Steel sheet, member, method for producing same, method for producing hot-rolled steel sheet for cold-rolled steel sheet, and method for producing cold-rolled steel sheet
By controlling the composition and structure of the steel plate, the problem of insufficient crack evaluation in the prior art during the crushing process is solved, and the high strength and excellent collision characteristics of the steel plate are achieved, which is suitable for automobile energy absorption components.
Patent Information
- Application Number
- CN202280092141.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-26
AI Technical Summary
When evaluating the collision characteristics of high-strength steel plates, the prior art cannot effectively evaluate the impact of crack generation and progress on absorption energy during the crushing process, resulting in insufficient evaluation of fracture resistance characteristics.
By controlling the composition and structure of the steel plate, the carbon equivalent is more than 0.18% and less than 0.46%, the ferrite area ratio is 55-90%, and the total area ratio of tempered martensite and bainite is more than 5%. The residual austenite is 2 to 10%, fresh martensite is less than 20%, and the bending recovery process is carried out under the condition of radius of curvature/plate thickness of 4.2 to form a steel plate with excellent collision characteristics.
The tensile strength of the steel plate is 440MPa or more and less than 780MPa, which improves its stable absorption energy and fracture resistance during collisions, and is suitable for use in automotive energy absorption components.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention relates to a steel sheet and a member having high strength and excellent collision characteristics, a method for producing the same, a method for producing a hot-rolled steel sheet for cold-rolled steel sheet, and a method for producing a cold-rolled steel sheet. The steel sheet of the present invention can be preferably used mainly as a steel sheet for automobiles. Background Art
[0002] From the perspective of protecting the global environment, in order to reduce CO2 emissions, it has always been an important issue in the automotive industry to seek lightweighting while maintaining the strength of the automobile body to improve the fuel efficiency of the automobile. In order to seek lightweighting while maintaining the strength of the automobile body, it is effective to make the steel plate thinner by increasing the strength of the steel plate used as the raw material for automobile parts. On the other hand, automobile parts made of steel plates as raw materials are premised on ensuring the safety of the occupants in the event of a collision. Therefore, for high-strength steel plates used as raw materials for automobile parts, in addition to the desired strength, excellent collision characteristics are also required.
[0003] In recent years, the application of high-strength steel plates in automobile bodies has been expanding. From the perspective of collision characteristics, automobile parts are roughly divided into non-deformation components such as pillars and bumpers and energy-absorbing components such as beams. In order to ensure the safety of passengers in the event of a collision while the car is running, necessary collision characteristics are required for each component. In order to suppress large deformation during collision, steel plates with high tensile strength (hereinafter also referred to as TS) are used for non-deformation components. On the other hand, in energy-absorbing components, it is required to stabilize the deformation and stably exert the collision energy absorption capacity when the deformation is complex during collision. At this time, if the component breaks during deformation, the deformation is unstable and the desired collision characteristics cannot be obtained. Therefore, by suppressing the breakage of components during collision and stably exerting high absorption energy, it can help improve collision safety. Based on the above situation, energy-absorbing components need to use high-strength steel plates with excellent collision characteristics and TS of 440MPa or more and less than 780MPa.
[0004] In response to such a demand, for example, Patent Document 1 discloses a technology related to an ultra-high strength steel sheet having excellent formability and impact resistance and having a TS of 1200 MPa or more. In addition, Patent Document 2 discloses a technology related to a high strength steel sheet having a maximum tensile strength of 780 MPa or more and being applicable to a shock absorbing member during a collision.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2012-31462
[0008] Patent Document 2: Japanese Patent Application Publication No. 2015-175061 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, although the collision characteristics are studied in Patent Document 1, the research is conducted on the impact resistance on the premise that no member fracture occurs during collision, and the collision characteristics are not studied from the viewpoint of resistance to member fracture.
[0011] In addition, in Patent Document 2, the hat material is subjected to crack judgment in a dynamic axial crushing test using a drop hammer, and the fracture resistance characteristics of the level with TS exceeding 780MPa are evaluated. However, in the crack judgment after crushing, it is impossible to evaluate the process from crack generation to fracture in the crushing, which is important for the collision characteristics. The reason is that if cracks are generated early in the crushing process, even slight cracks that do not penetrate the thickness of the plate may reduce the absorption energy. In addition, if cracks are generated later in the crushing process, even large cracks that penetrate the thickness of the plate may have little effect on the absorption energy. Therefore, it is considered that it is insufficient to evaluate the fracture resistance characteristics based solely on the crack judgment after crushing.
[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a steel plate and member having a tensile strength (TS) of 440 MPa or more and less than 780 MPa and excellent collision characteristics suitable for use as an energy absorbing member for an automobile, and a method for producing the same.
[0013] Methods used to solve problems
[0014] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found the following.
[0015] The steel sheet has a component composition satisfying a carbon equivalent (CE) of 0.18% or more and less than 0.46%, and a steel structure in which, in terms of area ratio, ferrite is 55-90%, the total of tempered martensite and bainite is 5% or more, retained austenite is 2-10%, fresh martensite is 20% or less, and the total of ferrite, tempered martensite, bainite, retained austenite and fresh martensite is 95% or more, the average crystal grain size of ferrite is 25 μm or less, the coefficient of variation (CV) of the ferrite grain size × carbon equivalent (CE) is 0.25 or less, and when the steel sheet is bent 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2 and then bent back to be flat again, the ratio (NF) of ferrite grains having voids at the interface to all ferrite grains in the L cross section in the region of 0-50 μm from the surface of the steel sheet on the compression-tension deformation side 空隙 / NF) is less than 5%, and the tensile strength is more than 440MPa and less than 780MPa. It can be seen that a steel plate with high strength and excellent collision characteristics can be obtained.
[0016] The present invention has been completed based on such findings, and the gist of the present invention is as follows.
[0017] [1] A steel sheet having a component composition satisfying a carbon equivalent (CE) of 0.18% or more and less than 0.46%, and a steel microstructure in which, by area ratio, ferrite is 55 to 90%, a total of tempered martensite and bainite is 5% or more, retained austenite is 2 to 10%, and fresh martensite is 20% or less, and the total of ferrite, tempered martensite, bainite, retained austenite and fresh martensite is 95% or more,
[0018] The average grain size of ferrite is less than 25 μm.
[0019] The coefficient of variation (CV) of ferrite grain size × carbon equivalent (CE) is less than 0.25,
[0020] When the steel sheet is bent 90° in the rolling (L) direction with the width (C) as the axis under the condition of curvature radius / plate thickness of 4.2 and then bent back to be flat again, the number ratio (NF) of ferrite grains with voids at the interface to the total number of ferrite grains in the L cross section within the region of 0 to 50 μm from the surface of the steel sheet on the compression-tension deformation side is 空隙 / NF) is less than 5%,
[0021] The tensile strength of the steel plate is greater than or equal to 440 MPa and less than 780 MPa.
[0022] [2] The steel sheet according to [1], wherein the chemical composition contains, in mass %, C: 0.02-0.12%, Si: 0.10-2.00%, Mn: 0.5-2.0%, P: 0.100% or less, S: 0.050% or less, Sol.Al: 0.005-0.100% and N: 0.0100% or less, with the balance being Fe and inevitable impurities.
[0023] [3] The steel sheet according to [2], wherein the above-mentioned chemical composition further contains, in terms of mass %, at least one selected from the group consisting of Cr: 1.000% or less, Mo: 0.500% or less, V: 0.500% or less, Ti: 0.500% or less, Nb: 0.500% or less, B: 0.0050% or less, Ni: 1.000% or less, Cu: 1.000% or less, Sb: 1.000% or less, Sn: 1.000% or less, As: 1.000% or less, Ca: 0.0050% or less, W: 0.500% or less, Ta: 0.100% or less, Mg: 0.050% or less, Zr: 0.050% or less, and REM: 0.005% or less.
[0024] [4] The steel sheet according to any one of [1] to [3], wherein the steel sheet has an electrogalvanized layer, a hot-dip galvanized layer, or an alloyed hot-dip galvannealed layer on the surface of the steel sheet.
[0025] [5] A member obtained by subjecting the steel plate according to any one of [1] to [4] to at least one of forming and welding.
[0026] [6] A method for manufacturing a steel plate, comprising:
[0027] A hot rolling process, wherein a steel slab having a carbon equivalent (CE) of not less than 0.18% and less than 0.46% and having the composition described in [2] or [3] is heated to a temperature range of 1100 to 1300°C, hot rolled at a finishing temperature of 800 to 950°C, the cumulative reduction ratio of the finishing rolling is set to 60% or more, the residence time in the temperature range of 750 to 600°C is set to 10 seconds or less during the cooling process from the finishing exit side to coiling, and the coiling is performed at a coiling temperature of 600°C or less;
[0028] A cold rolling step, wherein the hot-rolled steel sheet obtained in the hot rolling step is pickled and cold-rolled at a cumulative reduction ratio of 20% or more;
[0029] An annealing step, wherein the cold-rolled steel sheet obtained in the cold-rolling step is heated to an annealing temperature of 740 to 850° C. and maintained for more than 30 seconds;
[0030] A quenching step, wherein after the annealing step, cooling is performed to a cooling stop temperature of (Ms-250°C) to (Ms-50°C); and
[0031] The tempering step includes heating to a reheating temperature of 300 to 500° C. and maintaining the temperature for 20 seconds or more after the quenching step.
