Rapidly-vulcanized hydrazide-cured perfluorinated elastic composition as well as preparation method and application thereof
By using dihydrazide and magnesium oxide as curing systems in perfluoroelastomers, the vulcanization time is shortened and the mechanical properties are improved, and the problem of excessive vulcanization time of existing perfluoroelastomers is solved, thus achieving suitable for commercial production Rapid vulcanization and excellent mechanical properties.
Patent Information
- Application Number
- CN202411310110.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The vulcanization time of existing perfluoroelastomers is relatively long and it is difficult to meet the economic benefits of commercial production.
The modified perfluoroelastic composition is prepared by regulating the raw material ratio by regulating the ratio of raw materials, and vulcanizing under specific conditions, including preliminary vulcanization at a pressure of 10-25MPa and 160-200°C. The gradient is then warmed up to shorten the vulcanization time.
The vulcanization time is significantly shortened and the mechanical properties of the perfluoroelastic composition are improved, making it suitable for applications such as seals in commercial production in aerospace and petrochemical fields.
Smart Images

Figure BDA0005050394680000011 
Figure BDA0005050394680000041 
Figure FDA0005050394670000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical material processing, and in particular relates to a fast-vulcanized hydrazide-cured perfluoroelastic composition and a preparation method and application thereof. Background Art
[0002] Perfluoroelastomer is a copolymer formed by polymerization of tetrafluoroethylene (TFE), perfluoroalkyl vinyl ether (PAVE, including perfluoromethyl vinyl ether PMVE, perfluoroethyl vinyl ether PEVE, perfluoropropyl vinyl ether PPVE), and a third monomer (curing site monomer CSM), and has excellent high temperature resistance and chemical resistance. Among them, the curing site reacts with one or more curing agents, such as diamine compounds and peroxide compounds, to form a cross-linked polymer, which makes the perfluoroelastomer have more stable and excellent mechanical properties.
[0003] The existing patent US8765876B2 proposes that when hydrazide is used as the curing system of the perfluoroelastomer composition, it can be used for seals of aircraft engines, oil well drilling equipment, and sealing elements of industrial equipment operating at high temperatures. However, this method has the following problems: the vulcanization time in its embodiments is generally long, all above 15 minutes, and such a curing rate is too slow for commercial production seeking economic benefits. Summary of the invention
[0004] In order to overcome the defects of the prior art, the object of the present invention is to provide a fast-vulcanized hydrazide-cured perfluoroelastomer composition and a preparation method and application thereof.
[0005] The invention provides a modified perfluoroelastomer composition, which is prepared from the following raw materials in parts by mass: 100 parts of perfluoroelastomer, 0.05-7 parts of dihydrazide compound and 0.1-3 parts of magnesium oxide.
[0006] Furthermore, it is prepared from the following raw materials in parts by mass: 100 parts of perfluoroelastomer, 0.2-1.5 parts of dihydrazide compound, and 0.1-2 parts of magnesium oxide;
[0007] Preferably, it is prepared from the following raw materials in parts by weight: 100 parts of perfluoroelastomer, 0.5 parts of dihydrazide compound, and 1 part of magnesium oxide.
[0008] Furthermore, the general structural formula of the dihydrazide compound is as shown in Formula I:
[0009]
[0010] Where R is C 1-10 an alkylene group or an aryl group.
[0011] Furthermore, the R is C1-5 an alkylene group or an aryl group.
[0012] Furthermore, the perfluoroelastomer is a copolymerized unit of a nitrile-containing curing site monomer.
[0013] Furthermore, the perfluoroelastomer is perfluoroether rubber;
[0014] The dihydrazide compound is selected from malonic dihydrazide, succinic dihydrazide, adipic dihydrazide, isophthalic dihydrazide, phthalic dihydrazide or terephthalic dihydrazide.
[0015] The present invention also provides a method for preparing the modified perfluoroelastomer composition, which comprises the following steps: plasticizing the perfluoroelastomer, adding dihydrazide compound and magnesium oxide, mixing, rolling, thinning, sheeting, and vulcanizing to obtain the modified perfluoroelastomer.
[0016] Furthermore, the vulcanization conditions are: first vulcanization at a pressure of 10-25 MPa and a temperature of 160-200° C. for 5-40 minutes; then gradient vulcanization at a temperature of 100-300° C. for 0-48 hours.
[0017] Furthermore, the vulcanization conditions are: first vulcanize at a pressure of 16 MPa and a temperature of 170° C. for 10 minutes; then vulcanize at a gradient temperature of 180° C. for 4 hours, 230° C. for 8 hours, and 290° C. for 8 hours.
