Steel for high-frequency quenching

By optimizing the composition and microstructure structure of steel for high-frequency quenching, the problem of increasing manufacturing costs of the prior art annealing before cold forging and high-frequency quenching before high-frequency quenching heat treatment steps is solved, and the omission of high-frequency quenching components is achieved. These steps maintain excellent cold forging effect.

CN119032193APending Publication Date: 2024-11-26JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034442.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-24
Filing Date
2023-03-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing high-frequency quenching steels require annealing before cold forging and tempering heat treatment before high-frequency quenching during the manufacturing process, resulting in increased component manufacturing costs and seeking to reduce heat treatment steps when facing price competition and carbon neutrality requirements. demand.

Method used

A high-frequency quenching steel is developed, with a composition composition of C: 0.36 to 0.55 mass %, Si: 0.10 mass % or less, Mn: 0.15 to 0.45 mass % or less, P: 0.050 mass % or less, S: 0.050 mass % or less, Al: 0.010 to 0.090 mass %, Mo: 0.05 to 0.35 mass %, Ti: 0.010 to 0.200 mass %, B: 0.0005 to 0.0100 mass %, and N: 0.0150 mass %, total scores of ferrite structure and pearlite structure The rate is 80% or more, and excellent cold forging properties can be maintained when annealing before cold forging and tempering heat treatment before high-frequency quenching are omitted.

Benefits of technology

In the manufacturing process of high-frequency quenching, annealing before cold forging and tempering heat treatment before high-frequency quenching, the manufacturing cost of components is reduced, while maintaining excellent cold forging and strength after high-frequency quenching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005087086370000091
    Figure BDA0005087086370000091
  • Figure BDA0005087086370000101
    Figure BDA0005087086370000101
  • Figure HDA0005087086380000011
    Figure HDA0005087086380000011
Patent Text Reader

Abstract

Provided is a steel for high-frequency quenching which has excellent cold forgeability and which can omit annealing prior to cold forging and tempering heat treatment prior to high-frequency quenching in a process for producing a high-frequency quenched component. The steel for high-frequency quenching contains, as a component composition, 0.36 to 0.55 mass% of C, 0.10 mass% or less of Si, 0.15 to 0.45 mass% of Mn, 0.050 mass% or less of P, 0.050 mass% or less of S, 0.010 to 0.090 mass% of Al, 0.05 to 0.35 mass% of Mo, 0.010 to 0.200 mass% of Ti, 0.0005 to 0.0100 mass% of B, and 0.0150 mass% or less of N, with the remainder being Fe and impurities, the total fraction of a ferrite structure and a pearlite structure being 80% or more, and the fraction of the ferrite structure being 40% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to steel for high-frequency hardening. Background Art

[0002] Generally, mechanical structural parts used in automobiles and the like are formed by hot forging or cold forging and then cut to adjust to the final shape. In particular, cold forging has excellent dimensional accuracy, so there is an advantage of reducing the amount of cutting after forging. Therefore, in recent years, the application examples of cold forgings have been increasing.

[0003] For example, Japanese Patent No. 5679440 (Patent Document 1) discloses a high-frequency hardening steel having excellent cold forging properties of a spheroidized structure of cementite and excellent torsional strength after high-frequency quenching. In addition, Japanese Patent Publication No. 2020-100896 (Patent Document 2) discloses a high-frequency hardening steel and a high-frequency quenching component that have a predetermined balance of alloy elements and obtain excellent hardness and surface fatigue strength in high-frequency quenching after normalizing.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 5679440

[0007] Patent Document 2: Japanese Patent Application Publication No. 2020-100896 Summary of the invention

[0008] For mechanical structural parts, high-frequency quenching is sometimes performed as the final heat treatment after forming into the shape of the parts. Such parts are mostly subjected to softening annealing before cold forging and tempering heat treatment (quenching and tempering) before high-frequency quenching. In the face of the surge in component price competition in recent years and the improvement of the situation of carbon neutrality (CO2 emission reduction), the demand for steel that can omit heat treatment in the component manufacturing process is increasing.

[0009] In the high-frequency hardening steel disclosed in Patent Document 1, spheroidizing annealing is required before cold forging. In addition, in the high-frequency hardening steel disclosed in Patent Document 2, tempering heat treatment is required before high-frequency hardening. Thus, in the prior art, the increase in component manufacturing cost due to the additional heating treatment cost has become a problem.