[0032] [7] A method for manufacturing a hot-rolled steel sheet for cold-rolled steel sheet, comprising the following hot rolling process: heating a steel slab having a carbon equivalent (CE) of not less than 0.18% and less than 0.46% and having the composition described in [2] or [3] to a temperature range of 1100 to 1300°C, hot rolling the steel slab under the condition that the temperature at the finish rolling outlet is 800 to 950°C, setting the cumulative reduction rate of the finish rolling to not less than 60%, setting the residence time in the temperature range of 750 to 600°C to not more than 10 seconds during the cooling process from the finish rolling outlet to coiling, and coiling the steel slab at a coiling temperature of not more than 600°C, thereby manufacturing a hot-rolled steel sheet having a structure in which ferrite is not more than 50% and the total of fresh martensite and bainite is not less than 50% in terms of the area ratio of the hot-rolled steel sheet structure.
[0033] [8] A method for producing a cold-rolled steel sheet, comprising the cold rolling step described below: pickling the hot-rolled steel sheet obtained by the production method described in [7] and cold rolling it at a cumulative reduction ratio of 20% or more.
[0034] [9] The method for manufacturing a steel sheet according to [6], further comprising a step of plating the surface of the steel sheet with electrogalvanizing, hot-dip galvanizing or alloyed hot-dip galvannealing after the annealing step and before the quenching step, or after the tempering step.
[0035]
[10] The method for manufacturing a steel sheet according to [9], wherein the plating step after the annealing step and before the quenching step includes a step of maintaining the temperature in the range of 300 to 500° C. for 0 to 300 seconds before plating.
[0036]
[11] A method for manufacturing a member, comprising the step of performing at least one of forming and welding on a steel plate manufactured by the method for manufacturing a steel plate described in [6], [9] or
[10] .
[0037] Effects of the Invention
[0038] According to the present invention, a steel sheet having a tensile strength (TS) of 440 MPa or more and less than 780 MPa and excellent collision characteristics can be obtained. A member obtained by forming, welding, etc. the steel sheet of the present invention can be suitably used as an energy absorbing member used in the automotive field. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a figure for demonstrating the 90 degree bending process (primary bending process) in the bending-orthogonal bending test of an Example.
[0040] Figure 2 It is a figure for demonstrating the orthogonal bending (secondary bending process) in the bending-orthogonal bending test of an Example.
[0041] Figure 3 This is a perspective view showing a test piece subjected to 90° bending (primary bending).
[0042] Figure 4 This is a perspective view showing a test piece subjected to orthogonal bending (secondary bending process).
[0043] Figure 5 This is a front view of a test member produced in order to perform an axial crushing test of an example, in which a hat-shaped member and a steel plate are spot-welded.
[0044] Figure 6 yes Figure 5 A perspective view of the test component shown.
[0045] Figure 7 It is a schematic diagram for explaining the shaft crushing test of the example. DETAILED DESCRIPTION
[0046] The present invention will be described below in detail.
[0047] The steel sheet of the present invention has a component composition satisfying a carbon equivalent (CE) of 0.18% or more and less than 0.46%, and a steel structure in which, in terms of area ratio, ferrite is 55-90%, the total of tempered martensite and bainite is 5% or more, retained austenite is 2-10%, fresh martensite is 20% or less, and the total of ferrite, tempered martensite, bainite, retained austenite and fresh martensite is 95% or more, the average crystal grain size of ferrite is 25 μm or less, the coefficient of variation (CV) of the ferrite grain size×carbon equivalent (CE) is 0.25 or less, and when the steel sheet is bent 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2 and then bent back to be flat again, in an L cross section in a region of 0-50 μm from the surface of the steel sheet on the compression-tension deformation side, the number ratio (NF) of ferrite grains having voids at the interface to all ferrite grains is 空隙 / NF) is less than 5%, and the tensile strength is greater than 440 MPa and less than 780 MPa.
[0048] Carbon equivalent (CE): 0.18% or more and less than 0.46%
[0049] The carbon equivalent CE is obtained by converting the influence of elements other than C into the amount of C as an index of the strength of the steel. By setting the carbon equivalent CE to 0.18% or more and less than 0.46%, the area ratio of each metal structure such as ferrite described later can be controlled within the scope of the present invention, and the tensile strength (440 MPa or more and less than 780 MPa) and collision characteristics of the present invention can be obtained. Preferably, the carbon equivalent CE is 0.20% or more. In addition, the carbon equivalent CE is preferably 0.43% or less.
[0050] The carbon equivalent CE can be calculated by the following formula (1).
[0051] Carbon equivalent CE = [C%] + ([Si%] / 24) + ([Mn%] / 6) + ([Ni%] / 40) + ([Cr%] / 5) + ([Mo%] / 4) + ([V%] / 14) … (1)
[0052] In the above formula, [element symbol %] represents the content (mass %) of each element, and elements not contained are set to 0.
[0053] Ferrite area ratio: 55-90%
[0054] When the area ratio of ferrite exceeds 90%, it is difficult to take into account both the tensile strength (TS) of 440 MPa or more and the collision characteristics. When the area ratio of ferrite is less than 55%, the area ratio of the hard phase sometimes increases, and the formation of voids at the interface of the ferrite during deformation is promoted. Therefore, the area ratio of ferrite is 55 to 90%. The area ratio of ferrite is preferably 60% or more. In addition, the area ratio of ferrite is preferably 85% or less.
[0055] Total area ratio of tempered martensite and bainite: 5% or more
[0056] Tempered martensite improves collision characteristics by suppressing component breakage during collision deformation, and is effective in improving absorbed energy and strength during collision. In addition, it also contributes to high strength, so it is effective in improving collision characteristics and strength in a balanced manner. When the combined area ratio of tempered martensite and bainite is less than 5%, such an effect cannot be fully obtained. Therefore, the combined area ratio is greater than 5%, preferably greater than 7%. In addition, the upper limit of the combined area ratio is not limited, but considering the balance with other tissues and the tensile strength of the present invention (greater than 440MPa and less than 780MPa), the combined area ratio is preferably less than 30%.
[0057] Area ratio of retained austenite: 2-10%
[0058] Retained austenite delays the generation of cracks during collision and is effective in improving collision characteristics. Although the mechanism is not clear, it is considered as follows. During collision deformation, the retained austenite increases the radius of curvature in the bending deformation through work hardening, thereby dispersing the strain of the bent portion. By dispersing the strain, the stress concentration on the void generating portion caused by the primary processing is alleviated, resulting in improved collision characteristics. When the area ratio of retained austenite is less than 2%, such an effect cannot be obtained. Therefore, the area ratio of retained austenite is greater than 2%, preferably greater than 3%. On the other hand, when the area ratio of retained austenite exceeds 10%, the fresh martensite generated by the processing-induced phase transformation sometimes reduces the fracture resistance during collision. Therefore, the area ratio of retained austenite is less than 10%, preferably less than 8%.
[0059] Fresh martensite area ratio: less than 20%
[0060] Fresh martensite is effective for high strength. However, it is easy to generate voids at the grain boundary with the soft phase. When the area ratio of fresh martensite exceeds 20%, the generation of voids at the interface with ferrite is sometimes promoted, which reduces the collision characteristics. Therefore, the area ratio of fresh martensite is 20% or less, preferably 15% or less. The lower limit of the area ratio of fresh martensite can be 0%.
[0061] Total area ratio of ferrite, tempered martensite, bainite, retained austenite and fresh martensite: more than 95%
[0062] When the total area ratio of ferrite, tempered martensite, bainite, retained austenite and fresh martensite is less than 95%, the area ratio of the phases other than the above becomes high, and it is difficult to take into account both strength and collision characteristics. The phases other than the above can be listed as pearlite and cementite, and when these phases increase, they sometimes become the starting point of void generation during collision deformation and reduce the collision characteristics. In addition, when pearlite and cementite increase, the strength is sometimes reduced. When the above total area ratio is more than 95%, no matter what the type and area ratio of the remaining phases are, high strength and collision characteristics can be obtained. The total area ratio is preferably set to more than 97%. The total area ratio can be 100%. The total area ratio of pearlite and cementite as the surplus tissue other than the above is less than 5%. The preferred total area ratio of the surplus tissue is less than 3%.
[0063] The area ratio of each organization is the ratio of the area occupied by each phase in the observation area. The area ratio of each organization is determined as follows. The plate thickness section of the steel plate cut at right angles to the rolling direction is ground, and then corroded with a 3 volume % nitric acid ethanol solution. Three fields of view are taken at a magnification of 1500 times at the 1 / 4 position of the plate thickness using SEM (scanning electron microscope). From the obtained image data, the area ratio of each organization is calculated using Image-Pro manufactured by Media Cybernetics. The average value of the area ratio of the three fields of view is used as the area ratio of each organization of the present invention. In the image data, ferrite can be distinguished as black, bainite can be distinguished as black containing island-shaped residual austenite or gray containing carbides with consistent orientation, tempered martensite can be distinguished as bright gray containing fine carbides with inconsistent orientation, and residual austenite can be distinguished as white. Here, fresh martensite is also white, and fresh martensite and residual austenite are difficult to distinguish using SEM images. Therefore, the area ratio of fresh martensite is obtained by subtracting the area ratio of retained austenite obtained by the method described later from the total area ratio of fresh martensite and retained austenite.
[0064] In the present invention, the X-ray diffraction intensity is measured to find the volume fraction of retained austenite, and this volume fraction is regarded as the area fraction of retained austenite. The volume fraction of retained austenite is found by the ratio of the X-ray diffraction integrated intensity of the (200), (220), and (311) planes of fcc iron to the X-ray diffraction integrated intensity of the (200), (211), and (220) planes of bcc iron at a 1 / 4 plane of the plate thickness.
