milling method is an effective amorphization reaction method and also a mechanochemical synthesis method, which breaks the order of the crystal structure through mechanical force to form an amorphous substance. The material of the ball milling container includes a stainless steel ball milling jar, an agate ball milling jar or a zirconia ball milling jar, etc., which can be selected according to the experimental requirements in the specific implementation.

[0055] In the embodiment of the present application, the ratio of the total mass of the lithium raw material and the zirconium raw material to the mass of the ball milling balls is 1:(1-50).

[0056] Specifically, the grinding efficiency can be improved by changing the mass ratio of the total mass of the lithium raw material and the zirconium raw material to the mass ratio of the ball milling balls, wherein preferably, the ratio is 1:10.

[0057] In the embodiments of the present application, the ball milling time is 2 to 60 hours.

[0058] Specifically, the ball milling efficiency can be improved and the grain size and grain boundary structure of the material can be affected by changing the ball milling time; preferably, the ball milling time is 30 hours.

[0059] In the embodiment of the present application, the rotation speed of the ball mill is 200 to 600 rpm.

[0060] Specifically, the ball milling efficiency can be improved and the grain size and grain boundary structure of the material can be affected by changing the ball milling speed; preferably, the ball milling speed is 400 rpm.

[0061] In the embodiment of the present application, the lithium raw material and the zirconium raw material are subjected to an amorphization reaction to obtain a highly amorphous halide solid electrolyte material comprising:

[0062] Placing a lithium raw material and a zirconium raw material in a dispersion medium for an amorphization reaction to obtain a second amorphization reaction product; the amorphization reaction product includes a highly amorphized halide solid electrolyte material and a dispersion medium;

[0063] The dispersion medium includes: one or more of saturated alkane solvents or benzene solvents;

[0064] Based on the obtained second amorphization reaction product, the dispersion medium is removed using a reduced pressure filtration device to obtain a highly amorphous halide solid electrolyte material.

[0065] Specifically, the saturated alkane solvent may be n-hexane, n-heptane, or other saturated alkane liquids; the benzene solvent may be benzene, toluene, or ethylbenzene, which may be selected according to needs.

[0066] Specifically, by using a vacuum filtration device to perform a vacuum filtration operation, i.e., suction filtration, a vacuum pump is used to reduce the pressure in the suction filtration bottle, which can speed up the filtration rate and shorten the filtration time. Vacuum filtration can separate the highly amorphous halide solid electrolyte material from the dispersion medium as much as possible, ensuring the safety of the separation process, and can make the obtained highly amorphous halide solid electrolyte material easier to dry, which is convenient for subsequent processing and use.

[0067] In the examples of the present application, the mass ratio of the total mass of the lithium raw material and the zirconium raw material to the mass of the dispersion medium is 1:(0-50).

[0068] Specifically, by adding a dispersion medium, the flocculation and agglomeration of the particles can be effectively prevented, so that the particles are evenly dispersed, thereby achieving a stable dispersion effect, wherein the preferred ratio is 1:1.

[0069] In an embodiment of the present application, an all-solid-state battery is provided, comprising any one of the highly amorphous halide solid electrolyte materials disclosed in the embodiment of the present application. Figure 4 is a schematic diagram of the all-solid-state battery structure disclosed in the embodiment of this application, such as Figure 4 As shown, the all-solid-state battery includes a positive electrode, a negative electrode, a negative electrode side electrolyte and a positive electrode side electrolyte.

[0070] Among them, at least one of the positive electrode, the negative electrode, the positive electrode side electrolyte and the positive electrode side electrolyte contains any one of the highly amorphous halide solid electrolyte materials disclosed in the embodiments of the present application. Preferably, the positive electrode or the positive electrode side electrolyte is selected from any one of the highly amorphous halide solid electrolyte materials disclosed in the embodiments of the present application.

