Deoxidizer composition, deoxidizer package, and method for producing deoxidizer package

By covering metal salt on the iron surface and forming a water film of a specific thickness, the oxygen absorption reaction speed is controlled, and the problem of deterioration of oxygen absorption performance caused by the fast oxygen absorption rate of iron deoxidants in the atmosphere is solved, and the oxygen absorption performance during operation in the atmosphere is realized. Stable oxygen absorption performance.

CN119031972APending Publication Date: 2024-11-26MITSUBISHI GAS CHEM CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026590.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-03-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing iron-based deoxidant absorbs oxygen at a fast speed when operating in the atmosphere, but it is easy to cause excessive deoxidation reaction, resulting in deterioration of oxygen absorption performance in the sealed container, and it is difficult to maintain sufficient oxygen absorption performance after operating in the atmosphere for a certain period of time.

Method used

A deoxidant composition containing iron, metal salt and water is used, wherein the metal salt covers the iron surface to form a water film of a specific thickness to control the oxygen absorption reaction rate and inhibit the rapid progress of the deoxidation reaction in the atmosphere.

Benefits of technology

After operating in the atmosphere for a certain period of time, sufficient oxygen absorption performance can be maintained, which avoids deterioration of oxygen absorption performance and improves the stability and use efficiency of iron-based deoxidants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005035614790000241
    Figure BDA0005035614790000241
Patent Text Reader

Abstract

A deoxidizer composition containing iron, a metal salt, and water, the content of water present on the surface of iron per unit surface area of iron [content (g) of water present on the surface of iron / {content (g) of iron * specific surface area (m2 / g) of iron}] being more than 2.00 g / m2 and 3.50 g / m2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a deoxidizer composition, a deoxidizer package and a method for producing the deoxidizer package. Background Art

[0002] As a preservation technology for food, medicine, etc., a method using a deoxidizer is known. In this method, by enclosing the stored article and the deoxidizer in a gas-barrier sealed container and sealing, the deoxidizer absorbs the oxygen in the sealed container, and the atmosphere in the sealed container can be substantially kept in an oxygen-free state. As the function of the deoxidizer, it is necessary for it to be small and absorb more oxygen. In other words, a deoxidizer composition with a high oxygen absorption per unit volume is required.

[0003] Representative deoxidizers include iron-based deoxidizers with iron (iron powder) as the main agent and non-iron-based deoxidizers with ascorbic acid, glycerol, etc. as the main agent. The deoxidizer is appropriately selected according to the application, but iron-based deoxidizers are widely used from the viewpoint of oxygen absorption performance.

[0004] Under such circumstances, attempts have been made to improve the oxygen absorption rate of the iron-based deoxidizer.

[0005] For example, Patent Document 1 discloses an iron-based deoxidizer composition containing a water retaining agent, a swelling agent, an ammonium salt, and water, thereby achieving an improvement in oxygen absorption rate.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2021-146292 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] On the other hand, there is a tendency that the oxygen absorption rate of the iron-based deoxidizer is improved more, and the operation in the atmosphere is more difficult. Usually, the deoxidizer is degassed and packaged in a gas barrier packaging material and kept before use, and the packaging material is opened before use and the deoxidizer is taken out in the atmosphere, and is sealed in a sealed container together with the stored article and used. In the case of such use, there is a problem that the deoxidation reaction during the operation in the atmosphere of the iron-based deoxidizer with particularly fast oxygen absorption rate is also rapidly promoted, and the oxygen absorption performance deteriorates after being sealed in a sealed container.

[0011] Therefore, to date, the contradictory issues of improving the oxygen absorption rate and suppressing the degradation (deactivation) in the atmosphere have been addressed by (1) designing the composition of the deoxidizer composition in a manner that appropriately balances the two, or (2) considering the degree of degradation in the atmosphere in advance and using a large amount of the deoxidizer composition, etc., but further improvements are required.

[0012] Therefore, an object of the present invention is to provide a deoxidizer composition, a deoxidizer package, and a method for producing a deoxidizer package that can exhibit sufficient oxygen absorption performance even after being operated in the atmosphere for a certain period of time.

[0013] Solutions for solving problems

[0014] That is, the gist of the present invention is as follows.

[0015] [1] A deoxidizer composition comprising: iron, a metal salt and water,

[0016] The content of water present on the surface of iron per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g) × specific surface area of ​​iron (m 2 / g)}] more than 2.00g / m 2 And 3.50g / m 2 the following.

[0017] [2] The deoxidizer composition according to [1] above, wherein at least a portion of the metal salt is present on the surface of the iron.

[0018] [3] The deoxidizer composition according to [2] above, wherein the surface of the iron is coated with a metal salt present on the surface of the iron.

[0019] [4] The deoxidizer composition according to [2] or [3] above, wherein the metal salt present on the surface of the iron is one or more selected from the group consisting of calcium chloride, calcium bromide and sodium bromide.

[0020] [5] The deoxidizer composition according to any one of [2] to [4] above, wherein the content of the metal salt present on the surface of the iron is 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the iron.

[0021] [6] The deoxidizer composition according to any one of [1] to [5], wherein the specific surface area of ​​the iron is 0.03 m 2 / g or more and 0.20m 2 / g or less.

[0022] [7] The deoxidizer composition according to any one of [1] to [6] above, wherein the average particle size (D50) of the iron is 1 μm or more and 1000 μm or less.

[0023] [8] An oxygen decomposing agent package comprising: the oxygen decomposing agent composition according to any one of [1] to [7] above, and an air-permeable packaging container containing the oxygen decomposing agent composition.

[0024] [9] A method for producing a deoxidizer package, comprising the following steps (I) to (III).

[0025] Step (I): a step of obtaining a deoxidizing agent composition (a) containing a metal salt and iron

[0026] Step (II): water is supplied to the deoxidizer composition (a) to obtain a content of water present on the surface of iron per unit surface area of ​​iron, which contains iron, metal salt and water [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)}] more than 2.00g / m 2 And 3.50g / m 2 The following steps of preparing the deoxidizer composition (A)

[0027] Step (III): a step of placing at least one of the oxygen scavenger composition (a) and the oxygen scavenger composition (A) in a gas-permeable packaging container (b1)

[0028]

[10] The method for producing a deoxidizer package according to the above [9], wherein the following steps (III-1) and (II-1) are sequentially performed following the step (I).

[0029] Step (III-1): a step of placing the oxygen scavenger composition (a) in the air-permeable packaging container (b1)

[0030] Step (II-1): A step of supplying water to the oxygen scavenger composition (a) through the air-permeable packaging container (b1) to obtain the oxygen scavenger composition (A)

[0031]

[11] The method for producing a deoxidizer package according to

[10] , further comprising the following step (IV-1).

[0032] Step (IV-1): a step of further placing the air-permeable packaging container (b1) containing the oxygen scavenger composition (A) in a gas barrier container (b2)

[0033]

[12] The method for producing a deoxidizer package according to the above [9], wherein the following steps (III-2), (IV-2) and (II-2) are sequentially performed following the above step (I).

[0034] Step (III-2): a step of placing the oxygen scavenger composition (a) and the water supply agent in the air-permeable packaging container (b1)

[0035] Step (IV-2): A step of further housing the breathable packaging container (b1) containing the aforementioned deoxidizer composition (a) and the aforementioned water supply agent in a gas-barrier container (b2).