[0065] Average grain size of ferrite: 25 μm or less
[0066] In the steel sheet of the present invention, high collision characteristics can be obtained by making the average crystal grain size of ferrite less than 25μm. Although the mechanism is not clear, it is considered as follows. For the fracture during collision, which is the cause of the deterioration of collision characteristics, the generation and development of cracks become the starting point. It is believed that cracks are easily generated due to the reduction of work hardening ability and the generation and connection of voids in the high hardness difference area. In addition, in the collision of actual components, the part that is subjected to the primary processing during forming is deformed in a bending recovery manner in a direction orthogonal to the primary processing. At this time, if voids are generated in the high hardness difference area of the primary processing part, stress is concentrated around the voids, promoting the generation and development of cracks, resulting in fracture. The reason for the generation of voids in the high hardness difference area is that the deformation amount of the soft phase becomes larger relative to the hard phase. Therefore, by refining ferrite, the deformation amount can be reduced, the generation and development of voids in the primary processing part and the accompanying component fracture can be suppressed, and high fracture resistance characteristics can be obtained. Therefore, the average crystal grain size of ferrite is less than 25μm, preferably less than 20μm. In addition, the lower limit of the average crystal grain size of ferrite is not particularly specified, but is preferably 3 μm or more.
[0067] Regarding the average grain size of ferrite, a SEM (scanning electron microscope) was used to photograph a 40μm×50μm area of more than 10 fields of view at a magnification of 2000 times at the 1 / 4 thickness position of the plate. From the obtained image data, the equivalent circle diameter was calculated based on the area ratio of each ferrite grain using the above-mentioned Image-Pro, and the averaged result was used to determine the average grain size of ferrite.
[0068] In addition, the standard deviation of the ferrite grain size described later can be calculated from each ferrite grain size obtained using the above-mentioned Image-Pro.
[0069] Coefficient of variation of ferrite grain size (CV) × carbon equivalent (CE): 0.25 or less
[0070] In the steel plate of the present invention, high collision resistance can be obtained by setting CV×CE to less than 0.25. Although the mechanism is not clear, it is considered as follows. The generation and development of voids in the primary processing part, which becomes the starting point of fracture during collision, are promoted due to local stress concentration. In order to suppress the above-mentioned problems, it is considered effective to reduce the deviation of ferrite grain size in steel structure and the softening of hard phase. Therefore, the former index (reducing the deviation of ferrite grain size in steel structure) is set to CV, and the latter index (softening of hard phase) is set to CE, and high fracture resistance can be obtained by setting CV×CE to less than 0.25. Preferably it is less than 0.22.
[0071] The coefficient of variation CV of the ferrite grain size can be obtained by the following formula (2).
[0072]
[0073] The carbon equivalent CE can be calculated by the following formula (1).
[0074] CE=[C%]+([Si%] / 24)+([Mn%] / 6)+([Ni%] / 40)+([Cr%] / 5)+([Mo%] / 4)+([V%] / 14)…(1)
[0075] In the above formula, [element symbol %] represents the content (mass %) of each element, and elements not contained are set to 0.
[0076] It should be noted that by controlling the reduction ratio of the finishing rolling during hot rolling described later, the cooling process from the finishing rolling exit side to coiling, and the coiling temperature, the hot rolled structure is made into a structure mainly composed of fresh martensite and bainite, and the desired ferrite average crystal grain size and CV×CE can be obtained. Regarding the hot rolled structure, if a structure mainly composed of fine fresh martensite and bainite is made, the nucleation sites when ferrite is generated in the annealing process and the cooling process after annealing increase, thereby becoming a structure with uniform and fine ferrite grains dispersed.
[0077] When the steel sheet is bent 90° in the rolling (L) direction with the width (C) as the axis under the condition of curvature radius / plate thickness of 4.2 and then bent back to be flat again, the number ratio (NF) of ferrite grains with voids at the interface to the total number of ferrite grains in the L cross section within the region of 0 to 50 μm from the surface of the steel sheet on the compression-tension deformation side is 空隙 / NF): less than 5%
[0078] In the steel sheet of the present invention, by using NF 空隙 / NF is less than 5%, and high collision characteristics can be obtained (NF refers to the number of all ferrite grains in the L section within the region of 0 to 50 μm from the surface of the steel sheet on the compression-tension deformation side when the steel sheet is bent 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2 and then bent back to be flat again. NF 空隙 It refers to the number of ferrite grains with voids at the interface in the L section within the area of 0 to 50 μm from the surface of the steel plate on the compression-tension deformation side when the steel plate is bent 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2 and then bent back to be flat again.
[0079] Although the mechanism is not clear, it is considered as follows. For the fracture during collision, which is the cause of the degradation of collision characteristics, the generation and development of cracks become the starting point. It is believed that cracks are easily generated due to the reduction of work hardening ability and the generation and connection of voids in the high hardness difference area. In addition, in the collision of actual components, the part that is deformed during forming (primary processing) is subjected to secondary deformation during collision. At this time, the deformation history of the fracture starting point is considered to be the part that is subjected to tensile deformation after compression deformation due to primary processing and secondary deformation. In the compression-tensile deformation part, if voids are generated in the high hardness difference area, stress is concentrated around the voids, promoting the generation and development of cracks, and it is believed that the result leads to fracture. Therefore, by tempering martensite and bainite to reduce the high hardness difference area, and then effectively utilizing the residual austenite as needed, the macro stress concentration of the primary processing part is suppressed during deformation, and the micro stress concentration to the coarse ferrite grains is suppressed by controlling the particle size of ferrite, thereby suppressing the generation and development of voids in the primary processing part and the accompanying component fracture, and high fracture resistance characteristics can be obtained. Therefore, in order to obtain these effects, NF 空隙 / NF is set to 5% or less. Preferably, it is set to 3% or less. NF 空隙 / NF is set to 1% or more which is the industrially achievable lower limit.
[0080] It should be noted that as long as the primary bending processing conditions are met (bending 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2), the processing method is not limited. Examples of primary bending processing methods include bending using a V-block method, bending using deep drawing, etc. In the bending recovery processing, stamping using a flat fixture, etc. can be cited.
[0081] NF 空隙 / NF is determined as follows. For the steel plate, a 90° bending process is performed in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2. After the bending recovery process is performed until it is flat again, the plate thickness section is ground, and the L section in the area of 0 to 50 μm from the surface of the steel plate on the compression-tension side is observed. The L section is photographed in three fields of view at a magnification of 2000 times using an SEM (scanning electron microscope). From the obtained image data, the number of all ferrite grains in the field of view and the number of ferrite grains with voids at the interface are counted using Image-Pro manufactured by MediaCybernetics to calculate the ratio. The average value of the three fields of view is taken as the NF 空隙 / NF. It should be noted that the voids are a darker black color than ferrite and can be clearly distinguished from each structure.
[0082] In the present invention, the 90° bending process along the rolling (L) direction with the width (C) direction as the axis means that the bending process along the width (C) direction (refer to Figure 1 When observing the steel plate (width direction steel plate view (width direction vertical cross-sectional view)), the distance between the two ends is shortened along the width direction and the rolling direction (reference Figure 1 Bending by pressing is performed from one side of the surface of the steel plate in a direction perpendicular to the symbols D1 and D2), and the angle formed by the flat portions of both end portions that are not subjected to the bending process reaches 90°.
[0083] The steel sheet surface on the compression-tension side refers to the steel sheet surface on the side subjected to the pressing (the steel sheet surface on the side in contact with a pressing portion such as a punch for performing the pressing).
[0084] The L-section after the bending recovery process is a cross section formed by cutting the steel sheet in parallel with the direction of deformation caused by the bending process and perpendicularly to the surface of the steel sheet, and is a cross section perpendicular to the width direction.
[0085] The measurement position of the ferrite grains after the bending recovery process is set to include the ferrite grains formed by the bending process and in the width (C) direction (refer to Figure 1 More specifically, the number of ferrite grains is measured in the region of 0 to 50 μm in the plate thickness direction in the region that becomes the lowest region in the direction perpendicular to the width direction and the rolling direction (the pressing direction of the pressing part such as a punch) by bending.
[0086] The steel sheet of the present invention may have an electrogalvanized layer, a hot-dip galvanized layer, or an alloyed hot-dip galvanized layer on the surface of the steel sheet.
[0087] The tensile strength (TS) of the steel plate of the present invention is 440 MPa or more and less than 780 MPa. The high strength described in the present invention means that the tensile strength (TS) is 440 MPa or more. From the perspective of collision characteristics and coordination with formability, the upper limit of the tensile strength (TS) is less than 780 MPa. It should be noted that, regarding the method for measuring the tensile strength (TS), a JIS No. 5 tensile test piece (JIS Z2201) is cut from the steel plate in a direction perpendicular to the rolling direction, and a strain rate of 10 -3 The tensile strength (TS) was determined by a tensile test in accordance with JIS Z2241 (2011).
[0088] From the viewpoint of effectively obtaining the effects of the present invention, the thickness of the steel sheet of the present invention is preferably 0.2 mm or more. From the viewpoint of effectively obtaining the effects of the present invention, the thickness of the steel sheet of the present invention is preferably 3.2 mm or less.
[0089] The steel sheet of the present invention has excellent collision characteristics. The excellent collision characteristics mentioned in the present invention refer to good fracture resistance and good energy absorption. The good fracture resistance mentioned in the present invention refers to the average value of the stroke ΔS when the load is reduced by 50% from the maximum load when the bending-orthogonal bending test described below is carried out. 50 The collision characteristics described in the present invention are good, which means that the average value F of the area within the stroke range of 0 to 100 mm in the stroke-load curve diagram of the shaft crushing test described in the embodiment is ave More than 32000N.
[0090] The above-mentioned bending-orthogonal bending test is performed as follows.