[0071] The positive electrode active material in the positive electrode may include: rock salt layer type active materials, such as LiCoO2, LiMnO2, LiNiO2, LiVO2 or Li 1+x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O2; spinel active materials, such as LiMn2O4 or Li(Ni 0.5 Mn 1.5 )O4; inverse spinel type active materials, such as LiNiVO4 or LiCoVO4; olivine type active materials, such as LiFePO4, LiMnPO4, LiCoPO4 or LiNiPO4; silicon-containing active materials, such as Li2FeSiO4 or Li2MnSiO; rock salt layer type active materials in which a portion of transition metals are replaced by heterogeneous metals, such as LiNi 0.8 Co (0.2-x) Al x O2 (0<x<0.2); spinel-type active materials in which a portion of transition metals are replaced by heterogeneous metals, such as Li 1+x Mn 2-x-y My O4 (wherein M includes at least one of Al, Mg, Co, Fe, Ni, and Zn, and 0<x+y<2); and lithium titanate, such as Li4Ti5O 12 ; and the sulfide positive electrode active material may include: copper sulfide, iron sulfide, cobalt sulfide, nickel sulfide, etc.

[0072] Among them, the negative electrode active material on the negative electrode may include: metal materials, carbon materials, oxides, nitrides, tin compounds or silicon compounds. The metal material may be a simple metal material, or may be an alloy. Examples of metal materials are lithium metal or lithium alloys. Examples of carbon materials are natural graphite, coke, graphitizable carbon, carbon fiber, spherical carbon, artificial graphite or amorphous carbon. From the viewpoint of capacity density, suitable examples of negative electrode active materials are silicon, tin, silicon compounds or tin compounds.

[0073] Specifically, except Li 2+y ZrCl 6-x-y (OCN) x O y In addition to the electrolyte material, the positive electrode, the negative electrode, the positive electrode side electrolyte and the solid electrolyte in the positive electrode side electrolyte may include Li3YCl6, Li3InCl6, Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers, and Z is one of Ge, Zn and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, and In), Li 10 GeP2S 12 wait.

[0074] The present invention has no special requirements for the preparation of the battery, and the conventional preparation method of the all-solid-state lithium battery in the art can be adopted. The specific preparation process is well known in the field of solid-state batteries and will not be described in detail here.

[0075] The present invention will be described in detail below through examples.

[0076] In some of the following embodiments and some of the comparative examples, the XRD test conditions are as follows: in an argon atmosphere, an X-ray diffraction device is used, Cu-Kα rays are used as the X-ray source, the obtained solid electrolyte material is pressed into tablets, and the X-ray diffraction patterns of the solid electrolyte materials of some embodiments are measured at a temperature of 25°C.

[0077] Conductivity test: In an argon atmosphere, the powders of the solid electrolyte materials of the following embodiments and comparative examples are filled inside a pressurized mold. Inside the pressurized mold, upper and lower punches are used to apply a pressure of 500 MPa to the powder of the solid electrolyte material. While keeping the pressure unchanged, the upper and lower parts of the punches are respectively connected to a potentiostat equipped with a frequency response analyzer, and the ionic conductivity of the solid electrolyte material is measured by the electrochemical impedance method. The real value of the impedance at the measuring point where the absolute value of the phase of the complex impedance is the smallest is regarded as the resistance value of the solid electrolyte material to ionic conduction.

[0078] All-solid-state battery test: Li and Mg were mixed in an agate mortar in an argon atmosphere at a mass ratio of 30:70. 2+y ZrCl 6-x-y (OCN) x O y Solid electrolyte material and positive electrode active material, namely LiCoO2. These materials are mixed to obtain a positive electrode mixture. Li 2+y ZrCl 6-x-y (OCN) x O y (60 mg) and Li6PS5Cl solid electrolyte material (24 mg) were added to obtain a laminate. A pressure of 160 MPa was applied to the laminate to form a solid electrolyte layer. 2+y ZrCl 6-x-y (OCN) x O y A positive electrode mixture (5 mg) is stacked on the solid electrolyte layer to obtain a stack. A pressure of 360 MPa is applied to the stack to form a positive electrode. Next, a metal Li foil (300 μm thick) is stacked on the solid electrolyte layer formed by Li6PS5Cl to obtain a stack. A pressure of 5 MPa is applied to the stack to form a negative electrode. A current collector formed by stainless steel is arranged on the positive electrode and the negative electrode, and a current collecting lead is installed on the current collector. Finally, an insulating hoop is used to isolate the inside of the insulating cylinder from the external atmosphere, and the inside of the cylinder is sealed to obtain an all-solid-state battery, such as Figure 4 The battery was tested for 0.1-1C electrochemical performance in the voltage range of 2.5-4.2V.