[0036] Step (II-2): A step of supplying water from the aforementioned water supply agent to the aforementioned deoxidizer composition (a) to obtain the aforementioned deoxidizer composition (A).

[0037] Effects of the Invention

[0038] According to the present invention, it is possible to provide: a deoxidizer composition, a deoxidizer package, and a method for manufacturing a deoxidizer package that can exhibit sufficient oxygen absorption performance even after being operated in the atmosphere for a certain period of time. Detailed Embodiments

[0039] Embodiments of the deoxidizer composition, the deoxidizer package, and the method for manufacturing a deoxidizer package according to the present invention will be described in detail below.

[0040] It should be noted that in this specification, the term "A to B" for the description of numerical values means "not less than A and not more than B" (when A < B) or "not more than A and not less than B" (when A > B). In addition, in the present invention, a combination of preferred modes is a more preferred mode.

[0041] [Deoxidizer Composition]

[0042] The deoxidizer composition of the present invention contains: iron, a metal salt, and water. The content of water present on the surface of iron per unit surface area of iron [content of water present on the surface of iron (g) / {content of iron (g) × specific surface area of iron (m 2 / g)}] exceeds 2.00 g / m 2 and is 3.50 g / m 2 or less.

[0043] It should be noted that in this specification, the "content of water present on the surface of iron per unit surface area of iron" is an index of the "thickness of the water film formed on the surface of iron". If the "content of water present on the surface of iron per unit surface area of iron" is within the above-specified range, it means that a water film with a specified thickness is formed on the surface of iron.

[0044] The deoxidizer composition of the present invention can exhibit sufficient oxygen absorption performance even after being operated in the atmosphere for a certain period of time due to the above composition.

[0045] The reason for the deoxidizer composition of the present invention to exhibit the above effects is not certain, but it is speculated as follows.

[0046] First, in the case of an iron-based deoxidizer, iron reacts with water and oxygen to cause a rapid deoxidation reaction. In addition, it is known that such an iron-based deoxidizer generally has a fast reaction rate at the beginning of the deoxidation reaction.

[0047] In addition, the water in the above deoxidation reaction can be: the case where water vapor (water evaporated from the stored object, etc.) in the deoxidation environment is used (water-dependent type); and the case where a water-containing carrier (water supply agent, etc.) is included in the deoxidizer package in advance (self-reaction type). In either case, in order for iron to absorb oxygen, water must be introduced to the surface of iron, and the deliquesce phenomenon of metal salts is used for this.

[0048] In addition, the inventors of the present invention further analyzed the reaction of iron's oxygen absorption, and speculated that the above reaction is not a direct reaction between iron and gaseous water (water vapor) and oxygen, but a mechanism in which a water film is formed on the surface of the iron by first utilizing the deliquesce phenomenon of the metal salt, and the water and dissolved oxygen in the water film react with the iron.

[0049] Based on the above mechanism, it is believed that as the initial stage of the deoxidation reaction, when a water film is formed on the surface of iron, appropriate water and oxygen (dissolved oxygen) are supplied to the surface of iron, and the reaction rate of the deoxidation reaction becomes faster. It is believed that as the water absorption further advances and the thickness of the water film gradually increases, the concentration of dissolved oxygen in the water film decreases due to the diffusion law, and the reaction rate of the deoxidation reaction slows down.

[0050] It is believed that in the deoxidizer composition of the present invention, a water film having a predetermined thickness is formed on the surface of iron in advance, so that in the initial stage of the deoxidation reaction, the reaction rate can be slowed down based on the thick water film, and deterioration in the atmosphere can be suppressed. In addition, it is believed that by making the thickness of the water film a predetermined thickness, the initial thickness of the water film decreases based on evaporation and reaction in the atmosphere, and after a certain period of time, the thickness of the water film becomes the optimal thickness, and a high oxygen absorption performance can be exerted.

[0051] Hereinafter, each component and the like will be described.

[0052] (iron)

[0053] The shape of the iron contained in the deoxidizer composition of the present invention is not particularly limited, and from the viewpoint of oxygen absorption performance, ease of acquisition and ease of operation, iron powder is preferred. The surface of the iron powder is preferably exposed iron (metallic iron of zero valence), but within the scope of not hindering the effect of the present invention, it can have an extremely thin oxide film as the usual metal surface. Specifically, it can be suitable to use reduced iron powder, electrolytic iron powder, spray iron powder (atomized iron powder) etc. In addition, crushed objects and cut products such as cast iron can also be used.

[0054] The iron powder may be used alone or in combination of two or more kinds as required. Commercial products of these iron powders are easily available and may be used.

[0055] The average particle size (D50) of the iron powder is preferably 3000 μm or less, more preferably 1000 μm or less, and further preferably 300 μm or less from the viewpoint of good contact with oxygen, and is preferably 1 μm or more, more preferably 10 μm or more, and further preferably 20 μm or more from the viewpoint of suppressing the generation of dust. More specifically, the average particle size (D50) of the iron powder is preferably 1 μm or more and 3000 μm or less, more preferably 1 μm or more and 1000 μm or less, further preferably 10 μm or more and 1000 μm or less, and further preferably 20 μm or more and 300 μm or less.

[0056] It should be noted that the iron powder having an average particle size within the above range can be obtained by appropriately selecting commercially available iron powder or by, for example, classifying using a sieve that matches the desired average particle size.

[0057] The average particle size can be measured as an average particle size (D50) of cumulative frequency 50% in volume-based particle size distribution, for example, using a commercially available laser diffraction / scattering particle size distribution analyzer (LA-960 manufactured by Horiba, Ltd.).

[0058] In addition, the specific surface area of ​​the iron powder is preferably 0.03 m 2 / g or more, more preferably 0.05m 2 / g or more, and from the viewpoint of suppressing the generation of dust, preferably 0.20 m 2 / g or less, more preferably 0.10m 2 / g or less, more preferably 0.09m 2 More specifically, the specific surface area of ​​the iron powder is preferably 0.03 m 2 / g or more and 0.20m 2 / g or less, more preferably 0.03m 2 / g or more and 0.10m 2 / g or less, more preferably 0.05m 2 / g or more and 0.09m 2 / g or less.

[0059] It should be noted that the specific surface area of ​​the iron powder can be measured by the BET multipoint method. Specifically, it can be measured according to the method described in the Examples.

[0060] The deoxidizer composition of the present invention contains iron as a main agent. The content of iron is not particularly limited, but is preferably 40% by mass or more and 98% by mass or less, more preferably 45% by mass or more and 95% by mass or less, and further preferably 50% by mass or more and 90% by mass or less.

[0061] It should be noted that, when the deoxidizer composition does not contain a water supply agent, the iron content in the deoxidizer composition may be preferably 70 mass % or more and 98 mass % or less, more preferably 75 mass % or more and 95 mass % or less, further preferably 75 mass % or more and 90 mass % or less, and further preferably 75 mass % or more and 85 mass % or less.

[0062] When the deoxidizer composition contains a water supply agent, the iron content in the deoxidizer composition may be preferably 40 mass % to 75 mass %, more preferably 45 mass % to 65 mass %, and further preferably 50 mass % to 60 mass %.

[0063] (Metal Salt)

[0064] The metal salt contained in the deoxidizer composition of the present invention is a substance that catalyzes the oxidation reaction of iron and improves the activity of iron. In addition, the metal salt plays a role in preventing the water contained in the deoxidizer composition from evaporating and being lost from the deoxidizer composition.