[0010] The present disclosure has been made in view of the above-mentioned actual situation, and an object of the present disclosure is to provide a steel for high-frequency hardening having excellent cold forgeability, which can omit annealing before cold forging and tempering heat treatment before high-frequency hardening in the manufacturing process of high-frequency hardening parts.

[0011] The steel for induction hardening of the present invention for achieving the above-mentioned object is as follows.

[0012] (1) A steel for high-frequency hardening, comprising: 0.36 to 0.55 mass % C, 0.10 mass % or less Si, 0.15 to 0.45 mass % Mn, 0.050 mass % or less P, 0.050 mass % or less S, 0.010 to 0.090 mass % Al, 0.05 to 0.35 mass % Mo, 0.010 to 0.200 mass % Ti, 0.0005 to 0.0100 mass % B, and 0.0150 mass % or less N, with the remainder being Fe and impurities, wherein the total fraction of ferrite structure and pearlite structure is 80% or more, and the fraction of ferrite structure is 40% or more.

[0013] (2) The steel for induction hardening according to (1) above, further comprising, as the component composition, one or more selected from the group consisting of 0.65 mass % or less of Cr, 1 mass % or less of Cu, and 1 mass % or less of Ni.

[0014] (3) The steel for high-frequency hardening according to (1) or (2), further comprising, as the above-mentioned component composition, one or more selected from Se: 0.3 mass % or less, Ca: 0.05 mass % or less, Pb: 0.3 mass % or less, Bi: 0.3 mass % or less, Mg: 0.05 mass % or less, Zr: 0.2 mass % or less, REM: 0.01 mass % or less, and O: 0.025 mass % or less.

[0015] (4) The steel for induction hardening according to any one of (1) to (3) above, further comprising, as the component composition, one or more selected from the group consisting of 0.1 mass % or less of Nb and 0.3 mass % or less of V.

[0016] (5) The steel for induction hardening according to any one of (1) to (4) above, further comprising, as the component composition, one or more selected from Sn: 0.1 mass % or less and Sb: 0.1 mass % or less.

[0017] According to the present disclosure, it is possible to provide a steel for induction hardening having excellent cold forgeability, which allows annealing before cold forging and tempering heat treatment before induction hardening to be omitted in the manufacturing process of induction hardened parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a graph showing the pattern of induction hardening.

[0019] Figure 2 It is a graph showing the tempering pattern. DETAILED DESCRIPTION

[0020] The steel for high-frequency hardening according to the embodiment of the present disclosure will be described. First, the outline of the steel for high-frequency hardening according to the present embodiment will be described.

[0021] The high-frequency hardening steel involved in the present embodiment includes, as a component composition, C (carbon): 0.36-0.55 mass%, Si (silicon): 0.10 mass% or less, Mn (manganese): 0.15-0.45 mass%, P (phosphorus): 0.050 mass% or less, S (sulfur): 0.050 mass% or less, Al (aluminum): 0.010-0.090 mass%, Mo (molybdenum): 0.05-0.35 mass%, Ti (titanium): 0.010-0.200 mass%, B (boron): 0.0005-0.0100 mass% and N (nitrogen): 0.0150 mass% or less, and the remainder is Fe (iron) and impurities. In the high-frequency hardening steel of the present embodiment, the total fraction of ferrite structure and pearlite structure is 80% or more, and the fraction of ferrite structure is 40% or more. In the following description, when “a to b” (where a and b are numerical values, a<b) is described, it means “a or more and b or less”.

[0022] The steel for induction hardening of the present embodiment can omit annealing before cold forging and tempering heat treatment before induction hardening in the manufacturing process of induction hardened parts, and has excellent cold forgeability.

[0023] An example of the high-frequency hardening steel of the present embodiment is a high-frequency hardening steel used for machine structural parts in automobiles and the like, and specifically, is a steel bar and a wire rod.

[0024] In the automotive field, as the parts using the high-frequency hardened steel disclosed in the present invention, for example, there can be cited the crankshaft, camshaft, timing gear and diesel common rail of the engine, the transmission shaft, drive shaft and CVJ outer ring of the drive system, the wheel hub, steering pinion, worm and ball joint of the chassis, the rotor shaft and motor shaft of the electrical components, etc. In the field of industrial machinery, as the parts using the high-frequency hardened steel disclosed in the present invention, for example, there can be cited the shaft of the ball screw and the track of the linear bearing, etc., and in the field of construction machinery, for example, there can be cited the inner and outer rings of the gear ring and the slewing wheel of the travel reducer, etc.