[0079] Young's modulus test: Use ultrasonic late echo technology to measure the elastic modulus of the sample, using a 5MHz frequency transducer. For an isotropic solid medium, its longitudinal wave velocity CL and transverse wave velocity CS are determined by the density, elastic modulus and Poisson's ratio of the medium. By accurately measuring the longitudinal and transverse wave velocities of the medium, the elastic modulus of the medium can be calculated.

[0080] Example 1

[0081] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0082] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1, with masses of 9.792 g and 25.929 g, respectively. The raw materials and 357 g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and milled at 400 rpm for 30 h to obtain an amorphous product Li2Zr(OCN)6, whose XRD spectrum is shown in FIG. Figure 5 As shown; its ionic conductivity is 4.56mS / cm, its Young's modulus is 13.30Gpa, and its all-solid-state battery rate performance is 84.71(1C / 0.1C)%.

[0083] Example 2

[0084] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0085] LiCl: LiOCN: Li2O: ZrCl4 were added in a molar ratio of 1:0.5:0.5:1, with masses of 4.239 g, 2.448 g, 1.494 g, and 23.304 g, respectively; the raw materials and 315 g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400 rpm for 30 h to obtain an amorphous product Li 2.5 ZrCl5(OCN) 0.5 O 0.5 Its ionic conductivity is 2.87mS / cm, its Young's modulus is 17.38Gpa, and its all-solid-state battery rate performance is 86.34(1C / 0.1C)%.

[0086] Example 3

[0087] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0088] LiOCN: Li2O: ZrCl4 were added in a molar ratio of 1.5:0.5:1, with masses of 7.344 g, 1.494 g, and 23.304 g, respectively; the raw materials and 321 g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400 rpm for 30 h to obtain an amorphous product Li2.5 ZrCl4(OCN) 1.5 O 0.5 Its ionic conductivity is 2.87mS / cm, its Young's modulus is 17.38Gpa, and its all-solid-state battery rate performance is 86.34(1C / 0.1C)%.

[0089] Example 4

[0090] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0091] LiOCN: LiCl: Li2O: ZrCl4: Zr(OCN)4 were added in a molar ratio of 0.5:1:0.5:0.5:0.5, with masses of 2.448g, 4.239g, 1.494g, 11.652g, and 12.646g, respectively; the raw materials and 325g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400rpm for 30h to obtain an amorphous product Li 2.5 ZrCl3(OCN) 2.5 O 0.5 Its ionic conductivity is 4.08mS / cm, its Young's modulus is 16.28Gpa, and its all-solid-state battery rate performance is 73.82(1C / 0.1C)%.

[0092] Example 5

[0093] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0094] LiOCN: LiCl: Li2O: ZrCl4: Zr(OCN)4 were added in a molar ratio of 0.75: 0.75: 0.5: 0.5: 0.5, with masses of 3.672 g, 3.180 g, 1.494 g, 11.652 g, and 12.646 g, respectively; the raw materials and 326 g of zirconium dioxide ball milling balls were placed in a 2 L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400 rpm for 30 h to obtain an amorphous product Li 2.5 ZrCl 2.75 (OCN) 2.75 O 0.5 Its ionic conductivity is 4.67mS / cm, its Young's modulus is 14.61Gpa, and its all-solid-state battery rate performance is 82.05(1C / 0.1C)%.

[0095] Example 6

[0096] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0097] LiOCN: Li2O: ZrCl4: Zr(OCN)4 were added in a molar ratio of 1.5: 0.5: 0.5: 0.5, with masses of 7.344 g, 1.494 g, 11.652 g, and 12.646 g, respectively; the raw materials and 331 g of zirconium dioxide ball milling balls were placed in a 2 L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400 rpm for 30 h to obtain an amorphous product Li 2.5 ZrCl2(OCN) 3.5 O 0.5 , its XRD spectrum is as follows Figure 6 As shown; its ionic conductivity is 5.09mS / cm, its Young's modulus is 14.35Gpa, and its all-solid-state battery rate performance is 87.67(1C / 0.1C)%.