[0091] First, the steel plate was bent 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2, and then subjected to a bending recovery process (primary bending process) until it was flat again to prepare a test piece. In the 90° bending process (primary bending process), if Figure 1 As shown in FIG. 1 , a punch B1 is pressed into a steel plate placed on a die A1 having a V-shaped groove to obtain a test piece T1. Figure 2 As shown, the test piece T1 placed on the support roll A2 is subjected to orthogonal bending (secondary bending) by pressing a punch B2 in such a way that the bending direction is perpendicular to the rolling direction. Figure 1 and Figure 2 , D1 represents the width (C) direction, and D2 represents the rolling (L) direction.
[0092] Figure 3 , a test piece T1 is shown in which a 90° bending process (single bending process) is performed on a steel plate. Figure 4 2 shows a test piece T2 obtained by subjecting the test piece T1 to orthogonal bending (secondary bending processing). Figure 4 The position indicated by the dotted line in the test piece T2 corresponds to the position before orthogonal bending. Figure 3 The position of the test piece T1 is shown by the dotted line.
[0093] The conditions for orthogonal bending are as follows.
[0094] [Orthogonal bending condition]
[0095] Test method: Roller support, punch press
[0096] Roller diameter: φ30mm
[0097] Punch tip R: 0.4mm
[0098] Distance between rollers: (plate thickness × 2) + 1.5 mm
[0099] Stroke speed: 20mm / min
[0100] Test piece size: 60mm×60mm
[0101] Bending direction: rolling right angle direction
[0102] In the stroke-load curve obtained when performing the above-mentioned orthogonal bending, the stroke at the point where the load is reduced by 50% from the maximum load is calculated. The average value of the stroke at the point where the load is reduced by 50% from the maximum load when performing the above-mentioned bending-orthogonal bending test three times is taken as ΔS 50 .
[0103] In addition, the above-mentioned shaft crushing test was performed as follows.
[0104] First, in the shaft crushing test, considering the influence of plate thickness, all tests were conducted on steel plates with a thickness of 1.2 mm. The steel plates were cut out and formed (bent) to a depth of 40 mm using a die with a punch shoulder radius of 5.0 mm and a die shoulder radius of 5.0 mm. Figure 5 and Figure 6 The hat-shaped member 10 shown in FIG. 1 is also shown. In addition, the steel plate used as the raw material of the hat-shaped member is cut into a size of 200 mm × 80 mm. Next, the cut steel plate 20 and the hat-shaped member 10 are spot welded to produce a Figure 5 and Figure 6 The test component 30 is shown. Figure 5 It is a front view of a test member 30 produced by spot welding a hat-shaped member 10 and a steel plate 20 . Figure 6 30 is a perspective view of the test component 30. Regarding the position of the spot welding portion 40, as shown in FIG. Figure 6 As shown in FIG. 1 , the distance between the end of the steel plate and the weld is 10 mm, and the distance between the welds is 45 mm. Figure 7 As shown in FIG. 1 , the test member 30 and the bottom plate 50 are joined by TIG welding to produce a shaft crush test sample. Next, the impactor 60 is made to collide with the produced shaft crush test sample at a collision speed of 10 m / s, and the shaft crush test sample is crushed by 100 mm. Figure 7 As shown in FIG. 1 , the crushing direction D3 is set to be parallel to the longitudinal direction of the test member 30. The area in the stroke range of 0 to 100 mm in the stroke-load curve during crushing is calculated, and the average value of the area when the test is performed three times is taken as the absorbed energy (F ave ).
[0105] Next, the preferred range of the chemical composition of the steel sheet will be described. It should be noted that, unless otherwise specified, "%" indicating the content of a component element means "mass %".
[0106] C: 0.02~0.12%
[0107] C is an element required for improving strength because it easily generates phases other than ferrite and forms alloy compounds with Nb, Ti, etc. When the C content is less than 0.02%, even if the manufacturing conditions are optimized, the desired strength cannot be ensured sometimes. Therefore, the C content is preferably 0.02% or more, more preferably 0.03% or more. On the other hand, when the C content exceeds 0.12%, the strength of martensite increases excessively, and even if the manufacturing conditions are optimized, the collision characteristics of the present invention cannot be obtained sometimes. Therefore, the C content is preferably 0.12% or less, more preferably 0.10% or less.
[0108] Si: 0.10~2.00%
[0109] Si is a ferrite-forming element and also a solid solution strengthening element. Therefore, it helps to improve the balance between strength and ductility. In order to obtain this effect, the Si content is preferably 0.10% or more, more preferably 0.20% or more. On the other hand, when the Si content exceeds 2.00%, it sometimes causes the adhesion of the galvanized layer, the decrease of the adhesion and the deterioration of the surface properties. Therefore, the Si content is preferably 2.00% or less, more preferably 1.50% or less.
[0110] Mn: 0.5~2.0%
[0111] Mn is a martensite generating element and also a solid solution strengthening element. In addition, it contributes to the stabilization of retained austenite. In order to obtain these effects, the Mn content is preferably 0.5% or more. The Mn content is more preferably 1.0% or more. On the other hand, when the Mn content exceeds 2.0%, the retained austenite fraction sometimes increases and the collision characteristics decrease. Therefore, the Mn content is preferably 2.0% or less, more preferably 1.8% or less.
[0112] P: 0.100% or less
[0113] P is an element effective for strengthening steel. However, when the P content exceeds 0.100%, the alloying speed is sometimes greatly delayed. In addition, when P is contained in excess of 0.100%, embrittlement is caused due to grain boundary segregation, and even if the steel structure of the present invention is satisfied, the fracture resistance during collision is sometimes deteriorated. Therefore, the P content is 0.100% or less, preferably 0.050% or less. There is no particular lower limit for the P content, and the lower limit that can be implemented industrially at present is about 0.002%, preferably 0.002% or more.
[0114] S: 0.050% or less
[0115] S forms inclusions such as MnS, which cause cracks along the metal flow of the weld, and even if the steel structure of the present invention is satisfied, the collision characteristics may be reduced. Therefore, the amount of S is preferably as low as possible, and from the perspective of manufacturing cost, the S content is preferably 0.050% or less. The S content is more preferably 0.010% or less. There is no particular lower limit for the S content, and the lower limit that can be implemented industrially at present is about 0.0002%, preferably 0.0002% or more.
[0116] Sol.Al: 0.005~0.100%
[0117] Al acts as a deoxidizer and is also a solid solution strengthening element. When the Sol.Al content is less than 0.005%, these effects may not be obtained, and even if the steel structure of the present invention is satisfied, the strength may be reduced. Therefore, the Sol.Al content is preferably 0.005% or more. On the other hand, when the Sol.Al content exceeds 0.100%, the quality of the steel billet during steelmaking is deteriorated. Therefore, the Sol.Al content is preferably 0.100% or less, and more preferably 0.04% or less.
[0118] N: 0.0100% or less
[0119] N forms coarse inclusions of nitrides and carbonitrides such as TiN, (Nb, Ti) (C, N), and AlN in steel, which reduce the collision characteristics, so the content needs to be suppressed. When the N content exceeds 0.0100%, the collision characteristics are easily reduced, so the N content is preferably 0.0100% or less. The N content is more preferably 0.007% or less, and further preferably 0.005% or less. It should be noted that the lower limit of the N content is not particularly limited, and the lower limit that can be implemented in industry is currently about 0.0003%, preferably 0.0003% or more.
[0120] The steel sheet of the present invention has a composition containing the above-mentioned components and the balance of Fe (iron) and inevitable impurities. In particular, the steel sheet of one embodiment of the present invention preferably has a composition containing the above-mentioned components and the balance of Fe and inevitable impurities.
[0121] The steel sheet of the present invention may contain the following components (optional elements) as appropriate depending on desired characteristics.
[0122] At least one selected from the group consisting of Cr: 1.000% or less, Mo: 0.500% or less, V: 0.500% or less, Ti: 0.500% or less, Nb: 0.500% or less, B: 0.0050% or less, Ni: 1.000% or less, Cu: 1.000% or less, Sb: 1.000% or less, Sn: 1.000% or less, As: 1.000% or less, Ca: 0.0050% or less, W: 0.500% or less, Ta: 0.100% or less, Mg: 0.050% or less, Zr: 0.050% or less, and REM: 0.005% or less
[0123] Cr, Mo, and V are elements that improve hardenability and are effective for strengthening steel. However, when excessive amounts of Cr: 1.000%, Mo: 0.500%, and V: 0.500% are contained, the above effects are saturated and the cost of raw materials increases. In addition, the second phase fraction becomes too large, which sometimes deteriorates the fracture resistance during collision. Therefore, in the case of containing any one of Cr, Mo, and V, the Cr content is preferably less than 1.000%, the Mo content is preferably less than 0.500%, and the V content is preferably less than 0.500%. More preferably, the Cr content is less than 0.800%, the Mo content is less than 0.400%, and the V content is less than 0.400%. Even if the content of Cr, Mo, and V is small, the effect of the present invention can be obtained, so the lower limit of each content is not particularly limited. In order to more effectively obtain the effect of hardenability, the content of Cr, Mo, and V is preferably more than 0.005%.
[0124] Ti and Nb are elements effective for precipitation strengthening of steel. However, when the Ti content and the Nb content each exceed 0.500%, the fracture resistance during collision is sometimes deteriorated. Therefore, in the case of containing any one of Ti and Nb, the Ti content and the Nb content are each preferably below 0.500%. More preferably, the Ti content and the Nb content are each below 0.400%. Even if the content of Ti and Nb is small, the effect of the present invention can be obtained, therefore, the lower limit of each content is not particularly limited. In order to more effectively obtain the effect of precipitation strengthening of steel, the Ti content and the Nb content are each preferably above 0.005%.