[0065] In addition, the deoxidizer composition of the present invention needs to form a water film of a predetermined thickness on the surface of iron in advance, but when water is introduced to the surface of iron, the deliquescing phenomenon of the metal salt is utilized. Therefore, the metal salt is preferably at least partially, more preferably mainly present on the surface of iron.

[0066] Here, "at least a part of the metal salt is present on the surface of iron" means that a part or all of the metal salt contained in the deoxidizer composition is present on the surface of iron. The deoxidizer composition of the present invention may also include a water supply agent as described later, and the water supply agent sometimes includes a metal salt, but the metal salt is supported on the carrier of the water supply agent, and therefore, is distinguished from the metal salt present on the surface of iron. Therefore, when the deoxidizer composition includes a water supply agent, as long as a part of the metal salt is present on the surface of iron, the rest may also be supported on the carrier of the water supply agent.

[0067] In addition, “the metal salt is mainly present on the surface of iron” means that substantially all of the metal salt is present on the surface of iron, for example, when no component containing a metal salt such as a water supply agent is blended in the deoxidizer composition.

[0068] In addition, the metal salt present on the surface of the iron is more preferably formed by covering the surface of the iron. It should be noted that the method for the metal salt to cover the surface of the iron is not particularly limited, for example, as described later, after mixing iron powder with an aqueous solution containing the metal salt, drying, removing moisture, and making the metal salt adhere to the surface of the iron powder, it can be carried out.

[0069] The metal salt is not particularly limited, but preferably a deliquescent metal salt. Among them, a metal halide is preferred. As the metal halide, any generally known one can be used without particular limitation.

[0070] The metal in the metal halide is not particularly limited, and examples thereof include at least one selected from the group consisting of alkali metals, alkaline earth metals, copper, zinc, aluminum, tin, iron, cobalt, and nickel. Among them, at least one selected from the group consisting of lithium, potassium, sodium, magnesium, calcium, barium, and iron is more preferred, and at least one selected from the group consisting of sodium and calcium is further preferred.

[0071] The halide in the metal halide is not particularly limited, and examples thereof include chlorides, bromides, and iodides. Preferably, the halide is at least one selected from the group consisting of chlorides and bromides.

[0072] As the metal halide, in view of handleability, safety, etc., at least one selected from the group consisting of calcium chloride, sodium chloride, calcium bromide, sodium bromide, calcium iodide, and sodium iodide is preferred.

[0073] In particular, as the metal salt present on the surface of iron, from the viewpoint of controlling the thickness of the water film, at least one selected from the group consisting of calcium chloride, calcium bromide and sodium bromide is more preferably used.

[0074] The metal salt may be used alone or in combination of two or more kinds as required. In addition, these metal salts are easily commercially available and may be used.

[0075] The content of the metal salt is not particularly limited, but is preferably 0.09% by mass or more and 20% by mass or less, more preferably 0.10% by mass or more and 15% by mass or less, and further preferably 0.50% by mass or more and 10% by mass or less in the deoxidizer composition. In addition, the content of the metal salt in the deoxidizer composition excluding the water supply agent is preferably 0.09% by mass or more and 9.0% by mass or less, more preferably 0.10% by mass or more and 7.0% by mass or less, and further preferably 0.50% by mass or more and 5.0% by mass or less.

[0076] In addition, the content of the metal salt is preferably 0.1 mass part or more and 25 mass parts or less, and more preferably 0.1 mass part or more and 20 mass parts or less, relative to 100 mass parts of iron. It should be noted that when the deoxidizer composition does not contain a water supply agent, the content of the metal salt is further preferably 0.1 mass part or more and 10 mass parts or less, further preferably 0.1 mass part or more and 5 mass parts or less, further preferably 0.2 mass part or more and 5 mass parts or less, and further preferably 0.2 mass part or more and 3 mass parts or less. In addition, when the deoxidizer composition contains a water supply agent, the content of the metal salt is further preferably 1.0 mass part or more and 20 mass parts or less, further preferably 5.0 mass parts or more and 15 mass parts or less, and further preferably 10 mass parts or more and 15 mass parts or less.

[0077] The content of the metal salt present on the surface of the iron is not particularly limited, but is preferably 0.09% by mass or more and 9.0% by mass or less, more preferably 0.10% by mass or more and 5.0% by mass or less, and further preferably 0.10% by mass or more and 2.9% by mass or less in the deoxidizer composition. In addition, the content of the metal salt present on the surface of the iron is preferably 0.09% by mass or more and 9.0% by mass or less, more preferably 0.10% by mass or more and 7.0% by mass or less, and further preferably 0.50% by mass or more and 5.0% by mass or less in the deoxidizer composition excluding the water supply agent.

[0078] In addition, the content of the metal salt present on the surface of the iron is preferably 0.1 mass part or more and 20 mass parts or less, more preferably 0.1 mass part or more and 15 mass parts or less, further preferably 0.1 mass part or more and 10 mass parts or less, further preferably 0.3 mass part or more and 10 mass parts or less, further preferably more than 0.8 mass part and 10 mass parts or less. It should be noted that when the deoxidizer composition does not contain a water supply agent, the content of the metal salt present on the surface of the iron is further preferably 0.7 mass part or more and 5 mass parts or less, further preferably 0.7 mass part or more and 3 mass parts or less relative to 100 mass parts of iron. In addition, when the deoxidizer composition contains a water supply agent, the content of the metal salt present on the surface of the iron is further preferably 1.0 mass part or more and 7.0 mass parts or less, further preferably 2.0 mass parts or more and 7.0 mass parts or less relative to 100 mass parts of iron.

[0079] (water)

[0080] The water contained in the deoxidizing agent composition of the present invention is a component necessary for the deoxidation reaction to proceed.

[0081] In addition, the deoxidizer composition of the present invention needs to form a water film of a predetermined thickness on the surface of iron in advance, but it is believed that at this time, water is introduced into the metal salt present on the surface of iron by utilizing the deliquescence phenomenon of the metal salt. Therefore, water is preferably present on the surface of iron at least partially, more preferably mainly together with the metal salt.

[0082] Here, "at least a part of the water is present on the surface of the iron" means that a part or all of the water contained in the deoxidizer composition is present on the surface of the iron. The deoxidizer composition of the present invention may include a water supply agent as described later, and the water supply agent includes water, but the water is carried on the carrier of the water supply agent, and therefore, is distinguished from the water present on the surface of the iron. Therefore, when the deoxidizer composition includes a water supply agent, as long as a part of the water is present on the surface of the iron, the rest can be carried on the carrier of the water supply agent.

[0083] In addition, “water exists mainly on the surface of iron” means that substantially all of the water exists on the surface of iron, for example, when no water-containing component such as a water supply agent is blended in the deoxidizer composition.

[0084] Furthermore, it is more preferable that the water present on the surface of iron covers the surface of iron together with the metal salt.

[0085] In the deoxidizer composition of the present invention, by controlling the thickness of the water film formed on the surface of iron to a predetermined thickness, sufficient oxygen absorption performance can be exerted even after operating in the atmosphere for a certain period of time. It should be noted that the thickness of the water film can be the content of water present on the surface of iron relative to the per unit surface area of ​​iron as an index.