[0025] Hereinafter, the component composition of the steel for induction hardening according to the present embodiment will be described in detail.

[0026] C: 0.36-0.55 mass%

[0027] In order to ensure the strength of the solidified layer after high-frequency quenching, it is necessary to add at least 0.36 mass% of C. If the addition amount of C exceeds 0.55 mass%, the cold forgeability is reduced, and quenching cracks are likely to occur during high-frequency quenching. In addition, in order to improve the balance between cold forgeability and strength after high-frequency quenching, the addition amount of C is 0.36 mass% or more and 0.55 mass% or less, preferably 0.36 mass% or more and 0.50 mass% or less, and more preferably 0.36 mass% or more and 0.40 mass% or less.

[0028] Si: 0.10 mass % or less

[0029] Si is effective as a deoxidizer and is preferably added in an amount of 0.01% or more. If the amount of Si added exceeds 0.10% by mass, the cold forgeability is reduced. The amount of Si added is 0.10% by mass or less, preferably 0.08% by mass or less, and more preferably 0.07% by mass or less.

[0030] Mn: 0.15-0.45 mass%

[0031] Mn has the effect of improving hardenability. In order to ensure the strength after high-frequency quenching, at least 0.15 mass% needs to be added. If the addition amount of Mn exceeds 0.45 mass%, the cold forgeability decreases. The addition amount of Mn is 0.15 mass% or more and 0.45 mass% or less, preferably 0.20 mass% or more and 0.40 mass% or less, and more preferably 0.20 mass% or more and 0.35 mass% or less.

[0032] P: 0.050 mass% or less

[0033] P reduces the toughness of steel, so it is preferred to reduce its addition amount, but extreme low P leads to increased cost of steelmaking process. From the viewpoint of this cost, the addition amount of P is preferably 0.002 mass % or more. For mechanical structural parts, the addition amount of P is 0.050 mass % or less. The addition amount of P is preferably 0.030 mass % or less, and more preferably 0.015 mass % or less.

[0034] S: 0.050 mass % or less

[0035] S is an element that exists as a sulfide inclusion and is effective in improving machinability. The amount of S added is 0.050 mass% or less. Although the addition of S exceeding 0.050 mass% does not increase the deformation resistance during cold forging, it increases the incidence of cracks. It should be noted that, when it is necessary to improve machinability, S can be added in an amount of 0.005 mass% or more, and the amount of S added is preferably in the range of 0.005 mass% or more and 0.050 mass% or less. The amount of S added is more preferably 0.010 mass% or more and 0.035 mass% or less.

[0036] Al: 0.010 to 0.090 mass%

[0037] Al is an element effective for deoxidation. In addition, it has the effect of refining the crystal grain size by forming fine nitrides by bonding with N. In order to obtain these effects, the amount of Al added is 0.010 mass % or more. On the other hand, even if more than 0.090 mass % of Al is added, the above effects are only saturated. The amount of Al added is 0.010 mass % or more and 0.090 mass % or less, preferably 0.015 mass % or more and 0.050 mass % or less, and more preferably 0.015 mass % or more and 0.035 mass % or less.

[0038] Mo: 0.05-0.35 mass%

[0039] Mo has the effect of improving hardenability. In order to ensure the strength after high-frequency quenching, it is necessary to add at least 0.05 mass%. On the other hand, if the addition amount of Mo exceeds 0.35 mass%, the cold forgeability decreases. The addition amount of Mo is 0.05 mass% or more and 0.35 mass% or less, preferably 0.07 mass% or more and 0.30 mass% or less, and more preferably 0.07 mass% or more and 0.25 mass% or less.

[0040] Ti: 0.010 to 0.200 mass%

[0041] Ti forms nitrides by bonding with N, thereby having the effect of reducing the solid solution N in the steel. In addition, Ti has a strong tendency to form nitrides compared with B, so the nitride formation of B is suppressed, and by increasing the solid solution B, the hardenability of the steel can be improved. In order to obtain this effect, it is necessary to add at least 0.010% by mass of Ti. On the other hand, if more than 0.200% by mass of Ti is added, the nitrides coarsen and become the cause of fatigue failure. The addition amount of Ti is more than 0.010% by mass and less than 0.200% by mass, preferably more than 0.010% by mass and less than 0.050% by mass, and more preferably more than 0.012% by mass and less than 0.035% by mass.