[0125] B contributes to the improvement of hardenability by suppressing the generation and growth of ferrite from austenite grain boundary, so it can be added as required. But when B content exceeds 0.0050%, the fracture resistance during collision is sometimes deteriorated. Therefore, when containing B, B content is preferably below 0.0050%. More preferably, B content is below 0.0040%. Even if B content is few, the effect of the present invention can be obtained, therefore, the lower limit of B content is not particularly limited. In order to more effectively obtain the effect of the improvement of hardenability, preferably B content is set to more than 0.0003%.
[0126] Ni and Cu are elements effective for strengthening steel. However, when Ni and Cu each exceed 1.000%, the fracture resistance during collision is sometimes deteriorated. Therefore, in the case of containing any one of Ni and Cu, the content of Ni and Cu is preferably less than 1.000%. More preferably, the Ni content and the Cu content are each less than 0.800%. Even if the content of Ni and Cu is small, the effect of the present invention can be obtained, so the lower limit of each content is not particularly limited. In order to more effectively obtain the effect of strengthening steel, the Ni content and the Cu content are each preferably more than 0.005%.
[0127] From the viewpoint of inhibiting nitridation and oxidation on the surface of the steel plate and decarburization in the area near the surface of the steel plate, Sb and Sn can be added as needed. By inhibiting such nitridation and oxidation, it has the effect of preventing the amount of martensite generated on the surface of the steel plate from decreasing and improving the collision characteristics. However, when Sb and Sn each exceed 1.000%, the collision characteristics are sometimes reduced due to grain boundary embrittlement. Therefore, in the case of containing any one of Sb and Sn, the Sb content and the Sn content are each preferably less than 1.000%. More preferably, the Sb content and the Sn content are each less than 0.800%. Even if the content of Sb and Sn is small, the effect of the present invention can be obtained, so the lower limit of each content is not particularly limited. In order to more effectively obtain the effect of improving the collision characteristics, the Sb content and the Sn content are each preferably more than 0.005%.
[0128] As is an element segregating at the grain boundary and is contained as an impurity in the scrap iron as the raw material. From the viewpoint of suppressing grain boundary embrittlement, the As content is preferably 1.000% or less. More preferably, the As content is 0.800% or less. The lower the As content, the more preferable it is. The lower limit of the As content is not particularly limited, but from the viewpoint of refining cost, it is preferably 0.005% or more.
[0129] Ca is an element that is effective in improving workability by controlling the morphology of sulfides. However, when the Ca content exceeds 0.0050%, it is possible to have an adverse effect on the cleanliness of the steel and reduce the characteristics. Therefore, when Ca is contained, the Ca content is preferably set to 0.0050% or less. More preferably, the Ca content is 0.0040% or less. Even if the Ca content is small, the effect of the present invention can be obtained, so the lower limit of the content is not particularly limited. In order to more effectively obtain the effect of improving workability, the Ca content is preferably set to 0.0010% or more.
[0130] W forms fine carbides, nitrides or carbonitrides during hot rolling or annealing, which are useful for precipitation strengthening of steel. When the W content exceeds 0.500%, the workability decreases. Therefore, when W is contained, the W content is set to 0.500% or less. When W is contained, the W content is preferably 0.005% or more, more preferably 0.050% or more. When W is contained, the W content is preferably 0.400% or less, more preferably 0.300% or less.
[0131] Ta forms fine carbides, nitrides or carbonitrides during hot rolling or annealing, which is useful for precipitation strengthening of steel. When the Ta content exceeds 0.100%, the workability decreases. Therefore, when Ta is contained, the Ta content is set to 0.100% or less. When Ta is contained, the Ta content is preferably 0.001% or more, more preferably 0.010% or more. When Ta is contained, the Ta content is preferably 0.08% or less, more preferably 0.060% or less.
[0132] Mg is an element that is effective in improving workability by controlling the morphology of inclusions. On the other hand, when the Mg content exceeds 0.050%, it may have an adverse effect on the cleanliness of the steel. Therefore, when Mg is contained, the Mg content is set to 0.050% or less. When Mg is contained, the Mg content is preferably 0.0005% or more, more preferably 0.001% or more. When Mg is contained, the Mg content is preferably 0.040% or less, more preferably 0.030% or less.
[0133] Zr is an element effective in improving workability by controlling the morphology of inclusions. On the other hand, when the Zr content exceeds 0.050%, it may have an adverse effect on the cleanliness of the steel. Therefore, when Zr is contained, the Zr content is set to 0.050% or less. When Zr is contained, the Zr content is preferably 0.0005% or more, more preferably 0.001% or more. When Zr is contained, the Zr content is preferably 0.040% or less, more preferably 0.030% or less.
[0134] REM is an element that is effective in improving workability by controlling the morphology of sulfides. However, when the content of each REM exceeds 0.005%, it is possible to have an adverse effect on the cleanliness of the steel and reduce the characteristics. Therefore, in the case of containing any one of REM, the content of each REM is preferably set to 0.005% or less. More preferably, the REM content is 0.004% or less. Even if the content of REM is small, the effect of the present invention can be obtained, so the lower limit of each content is not particularly limited. In order to more effectively obtain the effect of improving workability, the content of each REM is preferably set to 0.001% or more.
[0135] It should be noted that the REM described in the present invention refers to the lanthanide elements of scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM concentration in the present invention refers to the total content of one or more elements selected from the above REM.
[0136] The REM is not particularly limited, but preferably scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), neodymium (Nd), dysprosium (Dy), holmium (Ho), and erbium (Er).
[0137] When the above-mentioned optional element is contained in an amount less than the above-mentioned preferred lower limit, the element is contained as an inevitable impurity.
[0138] Hereinafter, one embodiment of the method for manufacturing a steel plate of the present invention will be described in detail. It should be noted that, unless otherwise specified, the temperature when heating or cooling a steel slab (steel raw material), steel plate, etc. shown below refers to the surface temperature of the steel slab (steel raw material), steel plate, etc.
[0139] The method for manufacturing a steel plate of the present invention has, for example, a hot rolling process as described below: a steel slab having the above-mentioned composition is heated to a temperature range of 1100 to 1300° C., a finishing rolling temperature (finishing rolling exit side temperature) is set to 800 to 950° C., a finishing rolling reduction ratio is set to 60% or more, and during the cooling process from the finishing rolling exit side to coiling, a residence time in a temperature range of 750 to 600° C. is set to less than 10 s, and coiling is performed at a coiling temperature of less than 600° C.
[0140] After coiling, the hot-rolled steel sheet may have a structure in which ferrite accounts for 50% or less and the total of fresh martensite and bainite accounts for 50% or more in terms of area ratio.
[0141] In addition, the hot-rolled steel sheet after the hot-rolling step is pickled and cold-rolled at a cumulative reduction ratio of 20% or more.
[0142] In addition, it includes: an annealing process, in which the cold-rolled steel sheet after the above-mentioned cold rolling process is heated to an annealing temperature of 740 to 850°C and maintained for more than 30 seconds; a quenching process, in which, after the annealing process, it is cooled to a cooling stop temperature of (Ms-250°C) to (Ms-50°C); and a tempering process, in which, after the quenching process, it is heated to a reheating temperature of 300 to 500°C and maintained for more than 20 seconds.
[0143] Furthermore, the method for producing a steel sheet of the present invention may include a step of coating the surface of the steel sheet with hot-dip galvanizing or alloyed hot-dip galvannealing before the quenching step or after the tempering step.
[0144] First, the conditions of the hot rolling process will be described.
[0145] Finishing temperature: 800~950℃
[0146] When the finishing temperature (finishing exit temperature) is lower than 800°C, ferrite transformation may occur during rolling, and the hot rolled structure of the present invention may not be obtained. Therefore, the finishing temperature is 800°C or higher, preferably 850°C or higher, and more preferably 880°C or higher. On the other hand, when the finishing temperature exceeds 950°C, the grains may coarsen, and non-uniform ferrite grains may be generated after annealing. Therefore, the finishing temperature is 950°C or lower, preferably 930°C or lower.
[0147] Accumulated reduction rate of finishing rolling: more than 60%
[0148] By making the cumulative reduction rate of the finishing rolling more than 60%, the recrystallization rate during hot rolling increases, and a fine hot rolling structure is formed. In addition, it is believed that by controlling the cooling process and the coiling temperature from the finishing exit side until coiling, the generation of ferrite is suppressed, and by making a fine hot rolling structure of fresh martensite and bainite as the main body, the nucleation sites of ferrite are increased in the annealing process, and uniform and fine ferrite grains can be obtained. When the cumulative reduction rate of the finishing rolling is less than 60%, these effects cannot be obtained. Therefore, the cumulative reduction rate of the finishing rolling is more than 60%, preferably more than 70%. The upper limit is not particularly limited. Considering the balance with the reduction rate during cold rolling, the cumulative reduction rate of the finishing rolling is preferably set to less than 99%, more preferably less than 96%.
[0149] The residence time in the temperature range of 750 to 600°C during the cooling process from the finish rolling exit to coiling: 10 seconds or less
[0150] In the cooling process from the finish rolling exit side to coiling, if the residence time in the temperature range of 750 to 600°C exceeds 10 seconds, ferrite transformation may proceed and the hot rolled structure of the present invention may not be obtained. Therefore, the residence time in the temperature range of 750 to 600°C is 10 seconds or less, preferably 8 seconds or less.
[0151] The lower limit is not particularly limited, but the residence time is preferably set to 1 s or longer, more preferably 3 s or longer, in consideration of production cost.