[0086] The content of water present on the surface of iron per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g) × specific surface area of ​​iron (m 2 / g)}] more than 2.00g / m 2 And 3.50g / m 2 If the content of water on the surface of iron per unit surface area is 2.00 g / m 2 If the water film is less than 3.50 g / m, the oxygen absorption rate is fast, so it will deteriorate after being placed in the atmosphere for a certain period of time and cannot fully exert its oxygen absorption performance. In addition, it is believed that if the content of water on the surface of iron exceeds 3.50 g / m 2 , the water film is too thick, so even if it is placed in the atmosphere for a certain period of time, the thickness of the water film cannot be optimized, and the oxygen absorption rate slows down. In addition, the content of water on the surface of iron relative to the per unit surface area of ​​iron is preferably 2.01g / m 2 Above and 3.10g / m 2 Below, more preferably 2.10g / m 2Above and 3.10g / m 2 the following.

[0087] The content of water present on the surface of iron per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)} within a specified range is not particularly limited, and for example, (1) the method of supplying water to the surface of iron and its conditions are appropriately selected, or (2) the content of metal salt present on the surface of iron is adjusted, so that the desired thickness can be controlled. In particular, when water is introduced to the surface of iron, the deliquescence phenomenon of the metal salt is utilized, and therefore, it is more preferable to control it by the method (2) above. In this case, it is believed that the more the content of metal salt present on the surface of iron is increased, the more the content of water present on the surface of iron relative to the unit surface area of ​​iron [the content of water present on the surface of iron (g) / {the content of iron (g)×the specific surface area of ​​iron (m 2 / g)}.

[0088] It should be noted that the water content in the deoxidizer composition is not particularly limited, but is preferably 5% by mass or more and 40% by mass or less, more preferably 10% by mass or more and 30% by mass or less, and further preferably 10% by mass or more and 25% by mass or less. In addition, the water content in the deoxidizer composition excluding the water supply agent is preferably 5% by mass or more and 34% by mass or less, more preferably 10% by mass or more and 30% by mass or less, further preferably 14% by mass or more and 28% by mass or less, and further preferably 14% by mass or more and 25% by mass or less.

[0089] The water content is preferably 6 parts by mass to 35 parts by mass, more preferably 10 parts by mass to 35 parts by mass, and even more preferably 15 parts by mass to 30 parts by mass, relative to 100 parts by mass of iron, from the viewpoint of oxygen absorption performance.

[0090] (Water supply agent)

[0091] The deoxidizer composition of the present invention may further contain a water supply agent. The water supply agent is a carrier impregnated with water (a water-containing carrier), and supplies water to iron.

[0092] The water supply agent preferably comprises: a carrier, a metal salt and water.

[0093] As the carrier, any carrier can supply the water to be loaded to the iron, and granular materials such as zeolite, calcined diatomaceous earth, silica gel, pearlite, vermiculite, activated alumina, activated clay, activated carbon, and bentonite are usually suitable. Among them, zeolite, calcined diatomaceous earth, and activated carbon are preferred.

[0094] As the metal salt, the aforementioned components can be used, but sodium chloride is preferred.

[0095] When the deoxidizer composition of the present invention includes a water supply agent, the content of the water supply agent is not particularly limited as long as it is an amount that can provide the required amount of water. For example, in the deoxidizer composition, it is preferably 12% by mass or more and 85% by mass or less, more preferably 25% by mass or more and 70% by mass or less, further preferably 35% by mass or more and 70% by mass or less, and further preferably 35% by mass or more and 60% by mass or less. In addition, the content of the water supply agent is preferably 15 parts by mass or more and 500 parts by mass or less, more preferably 30 parts by mass or more and 200 parts by mass or less, further preferably 30 parts by mass or more and 150 parts by mass or less, further preferably 50 parts by mass or more and 130 parts by mass or less, and further preferably 50 parts by mass or more and 100 parts by mass or less, relative to 100 parts by mass of iron.

[0096] In addition, when the deoxidizer composition of the present invention contains a water supply agent, the content of the carrier in the deoxidizer composition is preferably 15 mass% or more and 100 mass% or less, more preferably 15 mass% or more and 60 mass% or less, further preferably 20 mass% or more and 40 mass% or less, and further preferably 20 mass% or more and 30 mass% or less. In addition, the content of the carrier is preferably 20 mass parts or more and 150 mass parts or less, more preferably 30 mass parts or more and 100 mass parts or less, further preferably 30 mass parts or more and 80 mass parts or less, and further preferably 30 mass parts or more and 50 mass parts or less, relative to 100 mass parts of iron.

[0097] (Other ingredients)

[0098] The deoxidizer composition of the present invention may contain other components as required in addition to the above components. Examples of other components include alkaline substances, swelling agents, fluidity improvers, catalysts, odor adsorbents, heat dispersants, and the like.

[0099] <Shape of deoxidizer composition>

[0100] The shape of the deoxidizer composition of the present invention is not particularly limited, and examples thereof include spherical, substantially spherical, elliptical and cylindrical shapes. From the perspective of better packing properties and a tendency for higher bulk density, spherical and substantially spherical shapes are preferred, and spherical shapes are more preferred.

[0101] [Method for producing deoxidizer composition]

[0102] The method for producing the deoxidizer composition of the present invention is not particularly limited, but preferably comprises, for example, the following steps (i) and (ii) in order.

[0103] Step (i): a step of obtaining a deoxidizing agent composition (a) containing iron and a metal salt

[0104] Step (ii): water is supplied to the deoxidizer composition (a) to obtain a solution containing iron, a metal salt and water, and the content of water present on the surface of the iron relative to the unit surface area of ​​the iron [content of water present on the surface of the iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)}] more than 2.00g / m 2 And 3.50g / m 2 The following steps of preparing the deoxidizer composition (A)

[0105] <Step (i)>

[0106] Step (i) is a step of obtaining a deoxidizing agent composition (a) containing iron and a metal salt.

[0107] Concerning iron and metal salts, as described above.

[0108] In the obtained deoxidizer composition (a), the metal salt is preferably present on the surface of iron, and more preferably covers the surface of iron. The method for obtaining such a deoxidizer composition (a) is not particularly limited, and for example, an aqueous solution of a metal salt is mixed with iron powder and dried to obtain iron powder with a metal salt attached thereto.

[0109] When the metal salt is made into an aqueous solution as a raw material, the concentration of the salt is preferably 1% by mass or more and 40% by mass or less, more preferably 2% by mass or more and 30% by mass or less, and further preferably 10% by mass or more and 30% by mass or less. By being within the above range, the iron powder and the metal salt aqueous solution can be uniformly mixed, and the metal salt can be uniformly covered on the surface of the iron powder.

[0110] <Step (ii)>

[0111] Step (ii) is to supply water to the deoxidizer composition (a) to obtain a solution containing iron, a metal salt and water, wherein the content of water present on the surface of the iron relative to the unit surface area of ​​the iron is [content of water present on the surface of the iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)}] more than 2.00g / m 2 And 3.50g / m 2 The following steps are performed for the deoxidizer composition (A).

[0112] According to this step, a water film having a desired thickness can be formed on the surface of iron, and a deoxidizer composition can be obtained which can exhibit sufficient oxygen absorbing performance even after being operated in the atmosphere for a certain period of time.

[0113] The method of supplying water to the deoxidizer composition (a) is not particularly limited, and examples thereof include the following methods.

[0114] First, (1) in the case of supplying water by moisture absorption from the outside, there can be cited a method of placing the deoxidizer composition (a) in an atmosphere adjusted to a predetermined humidity for a certain period of time to absorb water; a method of bringing the deoxidizer composition (a) into contact with a water-containing body (e.g., wetted absorbent cotton, etc.) to supply water from the water-containing body to the deoxidizer composition (a), etc. According to these methods, by appropriately adjusting the humidity and the placement time, as well as the water content and contact time of the water-containing body, etc., a water film having a desired thickness can be formed on the surface of iron.