[0042] B: 0.0005 to 0.0100 mass%

[0043] B has the effect of improving the hardenability of steel by being dissolved in steel. Especially compared with Si, Mn, Cr, etc., it is possible to achieve an increase in hardenability without increasing deformation resistance. In order to take into account excellent cold forging and sufficient hardenability, the addition of B is indispensable. In order to obtain this effect, it is necessary to add at least 0.0005% by mass of B. On the other hand, when the addition of B exceeds 0.0100% by mass, cracks after continuous casting are likely to occur, causing a reduction in yield. The addition of B is more than 0.0005% by mass and less than 0.0100% by mass, preferably in the range of more than 0.0005% by mass and less than 0.0050% by mass. More preferably, it is more than 0.0010% by mass and less than 0.0035% by mass.

[0044] N: 0.0150 mass % or less

[0045] N combines with Al, Ti, and B to form nitrides. The amount of N added is less than 0.0150 mass %. If the amount of N added exceeds 0.0150 mass %, the generation of BN (boron nitride) becomes significant, and the solid solution B decreases, thereby reducing the hardenability of the steel. In addition, excessive low N causes the cost of the steelmaking process to increase, so the preferred range of the amount of N added is more than 0.0010 mass % and less than 0.0150 mass %. The amount of N added is more preferably more than 0.0015 mass % and less than 0.0080 mass %, and most preferably more than 0.0020 mass % and less than 0.0065 mass %.

[0046] In the steel for high-frequency hardening of the present embodiment, the remainder of the composition is Fe and impurities. In the present embodiment, impurities are substances mixed from ore, scrap or the manufacturing environment as raw materials when steel is manufactured industrially. Impurities are allowed within a range that does not adversely affect the characteristics of the steel for high-frequency hardening of the present embodiment.

[0047] The steel for induction hardening of the present embodiment may further contain the following optional components.

[0048] Cr: 0.65 mass% or less

[0049] Cr (chromium) has the effect of improving hardenability. When it is necessary to improve the strength after high-frequency quenching, it is preferably added at 0.05% by mass or more. However, Cr is enriched in carbides and has a strong effect of increasing the thermal stability of carbides. If it is added in excess of 0.65% by mass, the carbides will not dissolve during the heating of high-frequency quenching, resulting in a decrease in the solid-solution carbon in the steel, and there is a disadvantage of reduced strength after high-frequency quenching. Therefore, as long as the amount of Cr added is within the range of 0.65% by mass or less, it can be appropriately added according to the conditions of high-frequency quenching, but in applications where the aforementioned disadvantages must be stably avoided, the amount of Cr added can be set to less than 0.35% by mass. The amount of Cr added is further preferably less than 0.25% by mass.

[0050] Cu: 1 mass% or less

[0051] Ni: 1 mass% or less

[0052] Cu (copper) and Ni (nickel) have the effect of improving hardenability. When it is necessary to improve the strength after high-frequency quenching, it is preferably added at 0.01 mass % or more. However, if more than 1 mass % of Cu and Ni are added, the cold forgeability decreases. The addition amounts of Cu and Ni are respectively 1 mass % or less, preferably 0.5 mass % or less, and more preferably 0.35 mass % or less.

[0053] Se: 0.3 mass% or less, Ca: 0.05 mass% or less, Pb: 0.3 mass% or less, Bi: 0.3 mass% or less, Mg: 0.05 mass% or less, Zr: 0.2 mass% or less, REM: 0.01 mass% or less, O: 0.025 mass% or less

[0054] Se (selenium), Ca (calcium), Pb (lead), Bi (bismuth), Mg (magnesium), Zr (zinc), REM (rare earth metal) and O (oxygen) all have the effect of improving machinability and can be added within the above range as needed, but even if added beyond the above range, the effect is saturated.

[0055] Nb: 0.1 mass% or less

[0056] V: 0.3 mass % or less

[0057] Nb (niobium) and V (vanadium) form fine carbides by combining with C, which have the effect of precipitation strengthening the steel. In order to obtain this effect, these Nb and V are preferably added at 0.005 mass % or more. The addition amount of Nb can be 0.1 mass % or less. The addition amount of V can be 0.3 mass % or less. The addition of Nb and V exceeding these will reduce the continuous casting property and lead to a reduction in the yield rate.