[0152] Coiling temperature: below 600℃
[0153] When the coiling temperature exceeds 600°C, the ferrite phase transformation sometimes proceeds after coiling, and the hot rolled structure of the present invention cannot be obtained. In addition, the carbides in the hot rolled steel sheet are sometimes coarsened, and such coarsened carbides are not completely melted during the soaking during annealing, and the necessary strength cannot be obtained. Therefore, the coiling temperature is 600°C or less, preferably 580°C or less. The lower limit of the coiling temperature is not particularly limited, but from the viewpoint of not easily causing the shape defects of the steel sheet and preventing the steel sheet from being over-hardened, the coiling temperature is preferably set to 400°C or more.
[0154] Area ratio of ferrite in hot-rolled steel sheet: 50% or less
[0155] In the steel sheet of the present invention, in order to obtain ferrite with an average crystal grain size of less than 25 μm and a CV×CE of less than 0.25 in the final structure, it is important to control the structure of the hot-rolled steel sheet (hot-rolled sheet). It is believed that: in the hot rolling process, the generation of ferrite is suppressed by controlling the reduction rate during finish rolling, the cooling process from the finish rolling exit side to coiling, and the coiling temperature. For the hot-rolled steel sheet structure, by making the area ratio of ferrite less than 50%, the fine hot-rolled structure containing more than 50% of fresh martensite and bainite described later can be obtained. In the annealing process, the nucleation sites of ferrite are increased, and uniform and fine ferrite grains can be obtained. Therefore, the area ratio of ferrite in the hot-rolled steel sheet is less than 50%, preferably less than 40%.
[0156] Total area ratio of fresh martensite and bainite of hot-rolled steel sheet: 50% or more
[0157] In the present invention, for the same reasons as above, in order to obtain ferrite with an average crystal grain size of 25 μm or less and a CV×CE of 0.25 or less in the final structure, it is important to control the structure of the hot-rolled steel sheet to a structure mainly composed of fresh martensite and bainite. Therefore, the total area ratio of fresh martensite and bainite in the hot-rolled steel sheet is 50% or more, preferably 60% or more.
[0158] It should be noted that as long as the area ratio of ferrite in the hot-rolled steel sheet (hot-rolled sheet) is less than 50% and the total area ratio of fresh martensite and bainite in the hot-rolled sheet is more than 50%, the structure, strength and collision characteristics of the present invention can be obtained regardless of the type and area ratio of the phases other than the above. The phases other than the above can be, for example, pearlite and cementite. When these phases are excessively increased and the total area ratio of fresh martensite and bainite in the hot-rolled steel sheet is less than 50%, sometimes uneven ferrite grains are formed during annealing, which become the starting point of void generation during collision deformation, thereby reducing the collision characteristics. These phases are preferably less than 15% in terms of area ratio.
[0159] The hot-rolled steel sheet obtained by the hot rolling step is subjected to pre-treatment such as pickling and degreasing by a generally known method, and then cold-rolled as necessary. The conditions of the cold rolling step when cold rolling is performed will be described.
[0160] Cumulative reduction rate of cold rolling: more than 20%
[0161] When the cumulative reduction rate of cold rolling is less than 20%, the recrystallization of ferrite is not promoted, unrecrystallized ferrite remains, and the steel structure of the present invention cannot be obtained. Therefore, the cumulative reduction rate of cold rolling is 20% or more, preferably 30% or more.
[0162] Next, the conditions of the annealing step when annealing the cold-rolled steel sheet obtained by the cold rolling step will be described.
[0163] Annealing temperature: 740-850°C, holding time: more than 30 seconds
[0164] When the annealing temperature is lower than 740°C, excessive ferrite is generated and the steel structure of the present invention cannot be obtained. When the annealing temperature exceeds 850°C, austenite sometimes becomes excessive and ferrite is insufficient. Therefore, the annealing temperature is 740 to 850°C. The annealing temperature is preferably 750°C or higher. In addition, the annealing temperature is preferably 840°C or lower, and more preferably 820°C or lower.
[0165] In addition, when the holding time is less than 30 seconds, the formation of austenite is insufficient, excessive ferrite is generated, and the steel structure of the present invention cannot be obtained. Therefore, the holding time is 30 seconds or more, preferably 60 seconds or more. The upper limit of the holding time is not particularly limited, but in order not to impair productivity, the holding time is preferably set to 600 seconds or less.
[0166] After the annealing step, quenching is performed. The conditions of the quenching step are described below.
[0167] Cooling stop temperature: (Ms-250℃)~(Ms-50℃)
[0168] When the cooling stop temperature exceeds (Ms-50°C), the formation of tempered martensite is insufficient, and the steel structure of the present invention cannot be obtained. Therefore, the cooling stop temperature is (Ms-50°C) or less, preferably (Ms-100°C) or less. On the other hand, when it is lower than (Ms-250°C), tempered martensite sometimes becomes excessive, and the formation of retained austenite is insufficient. Therefore, the cooling stop temperature is (Ms-250°C) or more, preferably (Ms-200°C) or more.
[0169] Ms can be calculated by the following formula (3).
[0170] Ms(℃)=539-423×{[C%]×100 / (100-[α area%])}-30×[Mn%]-12×[Cr%]-18×[Ni%]-8×[Mo%] …(3)
[0171] In the above formula, each element symbol represents the content (mass %) of each element, and an element not contained is set to 0.
[0172] In addition, [α area %] is the area ratio of ferrite after annealing. The area ratio of ferrite after annealing is obtained in advance by simulating the heating rate, annealing temperature, and holding time during annealing using a thermal expansion measuring device. [α area %] is treated as the same as the area ratio of ferrite contained in the steel sheet finally obtained after annealing and passing through the quenching process and tempering process of the present invention.
[0173] After the quenching step, tempering is performed. The conditions of the tempering step are described below.
[0174] Tempering temperature (reheating temperature): 300-500°C, holding time: more than 20 seconds
[0175] It is believed that: when the tempering temperature is lower than 300°C, the tempering of martensite is insufficient, and the hardness difference between ferrite and tempered martensite becomes large. As a result, the tempered martensite will not deform following the ferrite during the primary processing, and voids are easily generated at the interface with the ferrite, which reduces the collision characteristics. In addition, sometimes the bainite phase transformation is insufficient, and the steel structure and fracture resistance of the present invention cannot be obtained. Therefore, the tempering temperature (reheating temperature) is above 300°C, preferably above 350°C. On the other hand, when the tempering temperature (reheating temperature) exceeds 500°C, ferrite is excessively generated, and the steel structure of the present invention cannot be obtained. In addition, sometimes the bainite phase transformation is insufficient, and the steel structure and fracture resistance of the present invention cannot be obtained. Therefore, the tempering temperature (reheating temperature) is below 500°C, preferably below 450°C.
[0176] In addition, when the holding time is less than 20 seconds, the tempering of martensite is insufficient, and the fracture resistance of the present invention cannot be obtained. In addition, the bainite transformation is sometimes insufficient, and the steel structure and fracture resistance of the present invention cannot be obtained. Therefore, the holding time is 20 seconds or more, preferably 30 seconds or more. The upper limit of the holding time is not particularly limited, but from the viewpoint of productivity and suppression of excessive bainite transformation, the holding time is preferably set to 500 seconds or less.
[0177] Next, the conditions of the plating step will be described.
[0178] In the method for producing a steel sheet of the present invention, the surface of the steel sheet may be subjected to electrogalvanizing, hot-dip galvanizing, or alloyed hot-dip galvanizing after the annealing step and before the quenching step, or after the tempering step.
[0179] The plating step after the annealing step and before the quenching step preferably includes a step of maintaining the temperature in the range of 300 to 500° C. for 0 to 300 seconds before plating.
[0180] When the temperature is lower than 300°C, martensitic transformation may occur, and C may be excessively enriched in the untransformed austenite, which may decompose during plating or alloying of the plating layer, thereby reducing the retained austenite. On the other hand, when the temperature exceeds 500°C, ferrite may be generated, and the steel structure of the present invention may not be obtained.
[0181] On the other hand, when the holding time exceeds 300 seconds, the bainite transformation may excessively proceed, and the steel structure and fracture resistance of the present invention may not be obtained.
[0182] Therefore, in the present invention, the plating step after the annealing step and before the quenching step preferably includes a step of maintaining the temperature in the range of 300 to 500° C. for 0 to 300 seconds before plating.
[0183] The electrogalvanizing treatment is preferably performed by passing electricity while immersing the subject in a zinc melt at 50 to 60°C.
[0184] The hot-dip galvanizing treatment is preferably performed by immersing the steel sheet obtained above in a galvanizing bath at a temperature of 440°C to 500°C. Then, the coating adhesion is preferably adjusted by gas wiping or the like. It should be noted that an alloying step of performing an alloying treatment may be performed after the hot-dip galvanizing step. When the zinc coating is alloyed, it is preferably maintained in a temperature range of 450°C to 580°C for 1 second to 180 seconds.
[0185] For the purpose of shape correction, surface roughness adjustment, etc., the steel sheet subjected to hot-dip galvanizing or alloy hot-dip galvanizing can be subjected to surface temper rolling. However, in surface temper rolling, when the surface temper rolling rate exceeds 1.0%, the bendability sometimes deteriorates due to the hardening of the surface layer, so the surface temper rolling rate is preferably set to 1.0% or less. More preferably, it is 0.7% or less. In addition, various coating treatments such as resin and grease coating can also be implemented.
[0186] The conditions of other production methods are not particularly limited, but the production method is preferably carried out under the following conditions.