[0115] In addition, (2) a method of further mixing a water-containing carrier (water supply agent, etc.) into the deoxidizer composition (a) and supplying water from the water-containing carrier to the deoxidizer composition (a) can also be mentioned. According to this method, a water film having a desired thickness can be formed on the surface of iron by adjusting the amount of the water-containing carrier, the water content of the water-containing carrier, etc. It should be noted that the deoxidizer composition (A) obtained by this method substantially contains a carrier in addition to iron, a metal salt and water.

[0116] It should be noted that, in any of the above methods, once water starts to be supplied to the deoxidizer composition (a), the deoxidation reaction of iron will proceed. Therefore, step (ii) is preferably carried out in an inert atmosphere, and the deoxidizer composition (A) obtained is preferably stored in an inert atmosphere until it is used as a deoxidizer.

[0117] The mixing device for mixing the above-mentioned components is not particularly limited. As specific examples, a ribbon mixer (manufactured by Ohno Chemical Machinery Co., Ltd.), a Nauta mixer (manufactured by Hosokawa Micron Corporation), a cone mixer (manufactured by Ohno Chemical Machinery Co., Ltd.), a vertical granulator (manufactured by POWREX CORP.), an SP granulator (manufactured by Dalton Co., Ltd.), a high-speed mixer (manufactured by EARTHTECHNICA Co., Ltd.) and a granulator (manufactured by AKIRAKIKO Co., Ltd.) can be used.

[0118] [Deoxidizer packaging]

[0119] The oxygen deoxidizer package of the present invention comprises: the above-mentioned oxygen deoxidizer composition and a gas-permeable packaging container accommodating the oxygen deoxidizer composition.

[0120] (Breathable packaging container)

[0121] There is no particular limitation on the air-permeable packaging container as long as it is a container containing a packaging material used for the deoxidizer. From the viewpoint of fully exerting the oxygen absorption performance of the deoxidizer package, it contains at least an air-permeable packaging material, and examples thereof include: a bag-shaped bag formed by laminating two air-permeable packaging materials; a bag-shaped bag formed by laminating one air-permeable packaging material and one non-air-permeable packaging material; a bag-shaped bag formed by folding one air-permeable packaging material and sealing the edges except the folded part. In addition, a container in which an air-permeable packaging material is adhered to the opening surface of a non-air-permeable rigid container, etc. can also be mentioned.

[0122] Here, when the air-permeable packaging material and the non-air-permeable packaging material are square, the air-permeable packaging material may be formed into a bag shape by overlapping two air-permeable packaging materials and heat-sealing four sides; one air-permeable packaging material and one non-air-permeable packaging material are overlapped and heat-sealed four sides to form a bag shape; one air-permeable packaging material is folded and three sides other than the folded portion are heat-sealed to form a bag shape. In addition, the packaging material may be formed into a bag shape by forming the air-permeable packaging material into a tube and heat-sealing both ends of the tube and the main body.

[0123] (Breathable packaging material)

[0124] As the air-permeable packaging material, a packaging material that is permeable to oxygen and water vapor is selected. Among them, it is suitable to use a packaging material with an air permeability resistance of 600 seconds or less, more preferably 90 seconds or less, and further preferably 30 seconds or less based on the Gurley tester method. Here, the air permeability resistance refers to the value measured according to the method of JIS P8117:2009. More specifically, it refers to the time required for 100 mL of air to pass through the air-permeable packaging material using a Gurley air permeability meter (manufactured by Toyo Seiki Seisaku-sho, Ltd.).

[0125] As the above-mentioned breathable packaging material, in addition to paper and nonwoven fabrics, a breathable packaging material obtained by imparting air permeability to a plastic film can be used. As the plastic film, for example, a laminated film obtained by laminating and bonding a film of polyethylene terephthalate, polyamide, polypropylene, polycarbonate, etc., and a film of polyethylene, ionomer, polybutadiene, ethylene acrylic acid copolymer, ethylene methacrylic acid copolymer, or ethylene vinyl acetate copolymer, etc., as a sealant layer can be used. In addition, these laminates can also be used as breathable packaging materials.

[0126] As a method of imparting air permeability, various methods can be adopted in addition to perforation processing using a cold needle or a hot needle. When imparting air permeability by perforation processing, the air permeability can be freely adjusted by the diameter, number, material, etc. of the holes to be perforated.

[0127] The thickness of the laminated film is preferably 50 to 300 μm, particularly preferably 60 to 250 μm. In this case, a packaging material having excellent strength, heat-sealing properties, and packaging suitability can be obtained compared to a case where the thickness is not within the above range.

[0128] (Non-breathable packaging material)

[0129] As the non-air-permeable packaging material, the packaging material used for deoxidizer applications can be used, and suitable ones are those that can block moisture, alcohol, oil, and solid components of the stored items and have sealing properties. Specifically, there can be mentioned those with an oxygen permeability of 0.05 to 20 mL / m, such as polyethylene terephthalate, nylon-based coextruded multilayer sheets and films. 2 ·24 hr·atm (25°C, 50% RH) laminates, etc.

[0130] (Gas barrier container)

[0131] The deoxidizer package of the present invention may include: a gas barrier container further storing the gas permeable packaging container storing the above-mentioned deoxidizer composition. By storing the gas permeable packaging container storing the above-mentioned deoxidizer composition in the gas barrier container, air permeability with the outside can be blocked, and in particular, the inflow of oxygen into the gas barrier container and the outflow of water vapor can be prevented, and the oxygen absorption performance can be well maintained until it is used as a deoxidizer.

[0132] The gas-tight container is not particularly limited as long as it can be sealed and has substantial gas-tight properties, but is preferably made of the above-mentioned non-gas-permeable material from the viewpoint of blocking external air permeation.

[0133] Specifically, multilayer sheets and films having a laminated structure such as polyethylene terephthalate / aluminum vapor deposition / polyethylene, stretched polypropylene / polyvinyl alcohol / polyethylene, polyvinylidene chloride coated stretched nylon / polyethylene, and nylon-based coextruded multilayer sheets and films with an oxygen permeability of 0.05 to 20 mL / m can be easily used. 2 Bags and packaging containers formed from the laminated body at 24 hr·atm (25°C, 50% RH).

[0134] In addition to the above, as the gas barrier container, a metal can, a glass bottle, a plastic container, etc. can also be used.

[0135] [Method for producing deoxidizer package]

[0136] The method for manufacturing the deoxidizer package is not particularly limited, and preferably includes the following steps (I) to (III). According to this method, a deoxidizer package that can fully exert oxygen absorption performance after operating in the atmosphere for a certain period of time can be obtained. It should be noted that the order of the following steps (II) and (III) is not limited.

[0137] Step (I): a step of obtaining a deoxidizing agent composition (a) containing iron and a metal salt

[0138] Step (II): water is supplied to the deoxidizer composition (a) to obtain a content of water present on the surface of iron per unit surface area of ​​iron, which contains iron, metal salt and water [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)}] more than 2.00g / m 2 And 3.50g / m 2 The following steps of preparing the deoxidizer composition (A)

[0139] Step (III): a step of placing at least one of the oxygen scavenger composition (a) and the oxygen scavenger composition (A) in a gas-permeable packaging container (b1)

[0140] <Steps (I) and (II)>

[0141] Steps (I) and (II) are the same as steps (i) and (ii) in the method for producing the above-mentioned deoxidizer composition.