[0098] Example 7

[0099] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0100] LiOCN: LiCl: Li2O: Zr(OCN)4 were added in a molar ratio of 0.5:1:0.5:1, with masses of 2.448 g, 4.239 g, 1.494 g, and 25.929 g, respectively; the raw materials and 341 g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400 rpm for 30 h to obtain an amorphous product Li 2.5 ZrCl(OCN) 4.5 O 0.5 Its ionic conductivity is 4.82mS / cm, its Young's modulus is 13.24Gpa, and its all-solid-state battery rate performance is 85.73(1C / 0.1C)%.

[0101] Example 8

[0102] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0103] LiOCN: Li2O: Zr(OCN)4 were added in a molar ratio of 2:0.5:1, with masses of 9.792g, 1.494g, and 25.929g, respectively; the raw materials and 372g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400rpm for 30h to obtain an amorphous product Li 2.5 Zr(OCN) 5.5 O 0.5 Its ionic conductivity is 4.74mS / cm, its Young's modulus is 12.45Gpa, and its all-solid-state battery rate performance is 86.36(1C / 0.1C)%.

[0104] Example 9

[0105] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0106] LiOCN: LiCl: Li2O: ZrCl4: Zr(OCN)4 were added in a molar ratio of 0.5: 0.5: 1: 0.5: 0.5, with masses of 2.448 g, 2.120 g, 2.988 g, 11.652 g, and 12.965 g, respectively; the raw materials and 322 g of zirconium dioxide ball milling balls were placed in a 2 L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400 rpm for 30 h to obtain the amorphous product Li3ZrCl 2.5 (OCN) 2.5 O, its ionic conductivity is 3.09 mS / cm, its Young's modulus is 18.43 GPa, and its all-solid-state battery rate performance is 87.86 (1C / 0.1C)%.

[0107] Example 10

[0108] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0109] Li2O:ZrCl4:Zr(OCN)4 were added in a molar ratio of 2:0.5:0.5 with masses of 5.976g, 11.652g and 12.965g respectively; the raw materials and 306g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 30h to obtain an amorphous product Li4ZrCl2(OCN)2O2 with an ionic conductivity of 1.87mS / cm, a Young's modulus of 19.53Gpa and an all-solid-state battery rate performance of 72.05(1C / 0.1C)%.

[0110] Embodiment 11

[0111] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0112] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 9.792g and 25.929g respectively; the raw materials, 35.7g of n-heptane and 357g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 30h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 2.03mS / cm, a Young's modulus of 13.21Gpa and an all-solid-state battery rate performance of 70.15(1C / 0.1C)%.

[0113] Example 12

[0114] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0115] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 0.979g and 2.593g respectively; the raw materials, 178.5g of n-heptane and 35.7g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 30h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 1.12mS / cm, a Young's modulus of 11.09Gpa and an all-solid-state battery rate performance of 61.33(1C / 0.1C)%.

[0116] Example 13

[0117] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0118] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 9.792g and 25.929g respectively; the raw materials, 35.7g toluene and 357g zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 30h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 2.16mS / cm, a Young's modulus of 13.32Gpa and an all-solid-state battery rate performance of 69.87(1C / 0.1C)%.

[0119] Embodiment 14

[0120] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0121] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 9.792g and 25.929g respectively; the raw materials, 17.8g of n-heptane, 17.8g of toluene and 357g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 30h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 2.08mS / cm, a Young's modulus of 13.19Gpa and an all-solid-state battery rate performance of 64.75(1C / 0.1C)%.

[0122] Embodiment 15

[0123] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0124] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 9.792g and 25.929g respectively; the raw materials and 36g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 30h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 2.32mS / cm, a Young's modulus of 17.67Gpa, and an all-solid-state battery rate performance of 70.89(1C / 0.1C)%.