[0187] In order to prevent macro-segregation, the steel billet is preferably manufactured by a continuous casting method, and can also be manufactured by an ingot casting method or a thin slab casting method. In order to hot-roll the steel billet, the steel billet can be temporarily cooled to room temperature and then reheated for hot rolling. In addition, the steel billet can be loaded into a heating furnace for hot rolling without cooling it to room temperature. In addition, an energy-saving process of hot rolling immediately after a slight heat preservation can also be applied. When heating the steel billet, in order to prevent the increase of the rolling load and dissolve the carbide, it is preferably heated to above 1100°C. In addition, in order to prevent the increase of scale loss, the heating temperature of the steel billet is preferably set to below 1300°C.
[0188] When hot rolling the steel slab, from the viewpoint of preventing troubles during rolling when the heating temperature of the steel slab is lowered, the rough bar after rough rolling may be heated. In addition, the so-called continuous rolling process in which the rough bars are joined together and continuously finished rolling may be applied. In addition, in order to reduce the rolling load and make the shape and material uniform, it is preferred to perform lubrication rolling with a friction coefficient of 0.10 to 0.25 in all or part of the passes of the finishing rolling.
[0189] The scale of the coiled steel sheet can be removed by pickling, etc. After pickling, the steel sheet is cold-rolled, annealed, and galvanized under the above-mentioned conditions.
[0190] Next, the member of the present invention and a method for producing the same will be described.
[0191] The component of the present invention is formed by subjecting the steel plate of the present invention to at least one of forming and welding. In addition, the method for manufacturing the component of the present invention includes the step of subjecting the steel plate manufactured by the method for manufacturing the steel plate of the present invention to at least one of forming and welding.
[0192] The steel sheet of the present invention has high strength and excellent collision characteristics. Therefore, the components obtained using the steel sheet of the present invention also have high strength and excellent collision characteristics, and are less likely to break during collision deformation. Therefore, the components of the present invention can be suitably used as energy absorbing components in automobile parts.
[0193] The forming process can use a general processing method such as a press process without limitation. In addition, the welding can use a general welding method such as spot welding, arc welding, etc. without limitation.
[0194] Example
[0195] The present invention will be specifically described with reference to Examples. The scope of the present invention is not limited to the following Examples.
[0196] [Example 1]
[0197] The steel with the composition shown in Table 1 is melted in a vacuum melting furnace and rolled to form steel billets. The steel billets are heated to 1100-1300°C, and hot rolled, cold rolled, annealed, quenched, and tempered under the conditions shown in Table 2 to produce steel sheets. When the steel sheets are produced under the conditions shown in Table 2, a portion of the steel sheets is plated before the quenching process or after the tempering process. In the hot-dip galvanizing process, the steel sheets are immersed in a plating bath to form a coating with an adhesion amount of 10-100 g / m 2 In addition, in the alloying hot-dip galvanizing, the hot-dip galvanizing layer is formed on the steel sheet and then alloying treatment is performed to form the alloying hot-dip galvanizing layer (GA). It should be noted that the final thickness of each steel sheet is 1.2 mm.
[0198]
[0199]
[0200] After the obtained steel sheet was subjected to skin-pass rolling with a reduction rate of 0.2%, the area ratios of ferrite (F), bainite (B), fresh martensite (FM), tempered martensite (TM) and retained austenite (RA) were determined according to the following method. In addition, the ratio of ferrite grains with voids at the interface to all ferrite grains in the L cross section within the region of 0 to 50 μm from the surface of the steel sheet on the compression-tension deformation side when the steel sheet was bent 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2 and then bent back to be flat again (NF) was determined according to the above method. 空隙 / NF).
[0201] NF 空隙 / NF is determined as follows. The steel plate is bent 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2. After the bending is restored until it is flat again, the plate thickness section is ground and the L section in the area of 0 to 50 μm from the surface of the steel plate on the compression-tension side is observed. The L section is photographed in three fields of view at a magnification of 2000 times using an SEM (scanning electron microscope). From the obtained image data, the number of all ferrite grains in the field of view and the number of ferrite grains with voids at the interface are counted using Image-Pro manufactured by MediaCybernetics to calculate the ratio. The average value of the three fields of view is taken as NF 空隙 / NF. It should be noted that the voids are a darker black than the ferrite and can be clearly distinguished from each structure.
[0202] The measurement position of the ferrite grains after the bending recovery process is set to include the ferrite grains formed by the bending process in the width (C) direction (refer to Figure 1More specifically, in the area that becomes the lowest part in the direction perpendicular to the width direction and the rolling direction (the pressing direction of the pressing part such as a punch) by bending, the number of ferrite grains is measured in the area of 0 to 50 μm in the plate thickness direction.
[0203] The area ratio of each organization is determined as follows. The plate thickness section of the steel plate cut at right angles to the rolling direction is ground, and then corroded with a 3% volume nitric acid ethanol solution. Three fields of view are taken at a magnification of 1500 times at the 1 / 4 position of the plate thickness using SEM (scanning electron microscope). The area ratio of each organization is obtained using Image-Pro manufactured by Media Cybernetics from the obtained image data. The average value of the area ratio of the three fields of view is used as the area ratio of each organization of the present invention. In the image data, ferrite can be distinguished as black, bainite can be distinguished as black containing island-shaped residual austenite or gray containing carbides with consistent orientation, tempered martensite can be distinguished as bright gray containing fine carbides with inconsistent orientation, and residual austenite can be distinguished as white. Here, fresh martensite is also white, and fresh martensite and residual austenite are difficult to distinguish using SEM images. Therefore, the area ratio of fresh martensite is obtained by subtracting the area ratio of retained austenite obtained by the method described later from the total area ratio of fresh martensite and retained austenite.
[0204] It should be noted that, although not shown in Table 3, the residual structure is obtained by subtracting the total area ratio of ferrite (F), tempered martensite (TM), bainite (B), retained austenite (RA) and fresh martensite (FM) from 100%, and it is judged that these residual structures are pearlite and / or cementite.
[0205] The volume fraction of retained austenite is determined by measuring the X-ray diffraction intensity, and this volume fraction is regarded as the area fraction of retained austenite. The volume fraction of retained austenite is determined by the ratio of the X-ray diffraction integrated intensity of the (200), (220), and (311) planes of fcc iron to the X-ray diffraction integrated intensity of the (200), (211), and (220) planes of bcc iron at a 1 / 4 thickness plane.
[0206] In addition, tensile properties and collision properties were determined according to the following test methods. The results are shown in Table 3.
[0207] <Tensile test>
[0208] From each of the obtained steel sheets, a JIS No. 5 tensile test piece (JIS Z2201) was cut out in a direction perpendicular to the rolling direction, and a strain rate of 10 -3The tensile strength (TS) was determined by a tensile test according to JIS Z2241 (2011) of 1.5 s / s. A TS of 440 MPa or more and less than 780 MPa was considered acceptable.
[0209] <Bending-Orthogonal bending test>
[0210] The obtained steel plate was bent 90° in the rolling (L) direction with the width (C) direction as the axis under the condition of a curvature radius / plate thickness of 4.2, and then subjected to a bending recovery process (primary bending process) until it was flat again to prepare a test piece. In the 90° bending process (primary bending process), if Figure 1 As shown in FIG. 1 , a punch B1 is pressed into a steel plate placed on a die A1 having a V-shaped groove to obtain a test piece T1. Figure 2 As shown, the test piece T1 placed on the support roll A2 is subjected to orthogonal bending (secondary bending) by pressing a punch B2 in such a way that the bending direction is perpendicular to the rolling direction. Figure 1 and Figure 2 , D1 represents the width (C) direction, and D2 represents the rolling (L) direction.
[0211] A test piece T1 obtained by bending a steel plate at 90° (primary bending) is shown in FIG. Figure 3 In addition, a test piece T2 obtained by performing orthogonal bending (secondary bending) on the test piece T1 is shown in FIG. Figure 4 middle. Figure 4 The position indicated by the dotted line in the test piece T2 corresponds to the position before orthogonal bending. Figure 3 The position of the test piece T1 is shown by the dotted line.
[0212] The conditions for orthogonal bending are as follows.
[0213] [Orthogonal bending condition]
[0214] Test method: Roller support, punch press
[0215] Roller diameter: φ30mm
[0216] Punch tip R: 0.4mm
[0217] Distance between rollers: (plate thickness × 2) + 1.5 mm
[0218] Stroke speed: 20mm / min
[0219] Test piece size: 60mm×60mm
[0220] Bending direction: rolling right angle direction
[0221] In the stroke-load curve obtained when performing the above-mentioned orthogonal bending, the stroke at the point where the load is reduced by 50% from the maximum load is calculated. The average value of the stroke at the point where the load is reduced by 50% from the maximum load when performing the above-mentioned bending-orthogonal bending test three times is taken as ΔS 50 ΔS 50 When it is 35 mm or more, the fracture resistance is evaluated as good. 50 The load that determines the stroke amount is very important in the evaluation of fracture resistance. In the fracture caused by axial crush deformation, the cracks generated in the primary processing part of the component become larger, penetrating the plate thickness and causing fracture. In the bending-orthogonal bending test, cracks are generated in the test piece near the maximum load. As the cracks grow larger, the cross-sectional area of the bending part decreases and the load decreases. In other words, the ratio of the load reduction from the maximum load indicates the extent to which the crack has increased with deformation. The stroke ΔS at the point where the load is reduced by 50% from the maximum load is measured. 50 If the pressure is 35 mm or more, the fracture can be suppressed even if the actual deformation is considered. 50 When it was 35 mm or more, it was evaluated that the fracture resistance was good.