[0142] <Step (III)>

[0143] The step (III) is a step of housing at least one of the oxygen scavenger composition (a) and the oxygen scavenger composition (A) in a gas-permeable packaging container (b1).

[0144] By providing this step, the oxygen scavenger composition (a) and the oxygen scavenger composition (A) can be stored in a gas-permeable packaging container, and an oxygen scavenger package body that can exhibit sufficient oxygen absorption performance even after being exposed to the atmosphere for a certain period of time can be obtained.

[0145] In addition, as the air-permeable packaging container (b1), the above-mentioned containers can be used.

[0146] The above-mentioned production method preferably further comprises the following step (IV).

[0147] Step (IV): a step of further placing the air-permeable packaging container (b1) containing at least one of the oxygen scavenger composition (a) and the oxygen scavenger composition (A) in a gas barrier container (b2)

[0148] By providing the above step (IV), the aforementioned air-permeable packaging container (b1) containing at least one of the deoxidizer composition (a) and the deoxidizer composition (A) can be further contained in the gas-tight container (b2), and the inflow of oxygen and water vapor into the gas-tight container can be blocked. Therefore, the oxidation of iron can be suppressed, and the moisture content on the surface of iron can be appropriately managed.

[0149] This process is particularly suitable for the case where the deoxidizer composition (A) is stored in the air-permeable packaging container (b1). The deoxidizer composition (A) has already formed a water film, so the deoxidation reaction proceeds slowly in the presence of oxygen. Therefore, from the perspective of maintaining good oxygen absorption performance until use as a deoxidizer, this process is effective.

[0150] It should be noted that when the aforementioned air-permeable packaging container (b1) containing at least one of the deoxidizer composition (a) and the deoxidizer composition (A) is further contained in a gas-barrier container (b2), it is preferred that the interior of the gas-barrier container (b2) is substantially a closed system, and it is more preferred that the system be an oxygen-free reducing atmosphere.

[0151] Specific examples of the above-mentioned production method include the following methods 1 and 2.

[0152] <Method 1>

[0153] As method 1, in the above step (I), it is preferred that the following steps (III-1) and (II-1) are sequentially included.

[0154] Step (III-1): a step of placing the oxygen scavenger composition (a) in the air-permeable packaging container (b1)

[0155] Step (II-1): A step of supplying water to the oxygen scavenger composition (a) through the air-permeable packaging container (b1) to obtain the oxygen scavenger composition (A)

[0156] The step (III-1) corresponds to the above-mentioned step (III), and is a step of placing the oxygen scavenger composition (a) in the air-permeable packaging container (b1).

[0157] The step (II-1) corresponds to the step (II) and is a step of supplying water to the oxygen scavenger composition (a) through the air-permeable packaging container (b1) to obtain the oxygen scavenger composition (A).

[0158] Here, the method of supplying water to the above-mentioned deoxidizer composition (a) through the air-permeable packaging container (b1) is not particularly limited, and for example, a method of contacting a water-containing body (e.g., wetted cotton wool, etc.) from the outside of the air-permeable packaging container (b1) containing the deoxidizer composition (a) to allow the water contained in the water-containing body to pass (permeate) the air-permeable packaging container (b1) and be supplied to the deoxidizer composition (a). By having this step, a water film having a desired thickness can be easily formed in the obtained deoxidizer composition (A).

[0159] This method 1 preferably further comprises the following step (IV-1).

[0160] Step (IV-1): a step of further placing the air-permeable packaging container (b1) containing the oxygen scavenger composition (A) in a gas barrier container (b2)

[0161] Step (IV-1) is a step of further placing the air-permeable packaging container (b1) containing the oxygen scavenger composition (A) in a gas barrier container (b2). The oxygen scavenger composition (A) has excellent oxygen absorption performance and is therefore preferably placed in a gas barrier container until it is used as an oxygen scavenger.

[0162] <Method 2>

[0163] As method 2, in the above step (I), it is preferred that the following steps (III-2), (IV-2), and (II-2) are sequentially included.

[0164] Step (III-2): a step of placing the oxygen scavenger composition (a) and the water supply agent in the air-permeable packaging container (b1)

[0165] Step (IV-2): a step of further placing the air-permeable packaging container (b1) containing the oxygen scavenger composition (a) and the water supply agent in a gas-barrier container (b2)

[0166] Step (II-2): A step of supplying water from the water supply agent to the deoxidizer composition (a) to obtain the deoxidizer composition (A)

[0167] Step (III-2) corresponds to the above step (III) and is a step of placing the deoxidizer composition (a) in a gas-permeable packaging container (b1), but in this case, a water supply agent is placed in the gas-permeable packaging container (b1) together with the deoxidizer composition (a). According to this step, a self-reactive deoxidizer is obtained.

[0168] It should be noted that the water supply agent mentioned above can be used as the water supply agent.

[0169] Step (IV-2) is a step of further storing the air-permeable packaging container (b1) containing the aforementioned deoxidizer composition (a) and the aforementioned water supply agent in a gas-barrier container (b2). By further storing the air-permeable packaging container (b1) containing the aforementioned deoxidizer composition (a) and the aforementioned water supply agent in a gas-barrier container (b2), the air permeability to the outside can be blocked. As a result, water can be effectively supplied to the deoxidizer composition (a) from the water supply agent, and a deoxidizer composition (A) having a water film of a desired thickness can be obtained (corresponding to step (II-2)). In addition, as described above, when water is supplied to iron, the deoxidation reaction proceeds slowly, but the air permeability to the outside is blocked by the gas-barrier container, so that the oxygen absorption performance can be well maintained until it is used as a deoxidizer.

[0170] Although the embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept of the present invention and the claims, and various changes can be made within the scope of protection of the present invention.

[0171] Example

[0172] The present embodiment will be described in detail below using examples and comparative examples, but the present embodiment may be modified as appropriate as long as the effects of the present invention are exhibited. In addition, various measurements in the examples and comparative examples were performed as follows.

[0173] (Specific surface area)

[0174] The specific surface area was measured by using a specific surface area measuring apparatus (“BELSORP mini II” manufactured by Microtrac BEL Corp.) using a constant volume method. The nitrogen adsorption amount was measured under the following conditions, and the specific surface area was calculated according to the BET method.

[0175] Measuring temperature: -196℃

[0176] Pretreatment: 300°C, 3 hours, nitrogen flow

[0177] (Breathability resistance)

[0178] Air permeation resistance was measured by using a Glider densometer (manufactured by Toyo Seiki Seisaku-sho, Ltd.) to measure the time required for 100 mL of air to pass through the air-permeable packaging material.

[0179] (water activity)

[0180] The water activity was measured by placing 1.0 g of the water supply agent in a dedicated culture dish and using a water activity measuring device ("AquaLab TDL 2" manufactured by METER) at 25°C according to the procedure specified in the device.

[0181] (Example 1)

[0182] (1) Calcium chloride anhydrate (CaCl 2 ): 2 g was dissolved in 6 g of water, and the aqueous solution (CaCl 2 Concentration: 25 mass %) was mixed with reduced iron powder (manufactured by Hoganas, with an average particle size of 80 μm (D50 diameter measured by a laser diffraction / scattering particle size distribution measuring device), a specific surface area of ​​0.085 m 2 / g) 100 g, and dried to allow calcium chloride to adhere to the surface of the iron powder, thereby obtaining an iron powder (deoxidizer composition (a)) whose surface was covered with calcium chloride.