[0125] Example 16

[0126] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0127] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 0.979g and 2.593g respectively; the raw materials and 179g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 30h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 2.28mS / cm, a Young's modulus of 18.98Gpa, and an all-solid-state battery rate performance of 73.24(1C / 0.1C)%.

[0128] Embodiment 17

[0129] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0130] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 9.792g and 25.929g respectively; the raw materials and 357g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 200rpm for 30h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 3.09mS / cm, a Young's modulus of 14.89Gpa, and an all-solid-state battery rate performance of 80.09(1C / 0.1C)%.

[0131] Embodiment 18

[0132] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0133] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 9.792g and 25.929g respectively; the raw materials and 357g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 600rpm for 30h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 4.42mS / cm, a Young's modulus of 13.25Gpa, and an all-solid-state battery rate performance of 83.56(1C / 0.1C)%.

[0134] Embodiment 19

[0135] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0136] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 9.792g and 25.929g respectively; the raw materials and 357g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 2h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 1.09mS / cm, a Young's modulus of 16.77Gpa, and an all-solid-state battery rate performance of 81.31(1C / 0.1C)%.

[0137] Embodiment 20

[0138] This example is used to illustrate the solid electrolyte material and the preparation method thereof of the present invention.

[0139] LiOCN and Zr(OCN)4 were added in a molar ratio of 2:1 with masses of 9.792g and 25.929g respectively; the raw materials and 357g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar and high-speed ball milled at 400rpm for 60h to obtain an amorphous product Li2Zr(OCN)6 with an ionic conductivity of 3.98mS / cm, a Young's modulus of 12.36Gpa, and an all-solid-state battery rate performance of 82.47(1C / 0.1C)%.

[0140] Comparative Example 1

[0141] LiCl and ZrCl4 were added in a molar ratio of 2:1, with masses of 8.479 g and 23.304 g, respectively. The raw materials and 318 g of zirconium dioxide ball milling balls were placed in a 2L zirconium dioxide ball milling jar, and high-speed ball milling was performed at 400 rpm for 30 h to obtain an amorphous product Li2ZrCl6, whose XRD spectrum is shown as follows: Figure 7 As shown; its ionic conductivity is 0.48mS / cm, its Young's modulus is 25.90Gpa, and its all-solid-state battery rate performance is 69.30(1C / 0.1C)%.

[0142] Comparative Example 2

[0143] Li2O, LiCl, and ZrCl4 were fed in a molar ratio of 0.5:1.5:0.5 and masses of 1.494 g, 6.359 g, and 11.652 g respectively; the raw materials and 195 g of zirconia milling balls were placed in a 2 L zirconia milling jar and ball-milled at 400 rpm for 30 h to obtain the amorphous product Li 2.5 ZrCl 5.5 O 0.5 , with an ionic conductivity of 2.41 mS / cm, a Young's modulus of 19.68 GPa, and a full-solid-state battery rate performance of 71.25 (1C / 0.1C)%.

[0144] Comparative Example 3

[0145] Li2O, ZrCl4, and Zr(OCN)4 were fed in a molar ratio of 0.5:0.5:0.5 and masses of 1.494 g and 12.965 g respectively; the raw materials and 357 g of zirconia milling balls were placed in a 2 L zirconia milling jar and ball-milled at 400 rpm for 30 h to obtain the amorphous product Li2Zr(OCN)6, with an ionic conductivity of 0.96 mS / cm, a Young's modulus of 24.12 GPa, and a full-solid-state battery rate performance of 85.03 (1C / 0.1C)%.

[0146] The present invention discloses a highly amorphous halide solid electrolyte material, its preparation method, and a full-solid-state battery. The highly amorphous halide solid electrolyte material is represented by the following chemical formula: Li 2+y ZrCl 6-x-y (OCN) x O y ; where x and y satisfy the following relationship: 0 < x ≤ 6, 0 ≤ y ≤ 2, and x + y ≤ 6. By using OCN - with an ionic radius close to and larger than that of Cl - to replace part of Cl - , the effective ionic potential ratio of the solid electrolyte material is increased, thereby weakening the interaction between anions and carriers, reducing the Li + diffusion barrier, and improving the ionic conductivity. At the same time, compared with the melting point of LiCl (886 K), the melting point of LiOCN (648 K) is lower and the lattice energy is lower, enabling the material to maintain a lower Young's modulus, which helps to increase the contact area between the electrode and the solid electrolyte. Furthermore, based on the highly amorphous halide solid electrolyte material Li 2+y ZrCl 6-x-y (OCN) x O yThe all-solid-state battery has excellent rate performance, and the raw materials used to prepare the highly amorphous halide solid electrolyte material are inexpensive, which is conducive to the large-scale production of the material.