[0058] Sn: 0.1 mass% or less

[0059] Sb: 0.1 mass% or less

[0060] Sb (antimony) and Sn (tin) have the effect of easily removing oxide scale in descaling treatments such as shot blasting and pickling. In order to obtain this effect, it is preferably added in an amount of 0.003 mass % or more. The amount of Sb and Sn added may be 0.1 mass % or less. However, even if more than 0.1 mass % of Sb and Sn are added, the effect of improving descaling properties is saturated.

[0061] As mentioned above, the components of the present disclosure have been described. However, in order to soften the steel material and improve the cold forgeability, it is also necessary to control the microstructure.

[0062] The ferrite fraction is 40% or more

[0063] In the steel of the present invention, in order to omit annealing before cold forging, the fraction of ferrite structure needs to be 40% or more. If the fraction of ferrite structure is 40% or more, the reduction of deformation resistance becomes significant, and annealing can be omitted. Therefore, the heating temperature in hot rolling can be 1050°C or less. If the heating temperature of hot rolling is lowered, austenite becomes fine, and the nucleation of the subsequent ferrite phase transformation is promoted, thereby increasing the fraction of ferrite.

[0064] The total fraction of ferrite and pearlite is 80% or more

[0065] According to the cooling rate after hot rolling, the microstructure in the steel disclosed in the present invention contains at least ferrite, and may contain any one of pearlite, bainite and martensite. The bainite and martensite produced when the cooling rate is high are relatively hard structures, and therefore are microstructures that increase the hardness of the steel and even the deformation resistance. On the other hand, the ferrite and pearlite produced when the cooling rate is low are relatively soft structures, and therefore are microstructures suitable for reducing the hardness of the steel and even the deformation resistance. Therefore, in the steel disclosed in the present invention, in order to improve the cold forgeability, the combined fraction of the ferrite structure and the pearlite structure is made to be 80% or more. More preferably, it is 90% or more. Of course, it can also be 100%.

[0066] In addition, when it is necessary to promote austenitization during high-frequency heating for the purpose of further thickening the solidified layer, it is preferred that the total fraction of ferrite and pearlite be 90% or more, and the aspect ratio of cementite in pearlite or ferrite be 2 or more. This is because if the aspect ratio of cementite is 2 or more, the dissolution rate of cementite is high, and austenitization can be rapidly generated.

[0067] It should be noted that in order to obtain the desired microstructure, water cooling (including spraying), blast cooling and other cooling promotions are not recommended during cooling after hot rolling. However, if the temperature of the steel material is reduced to below 400°C, there is no problem even if water cooling (including spraying), blast cooling and other cooling promotions are applied. The cooling rate is set to 5.0°C / s or less in the temperature range of 1000 to 400°C after hot rolling. It is preferably 3.0°C / s or less, and the best is 1.0°C / s or less. In addition, any cooling rate can be used below 400°C.

[0068] Example

[0069] The following is a more specific description of the structure and effects of the present disclosure according to the embodiments. In addition, the present disclosure is not limited to the following embodiments, and can be appropriately changed within the scope of the present disclosure, and these are all included in the technical scope of the present disclosure.

[0070] The steel with the composition shown in Table 1 was formed into a round bar with a diameter of 30 mm by hot rolling at the heating temperature shown in Table 2. After air cooling (partially water cooling or air cooling), a cylinder with a diameter of 20 mm and a height of 30 mm was taken from the center of the round bar by machining as a test piece for cold forging. In addition, for steels No. 1 to 41, No. 44 and No. 45, the test pieces for cold forging were cold forged. As the cold forging, an upset forging process with a height reduction rate of 30% was performed. Then, according to Figure 1 and Figure 2 The high-frequency quenching and tempering were carried out in the pattern shown to make high-frequency quenched steel. It should be noted that the microscope test piece for microstructure observation described later was taken from the test piece for cold forging. It should be noted that in Tables 1 and 2, the underlined parts indicate that they are outside the prescribed range of the present disclosure.

[0071] Table 1 (mass %)

[0072]

[0073] Table 2

[0074]

[0075] In addition, for comparison, the steel No. 42 was formed into a round bar with a diameter of 30 mm by hot rolling, air-cooled (partially water-cooled or air-cooled), and then maintained at 760°C for 4 hours for softening annealing by furnace cooling. Then, a cylinder with a diameter of 20 mm and a height of 30 mm was taken from the center of the round bar by machining as a test piece for cold forging. Cold forging and high-frequency quenching and tempering were performed in the same order as in the case of the steels No. 1 to 41, No. 44 and No. 45.