[0183] (2) 1.00 g of the deoxidizer composition (a) obtained in the above (1) was filled into a 40 mm × 40 mm bag (air-permeable packaging container (b1)) using an air-permeable laminate film (composition: polyethylene nonwoven fabric (manufactured by UNITIKA LTD., "Eleves") / oil-resistant synthetic paper (manufactured by Awa Paper Industries, Ltd., "ALT"), air permeability resistance: 10 seconds, thickness: 200 μm), and the three sides were sealed to obtain a deoxidizer package (x1).

[0184] (3) The deoxidizer package (x1) obtained in the above (2) and the water-absorbed cotton wool (3.5 g of deoxidizer wool, 5.0 g of water) are introduced into an aluminum three-side sealed bag (made by cutting "700 aluminum bag" manufactured by Sun A Kaken Co., Ltd. into 180 mm×250 mm, a gas-barrier container (b2)), the inside of the bag is replaced with nitrogen in such a way that the oxygen concentration in the bag becomes less than 0.1 volume %, and the bag opening is heat-sealed and sealed to obtain a deoxidizer package (y1).

[0185] (4) The deoxidizer package (y1) obtained in the above (3) was stored at 25°C for 2 days, and water was supplied to the deoxidizer composition (a) from the above water-absorbed absorbent cotton (water-containing body), thereby obtaining a deoxidizer composition (A) containing iron, a metal salt and water, and a deoxidizer package (x2) containing the deoxidizer composition (A) in a breathable packaging container (b1). Then, after the above storage period, the aluminum three-side sealed bag was opened in the atmosphere (24°C, 40% RH), the deoxidizer package (x2) was taken out, and the following deoxidation test was performed to evaluate the oxygen absorption performance.

[0186] (5) It should be noted that the content of water present on the surface of iron in the deoxidizer composition (A) per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)}] is obtained by the following method.

[0187] First, the weight W of the deoxidizer package (x1) immediately after production (before water absorption) is measured in advance. 1 .

[0188] Next, the weight W of the deoxidizer package (x2) obtained by supplying water to the deoxidizer package (x1) is measured. 2 The measurement was performed in the atmosphere (24° C., 40% RH) immediately after the deoxidizer package (x2) was taken out from the aluminum three-side sealed bag.

[0189] In addition, the above-mentioned weights were measured using a precision balance.

[0190] Furthermore, since it was confirmed that there was no condensation water on the outside and inside of the packaging material when the deoxidizer package (x2) was taken out of the aluminum three-side sealed bag, the total amount of moisture calculated by the following formula (1) can be estimated as the amount of water supplied from the absorbent cotton after absorbing water to the iron surface of the deoxidizer composition (a), that is, the content of water present on the iron surface in the deoxidizer composition (A).

[0191] Therefore, the content of water present on the surface of iron per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 The results are shown in Table 1.

[0192] Water content (g) = W 2 -W 1 ···(1)

[0193] (Examples 2 and 3, and Comparative Examples 1 to 6)

[0194] In Examples 2 and 3 and Comparative Examples 1 to 6, except that the type and amount of the metal salt and the storage days were changed as shown in Table 1, deoxidizer compositions (A) and deoxidizer packages (x2) were prepared in the same manner as in Example 1.

[0195] The obtained deoxidizer package (x2) was subjected to the same measurements and the following evaluations as in Example 1. The results are shown in Table 1.

[0196] (Example 4)

[0197] (1) 5.88 g of calcium chloride dihydrate was dissolved in 7.43 g of water, and the aqueous solution was mixed with atomized iron powder (manufactured by Kobe Steel, Ltd., with an average particle size of 100 μm (D50 diameter measured by a laser diffraction / scattering particle size distribution measuring device) and a specific surface area of ​​0.073 m 2 / g) 100 g, and dried to allow calcium chloride to adhere to the surface of the iron powder, thereby obtaining an iron powder (deoxidizer composition (a)) whose surface was covered with calcium chloride.

[0198] (2) Next, 17.5 g of sodium chloride was dissolved in 51.5 g of water and impregnated into 75 g of granular diatomaceous earth (manufactured by Showa Chemical Industry Co., Ltd., average particle size 1000 μm (D50 diameter measured by a laser diffraction / scattering particle size distribution measuring device)) to prepare a water supply agent. The water activity of the obtained water supply agent was 75% RH.

[0199] (3) 1.06 g of the deoxidizer composition (a) obtained in the above (1) and 0.70 g of the water supply agent obtained in the above (2) were filled into a 40 mm × 40 mm bag (air-permeable packaging container (b1)) using an air-permeable laminate film (same as above), and the three sides were sealed to obtain a deoxidizer package (x1).

[0200] (4) The deoxidizer package (x1) obtained in the above (3) is introduced into an aluminum three-side sealed bag (same as above, gas-barrier container (b2)), the inside of the bag is replaced with nitrogen in such a way that the oxygen concentration in the bag becomes less than 0.1 volume %, and the bag opening is heat-sealed and sealed to obtain a deoxidizer package (y1).

[0201] (5) The obtained deoxidizer package (y1) was stored at 25°C for 14 days, and water was supplied from the above water supply agent to the deoxidizer composition (a), thereby obtaining a deoxidizer composition (A) containing iron, a metal salt and water, and a water supply agent, and a deoxidizer package (x2) containing the deoxidizer composition (A) and the water supply agent in a breathable packaging container (b1). Then, after the above storage period, the aluminum three-side sealed bag was opened in the atmosphere (24°C, 40% RH), and the deoxidizer package (x2) was taken out, and the following deoxidation test was performed to evaluate the oxygen absorption performance.

[0202] (6) It should be noted that the content of water present on the surface of iron in the deoxidizer composition (A) per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)}] is calculated using the following method.

[0203] First, 5.88 g of calcium chloride dihydrate was placed in a beaker (container), and the initial weight was quickly measured together with the container using a precision balance. After that, moisture was absorbed at 24°C in an environment of 75% RH, which is consistent with the water activity of the above-mentioned water supply agent, and the weight after moisture absorption was measured together with the container using a precision balance on the 7th and 14th days from the start of moisture absorption. As a result, the weight increased by 17.60 g on both the 7th and 14th days compared with the initial weight, and the increased component was taken as the saturated moisture content of calcium chloride dihydrate.

[0204] Furthermore, since it was confirmed that no condensation water was formed on the outside or inside of the packaging material when the deoxidizer package (x2) was taken out of the aluminum three-side sealed bag, the total amount (19.04 g) of the saturated water content (17.60 g) of the calcium chloride dihydrate and the water content (1.44 g) in the calcium chloride dihydrate was estimated to be the amount of water supplied from the water supply agent to the surface of the iron of the deoxidizer composition (a), that is, the content of water present on the surface of the iron in the deoxidizer composition (A).

[0205] Then, the content of water present on the surface of iron per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 The results are shown in Table 1.

[0206] (Comparative Example 7)

[0207] A deoxidizer composition (A) and a deoxidizer package (x2) were prepared in the same manner as in Example 4 except that the amount of calcium chloride dihydrate was changed to 1.99 g, and the same measurements and the following evaluations as in Example 4 were performed. The results are shown in Table 1.

[0208] It should be noted that the same test as in Example 4(6) was performed under the following conditions.