[0147] The above description has fully disclosed the specific embodiments of the present invention. It should be pointed out that any changes made by those skilled in the art to the specific embodiments of the present invention do not deviate from the scope of the claims of the present invention. Accordingly, the scope of the claims of the present invention is not limited to the above specific embodiments.

Claims

1. A highly amorphous halide solid electrolyte material, characterized in that: The high-amorphization halide solid electrolyte material is represented by the following chemical formula: Li 2+y ZrCl 6-x-y (OCN) x O y ; Wherein, x and y satisfy the following relationship: 0 < x ≤ 6, 0 ≤ y ≤ 2, and x + y ≤ 6.

2. A highly amorphous halide solid electrolyte material according to claim 1, characterized in that: The high-amorphization halide solid electrolyte material is an amorphous compound.

3. A method for preparing the highly amorphous halide solid electrolyte material according to any one of claims 1 and 2, characterized in that: The method includes: Providing a lithium raw material and a zirconium raw material, the lithium raw material includes at least one of Li2O, Li2O2, LiOCN, and LiCl, the zirconium raw material includes at least one of ZrCl4, ZrOCl2, and Zr(OCN)4, and at least one of the lithium raw material and the zirconium raw material contains cyanate; Performing an amorphization reaction on the lithium raw material and the zirconium raw material to obtain the high-amorphization halide solid electrolyte material.

4. The method for preparing a highly amorphous halide solid electrolyte material according to claim 3, characterized in that: The performing an amorphization reaction on the lithium raw material and the zirconium raw material to obtain the high-amorphization halide solid electrolyte material includes: Placing the lithium raw material and the zirconium raw material in a ball milling container and performing ball milling with ball milling balls to obtain a first amorphization reaction product; the first amorphization reaction product includes the high-amorphization halide solid electrolyte material and the ball milling balls; Based on the obtained first amorphization reaction product, using a sieve to remove the ball milling balls to obtain the high-amorphization halide solid electrolyte material.

5. The method for preparing a highly amorphous halide solid electrolyte material according to claim 4, characterized in that: The mass ratio of the total mass of the lithium raw material and the zirconium raw material to the mass of the ball milling balls is 1:(1 - 50).

6. The method for preparing a highly amorphous halide solid electrolyte material according to claim 4, characterized in that: The time of the ball milling is 2 - 60 h.

7. A method for preparing a highly amorphous halide solid electrolyte material according to claim 4, characterized in that: The rotation speed of the ball milling is 200 - 600 rpm.

8. The method for preparing a highly amorphous halide solid electrolyte material according to claim 3, characterized in that: The performing an amorphization reaction on the lithium raw material and the zirconium raw material to obtain the high-amorphization halide solid electrolyte material includes: Placing the lithium raw material and the zirconium raw material in a dispersion medium to perform an amorphization reaction to obtain a second amorphization reaction product; the amorphization reaction product includes the high-amorphization halide solid electrolyte material and the dispersion medium; The dispersion medium includes: one or more of saturated alkane solvents or benzene solvents; Based on the obtained second amorphization reaction product, using a vacuum filtration device to remove the dispersion medium to obtain the high-amorphization halide solid electrolyte material.

9. The method for preparing a highly amorphous halide solid electrolyte material according to claim 8, characterized in that: The mass ratio of the total mass of the lithium raw material and the zirconium raw material to the mass of the dispersion medium is 1:(0 - 50).

10. An all-solid-state battery, characterized in that: Including a high-amorphization halide solid electrolyte material according to any one of claims 1 - 2.