[0222] <Shaft crush test>
[0223] In the shaft crushing test, considering the influence of plate thickness, all the tests were conducted using steel plates with a thickness of 1.2 mm. The steel plates obtained through the above manufacturing process were cut out and formed (bent) to a depth of 40 mm using a die with a punch shoulder radius of 5.0 mm and a die shoulder radius of 5.0 mm to produce Figure 5 and Figure 6 The hat-shaped member 10 shown in FIG. 1 is a hat-shaped member. In addition, the steel plate used as the raw material of the hat-shaped member is cut into a size of 200 mm×80 mm. Then, the cut steel plate 20 and the hat-shaped member 10 are spot welded to produce a hat-shaped member as shown in FIG. Figure 5 and Figure 6 The test component 30 is shown. Figure 5 It is a front view of a test member 30 produced by spot welding a hat-shaped member 10 and a steel plate 20 . Figure 6 FIG. 4 is a perspective view of the test component 30. As for the position of the spot welding portion 40, Figure 6 As shown in FIG. 1 , the distance between the end of the steel plate and the weld is 10 mm, and the distance between the welds is 45 mm. Figure 7 As shown in FIG. 1 , the test member 30 and the bottom plate 50 are joined by TIG welding to produce a shaft crush test sample. Next, the impactor 60 is made to collide with the produced shaft crush test sample at a collision speed of 10 m / s, and the shaft crush test sample is crushed by 100 mm. Figure 7As shown in FIG. 1 , the crushing direction D3 is set to be parallel to the longitudinal direction of the test member 30. The area in the stroke range of 0 to 100 mm in the stroke-load curve during crushing is obtained, and the average value of the area when the test is performed three times is taken as the absorbed energy (F ave ). ave When it is 32000 N or more, the absorbed energy is evaluated as good. In addition, when both the fracture resistance and the absorbed energy are good, the collision property is evaluated as good.
[0224]
[0225] The steel sheets of the invention examples have a TS of 440 MPa or more and less than 780 MPa, and have excellent collision properties. On the other hand, the steel sheets of the comparative examples have a TS of less than 440 MPa or more than 780 MPa, and have poor collision properties.
[0226] [Example 2]
[0227] The steel plate No. 1 (the present invention example) in Table 3 of Example 1 was formed by stamping to produce the member of the present invention example. Furthermore, the steel plate No. 1 in Table 3 of Example 1 and the steel plate No. 58 (the present invention example) in Table 3 of Example 1 were joined by spot welding to produce the member of the present invention example. It can be confirmed that the member of the present invention example manufactured using the steel plate of the present invention has excellent collision characteristics and high strength, and the member manufactured by forming the steel plate No. 1 (the present invention example) in Table 3 of Example 1 and the member manufactured by spot welding the steel plate No. 1 in Table 3 of Example 1 and the steel plate No. 58 (the present invention example) in Table 3 of Example 1 can be suitable for use in automotive frame parts, etc.
[0228] [Example 3]
[0229] The galvanized steel sheet No. 1 (the present invention example) in Table 3 of Example 1 was formed by stamping to manufacture the member of the present invention example. Furthermore, the galvanized steel sheet No. 1 in Table 3 of Example 1 and the galvanized steel sheet No. 58 (the present invention example) in Table 3 of Example 1 were joined by spot welding to manufacture the member of the present invention example. It can be confirmed that the member of the present invention example manufactured using the steel sheet of the present invention has excellent collision characteristics and high strength, and the member manufactured by forming the steel sheet No. 1 (the present invention example) in Table 3 of Example 1 and the member manufactured by spot welding the steel sheet No. 1 in Table 3 of Example 1 and the steel sheet No. 58 (the present invention example) in Table 3 of Example 1 can be suitable for use in automotive frame parts, etc.
[0230] Explanation of symbols
[0231] 10 Hat-shaped components
[0232] 20 Steel Plate
[0233] 30 Test components
[0234] 40 Spot welding
[0235] 50 Base Plate
[0236] 60 Impactor
[0237] A1 Die
[0238] A2 Support Roller
[0239] B1 Punch
[0240] B2 Punch
[0241] D1 Width (C) direction
[0242] D2 Rolling (L) direction
[0243] D3 crush direction
[0244] T1 test piece
[0245] T2 test piece
[0246] Industrial Applicability
[0247] According to the present invention, a steel sheet having a TS of 440 MPa or more and less than 780 MPa and excellent collision characteristics can be obtained. If a member obtained using the steel sheet of the present invention is used as an automobile component, it can contribute to the weight reduction of the automobile and greatly contribute to the high performance of the automobile body.
Claims
1. A steel sheet having a component composition satisfying a carbon equivalent (CE) of 0.18% or more and less than 0.46%, and a steel structure in which, by area ratio, ferrite is 55-90%, the total of tempered martensite and bainite is 5% or more, retained austenite is 2-10%, fresh martensite is 20% or less, and the total of ferrite, tempered martensite, bainite, retained austenite and fresh martensite is 95% or more, The average grain size of ferrite is less than 25 μm. The coefficient of variation (CV) of ferrite grain size × carbon equivalent (CE) is less than 0.25, When the steel sheet is bent 90° in the rolling (L) direction with the width (C) as the axis under the condition of curvature radius / plate thickness of 4.2 and then bent back to be flat again, the number ratio (NF) of ferrite grains with voids at the interface to the total number of ferrite grains in the L cross section within the region of 0 to 50 μm from the surface of the steel sheet on the compression-tension deformation side is 空隙 / NF) is less than 5%, The tensile strength of the steel plate is greater than or equal to 440 MPa and less than 780 MPa.
2. The steel plate according to claim 1, wherein: The component composition contains, in mass %, C: 0.02-0.12%, Si: 0.10-2.00%, Mn: 0.5-2.0%, P: 0.100% or less, S: 0.050% or less, Sol.Al: 0.005-0.100% and N: 0.0100% or less, and the balance is Fe and inevitable impurities.
3. The steel plate according to claim 2, wherein: The component composition further contains, in mass %, at least one selected from the group consisting of Cr: 1.000% or less, Mo: 0.500% or less, V: 0.500% or less, Ti: 0.500% or less, Nb: 0.500% or less, B: 0.0050% or less, Ni: 1.000% or less, Cu: 1.000% or less, Sb: 1.000% or less, Sn: 1.000% or less, As: 1.000% or less, Ca: 0.0050% or less, W: 0.500% or less, Ta: 0.100% or less, Mg: 0.050% or less, Zr: 0.050% or less, and REM: 0.005% or less.
4. The steel plate according to any one of claims 1 to 3, wherein The surface of the steel plate has an electro-galvanized layer, a hot-dip galvanized layer or an alloyed hot-dip galvanized layer. 5 . A member obtained by subjecting the steel plate according to claim 1 to at least one of forming and welding.
6. A method for manufacturing a steel plate, comprising: A hot rolling process, wherein a steel slab having a carbon equivalent (CE) of 0.18% or more and less than 0.46% and having a composition as claimed in claim 2 or claim 3 is heated to a temperature range of 1100 to 1300° C., hot rolling is performed under the condition that a finishing temperature is 800 to 950° C., the cumulative reduction rate of finishing rolling is set to 60% or more, the residence time in the temperature range of 750 to 600° C. is set to 10 seconds or less in the cooling process from the finishing exit side to coiling, and coiling is performed at a coiling temperature of 600° C. or less; A cold rolling step, wherein the hot-rolled steel sheet obtained in the hot rolling step is pickled and cold-rolled at a cumulative reduction ratio of 20% or more; An annealing step, wherein the cold-rolled steel sheet obtained in the cold-rolling step is heated to an annealing temperature of 740 to 850° C. and maintained for more than 30 seconds; A quenching process, wherein after the annealing process, cooling is performed to a cooling stop temperature of (Ms-250°C) to (Ms-50°C); and The tempering step comprises heating to a reheating temperature of 300 to 500° C. and maintaining the temperature for 20 seconds or more after the quenching step.
7. A method for manufacturing a hot-rolled steel sheet for cold-rolled steel sheet, comprising the hot rolling step as described below: heating a steel slab having a carbon equivalent (CE) of not less than 0.18% and less than 0.46% and having a component composition as described in claim 2 or claim 3 to a temperature range of 1100 to 1300° C., hot rolling is performed under the condition that the finishing rolling temperature is 800 to 950° C., the cumulative reduction rate of the finishing rolling is set to 60% or more, and in the cooling process from the finishing rolling outlet side to coiling, the residence time in the temperature range of 750 to 600° C. is set to 10 seconds or less, and the coiling temperature is set to 600° C. or less for coiling, thereby manufacturing a hot-rolled steel sheet having a structure in which ferrite is not more than 50% and the total of fresh martensite and bainite is not less than 50% in terms of the area ratio of the hot-rolled steel sheet structure.
8. A method for producing a cold-rolled steel sheet, comprising the cold rolling step of pickling the hot-rolled steel sheet obtained by the method for producing a hot-rolled steel sheet for a cold-rolled steel sheet according to claim 7, and cold rolling the hot-rolled steel sheet at a cumulative reduction ratio of 20% or more.
9. The method for manufacturing a steel plate according to claim 6, wherein: The method includes a step of plating the surface of the steel sheet with electrogalvanizing, hot-dip galvanizing or alloyed hot-dip galvannealing after the annealing step and before the quenching step, or after the tempering step.
10. The method for manufacturing a steel plate according to claim 9, wherein: The plating step after the annealing step and before the quenching step includes a step of maintaining the temperature in a range of 300 to 500° C. for 0 to 300 seconds before plating. 11 . A method for manufacturing a member, comprising the step of performing at least one of forming and welding on a steel plate manufactured by the method for manufacturing a steel plate according to claim 6 , claim 9 , or claim 10 .