[0209] 1.99 g of calcium chloride dihydrate was placed in a beaker (container), and the initial weight was quickly measured together with the container using a precision balance. After that, moisture was absorbed at 24°C in a humidity environment of 75% RH, which corresponds to the water activity of the above-mentioned water supply agent, and the weight after moisture absorption was measured together with the container using a precision balance on the 7th and 14th days from the start of moisture absorption. As a result, the weight increased by 6.00 g on both the 7th and 14th days compared with the initial weight, and the increased component was taken as the saturated moisture content of calcium chloride dihydrate.

[0210] Furthermore, since it was confirmed that no condensation water was formed on the outside or inside of the packaging material when the deoxidizer package (x2) was taken out of the aluminum three-side sealed bag, the total amount (6.49 g) of the saturated water content (6.00 g) of the calcium chloride dihydrate and the water content (0.49 g) in the calcium chloride dihydrate was estimated to be the amount of water supplied from the water supply agent to the surface of the iron of the deoxidizer composition (a), that is, the content of water present on the surface of the iron in the deoxidizer composition (A).

[0211] Then, the content of water present on the surface of iron per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 The results are shown in Table 1.

[0212] <Evaluation>

[0213] The following evaluations were performed using the deoxidizer packages (x2) produced in Examples 1 to 4 and Comparative Examples 1 to 7. The results are shown in Table 1.

[0214] (Deoxygenation experiment)

[0215] First, a sampling rubber sheet (25 mm × 25 mm, thickness 2 mm) was adhered to one surface of an aluminum bag (aluminum foil laminated plastic film bag, manufactured by Dai Nippon Printing Co., Ltd., "#01 aluminum bag solid color 85×75", 75 mm × 85 mm, thickness 0.065 mm) to obtain an aluminum bag for measurement.

[0216] Next, the deoxidizer package (x2) was left in the atmosphere (24°C, 40% RH) for 2 hours (2 hours after the aluminum three-side sealed bag was opened and the deoxidizer package (x2) was taken out).

[0217] The deoxidizer package (x2) left for 2 hours and 400 mL of air were placed in the above-mentioned aluminum bag for measurement, and the opening was heat-sealed and sealed. Then, the aluminum bag was quickly placed in a thermostatic chamber at 25°C.

[0218] Thereafter, the oxygen concentration in the aluminum bag was measured every 3 hours for 24 hours, the change in oxygen concentration was plotted, and the estimated time when the oxygen concentration in the aluminum bag became 0.1 volume % or less was taken as the deoxygenation time to evaluate the oxygen absorption performance.

[0219] The measurement was performed by using an oxygen analyzer (ISM-3, MOCON Co.), inserting a measuring needle from the rubber sheet into the aluminum bag, and automatically measuring for 24 hours.

[0220] In this example, those with a deoxygenation time exceeding 24 hours (indicated as ">24" in the table) were judged to have insufficient deoxygenation capacity.

[0221] [Table 1]

[0222] Table 1

[0223]

[0224] ※Value obtained by converting the compounding amount of calcium chloride dihydrate into calcium chloride anhydrate

[0225] The components in Table 1 are shown below.

[0226] ·CaCl 2 :Calcium chloride anhydrate

[0227] ·CaBr 2 :Calcium bromide

[0228] ·NaBr: Sodium bromide

[0229] As shown in Table 1, it was confirmed that the content of water present on the surface of iron per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)}] is more than 2.00g / m 2 And 3.50g / m 2 The deoxidizer compositions within the following ranges can also exhibit sufficient oxygen absorbing performance after being operated in the atmosphere for a certain period of time (Examples 1 to 4).

[0230] On the other hand, it was confirmed that the content of water present on the surface of iron per unit surface area of ​​iron was 2.00 g / m 2 The following deoxidizer compositions have a fast oxygen absorption rate, so they deteriorate after being placed in the atmosphere for 2 hours and cannot exert sufficient oxygen absorption performance (Comparative Examples 1, 3, 5 and 7). In addition, it was confirmed that the content of water present on the surface of iron relative to the per unit surface area of ​​iron exceeded 3.50 g / m 2 The deoxidizer composition was unable to optimize the thickness of the water film even after being left in the atmosphere for 2 hours, and the oxygen absorption rate was slow (Comparative Examples 2, 4 and 6).

Claims

1. A deoxidizer composition comprising: iron, a metal salt and water, The content of water present on the surface of iron per unit surface area of ​​iron [content of water present on the surface of iron (g) / {content of iron (g) × specific surface area of ​​iron (m 2 / g)}] more than 2.00g / m 2 And 3.50g / m 2 the following.

2. The deoxidizer composition according to claim 1, in, At least a portion of the metal salt is present on the surface of the iron. 3 . The deoxidizer composition according to claim 2 , wherein the surface of the iron is covered with a metal salt present on the surface of the iron.

4. The deoxidizer composition according to claim 2 or 3, in, The metal salt present on the surface of the iron is at least one selected from the group consisting of calcium chloride, calcium bromide and sodium bromide.

5. The deoxidizer composition according to any one of claims 2 to 4, in, The content of the metal salt present on the surface of the iron is 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the iron.

6. The deoxidizer composition according to any one of claims 1 to 5, in, The specific surface area of ​​the iron is 0.03m 2 / g or more and 0.20m 2 / g or less.

7. The deoxidizer composition according to any one of claims 1 to 6, in, The average particle size (D50) of the iron is 1 μm or more and 1000 μm or less. 8 . An oxygen scavenger package, comprising: the oxygen scavenger composition according to claim 1 , and an air-permeable packaging container containing the oxygen scavenger composition.

9. A method for producing a deoxidizer package, comprising the following steps (I) to (III): Step (I): a step of obtaining a deoxidizing agent composition (a) containing a metal salt and iron, Step (II): supplying water to the deoxidizer composition (a) to obtain a content of water present on the surface of iron relative to the unit surface area of ​​iron, which contains iron, metal salt and water [content of water present on the surface of iron (g) / {content of iron (g)×specific surface area of ​​iron (m 2 / g)}] more than 2.00g / m 2 And 3.50g / m 2 The following steps of preparing the deoxidizer composition (A): Step (III): a step of placing at least one of the oxygen scavenger composition (a) and the oxygen scavenger composition (A) in a gas-permeable packaging container (b1).

10. The method for producing a deoxidizer package according to claim 9, in, Following the step (I), the following steps (III-1) and (II-1) are sequentially provided: Step (III-1): a step of placing the oxygen scavenger composition (a) in the air-permeable packaging container (b1), Step (II-1): A step of supplying water to the oxygen scavenger composition (a) through the air-permeable packaging container (b1) to obtain the oxygen scavenger composition (A).

11. The method for producing a deoxidizer package according to claim 10, further comprising the following step (IV-1): Step (IV-1): a step of further housing the air-permeable packaging container (b1) housing the oxygen scavenger composition (A) in a gas barrier container (b2).

12. The method for producing a deoxidizer package according to claim 9, in, Following the step (I), the following steps (III-2), (IV-2) and (II-2) are sequentially included. Step (III-2): a step of placing the oxygen scavenger composition (a) and the water supply agent in the air-permeable packaging container (b1), Step (IV-2): a step of further placing the air-permeable packaging container (b1) containing the deoxidizer composition (a) and the water supply agent in a gas barrier container (b2), Step (II-2): a step of supplying water from the water supply agent to the deoxidizer composition (a) to obtain the deoxidizer composition (A).