[0076] In addition, for steel No. 43, after cold forging in the same order as No. 42, it was kept at 900°C for 30 minutes and then rapidly cooled, and then kept at 150°C for 30 minutes and then air-cooled for tempering heat treatment (tempering heat treatment before high-frequency quenching and tempering). Then, the steel No. 43 after the tempering heat treatment was subjected to high-frequency quenching and tempering in the same manner as the steels No. 1-41, No. 44 and No. 45.

[0077] Here, the observation of the microstructure was conducted by etching the cross section perpendicular to the cylindrical axis direction of the cold forging test piece with 3% nitric acid solution after mirror polishing. The area ratio of the ferrite structure and the area ratio of the pearlite structure were calculated using the image analysis software Image-Pro PLUS using the image captured by the optical microscope, and the total fraction of these structures was evaluated based on these area ratios.

[0078] In addition, regarding cold forging properties, the load during the upsetting process with the height reduction rate of 30% is measured, and the measured value is converted into a deformation resistance value according to the cold upsetting test method described in the journal "Plasticity and Processing" (Volume 22, No. 241, February 1981) of the Japanese Society of Plastic Processing, page 139, and compared and evaluated. If the deformation resistance value is below 730MPa, annealing can be omitted. Furthermore, for the strength after high-frequency quenching and tempering, for the treated test piece, the Vickers hardness (load 300g) at a depth of 0.1mm from the surface is measured at any 10 points, and their average values ​​are compared and evaluated. The above evaluation results are shown in Table 2.

[0079] Steel No. 40 to No. 44 is equivalent to S38C of the general JIS standard steel. From the results shown in Table 2, it can be seen that the steels disclosed in the present invention (steels of the embodiments, No. 1 to 27) all omit the annealing before cold forging, and also have the same degree of cold forging properties as S38C (No. 42 and No. 43) after annealing. In addition, according to the steel disclosed in the present invention, even if the tempering heat treatment before high-frequency quenching is omitted, it is judged to have the same degree of strength as S38C (No. 43) after the tempering heat treatment. In addition, it can be seen that the alloy composition of the steel is closely related to the annealing before cold forging. Therefore, according to the present disclosure, both the annealing before cold forging and the tempering heat treatment before high-frequency quenching and tempering can be omitted at the same time.

[0080] As described above, it is possible to provide a steel for induction hardening having excellent cold forgeability, in which annealing before cold forging and tempering heat treatment before induction hardening can be omitted in the production process of induction hardened parts.

Claims

1. A steel for high-frequency hardening, comprising, as a component composition, 0.36-0.55 mass % of C, 0.10 mass % or less of Si, 0.15-0.45 mass % of Mn, 0.050 mass % or less of P, 0.050 mass % or less of S, 0.010-0.090 mass % of Al, 0.05-0.35 mass % of Mo, 0.010-0.200 mass % of Ti, 0.0005-0.0100 mass % of B and 0.0150 mass % or less of N, the remainder being Fe and impurities, Furthermore, the total fraction of the ferrite structure and the pearlite structure is 80% or more, and the fraction of the ferrite structure is 40% or more. 2 . The steel for high-frequency hardening according to claim 1 , further comprising, as the component composition, one or more selected from the group consisting of 0.65 mass % or less of Cr, 1 mass % or less of Cu, and 1 mass % or less of Ni.

3. The steel for high-frequency hardening according to claim 1 or 2, further comprising, as the component composition, one or more selected from the group consisting of Se: 0.3 mass % or less, Ca: 0.05 mass % or less, Pb: 0.3 mass % or less, Bi: 0.3 mass % or less, Mg: 0.05 mass % or less, Zr: 0.2 mass % or less, REM: 0.01 mass % or less, and O: 0.025 mass % or less. 4 . The steel for induction hardening according to claim 1 , further comprising, as the component composition, one or more selected from the group consisting of Nb: 0.1 mass % or less and V: 0.3 mass % or less. 5 . The steel for induction hardening according to claim 1 , further comprising, as the component composition, one or more selected from the group consisting of Sn: 0.1 mass % or less and Sb: 0.1 mass % or less.