[0018] The present invention also provides the use of the modified perfluoroelastomer composition in the preparation of aerospace and petrochemical materials.
[0019] The present invention has achieved the following beneficial effects:
[0020] Compared with the hydrazide curing system used in patent US8765876B2, the curing time of the modified perfluoroelastomer composition of the present invention using dihydrazide compound and magnesium oxide as the curing system is significantly shortened. At the same time, the present invention also found that adding magnesium oxide to the hydrazide curing system not only effectively increases its curing rate and promotes crosslinking, but also further improves its mechanical properties.
[0021] The present invention utilizes dihydrazide compounds and magnesium oxide as a curing system. The perfluoroelastomer composition prepared by adjusting the raw material ratio can not only be rapidly vulcanized but also has excellent mechanical properties, is suitable for commercial production, and has broad application prospects in the preparation of seals, gaskets and other products in the fields of aerospace and petrochemicals.
[0022] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.
[0023] The above contents of the present invention are further described in detail below through specific implementation methods in the form of examples. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. DETAILED DESCRIPTION
[0024] The raw materials and equipment used in the present invention are all known products, which are obtained by purchasing commercially available products.
[0025] The perfluoroether rubber used in the examples and comparative examples was purchased from HALOPOLYMER of Russia, model 1000.
[0026] The method for preparing the perfluoroelastomer composition in the embodiments and comparative examples of the present invention is as follows:
[0027] S1. Preparation of rubber compound: firstly, add perfluoroether rubber into a two-roll open mill, fully plasticize at room temperature, then add all other raw materials in the formula, and after uniform mixing, adjust the roller distance to less than 1mm, wrap the rollers, thinly pass the triangle wrap and roll, and finally adjust the roller distance to 2mm to produce a sheet to obtain the rubber compound;
[0028] S2. Vulcanization: Put the mixed rubber into a mold and vulcanize it for 10 minutes at a pressure of 16MPa and a temperature of 170°C. Then carry out a second-stage vulcanization in an oven at a gradient temperature of 180°C for 4h, 230°C for 8h, and 290°C for 8h.
[0029] Normal temperature is (25±5℃).
[0030] Example 1
[0031] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber, 0.5 parts of terephthaloyl hydrazide, and 1 part of magnesium oxide.
[0032] Example 2
[0033] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber, 0.5 parts of isophthalic dihydrazide, and 0.2 parts of magnesium oxide.
[0034] Example 3
[0035] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber, 0.5 parts of adipic acid dihydrazide, and 1.5 parts of magnesium oxide.
[0036] Example 4
[0037] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber, 1.2 parts of malonic acid hydrazide, and 1.8 parts of magnesium oxide.
[0038] The following comparative samples are prepared by comparative examples.
[0039] Comparative Example 1
[0040] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber and 0.5 parts of terephthaloylhydrazide.
[0041] Comparative Example 2
[0042] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber, 0.5 parts of terephthaloyl hydrazide, and 0.2 parts of phthalamide.
[0043] Comparative Example 3
[0044] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber, 0.5 parts of terephthaloyl hydrazide, and 1 part of zinc oxide.
[0045] Comparative Example 4
[0046] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber and 0.5 parts of isophthalic dihydrazide.
[0047] Comparative Example 5
[0048] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber and 0.5 parts of adipic acid dihydrazide.
[0049] Comparative Example 6
[0050] The perfluoroelastic composition was prepared by using the following formula: 100 parts of perfluoroether rubber and 0.5 parts of malonic acid hydrazide.
[0051] The beneficial effects of the present invention are demonstrated by experimental examples below.
[0052] Experimental Example 1
[0053] 1. Experimental methods
[0054] The samples of Examples 1-4 and Comparative Examples 1-6 were subjected to vulcanization tests, test standard: GB / T16584-1996, test conditions: test equipment GT-M3000A, condition MDR
[0055] 185℃@30min, Arc0.5.
[0056] Tensile strength and other properties are tested according to the national standard GB / T 528-2009.
[0057] 2. Experimental results
[0058] The specific experimental results are shown in Tables 1 and 2.
[0059] Table 1 Vulcanization test results of samples
[0060] MH ML TS2 TC90 Example 1 9.69 1.18 1.59 5.22 Example 2 9.74 0.89 1.51 4.55 Example 3 9.21 0.92 1.05 8.12 Example 4 9.92 1.03 0.56 8.45 Comparative Example 1 2.29 0.68 0.00 28.19 Comparative Example 2 9.19 0.61 6.40 16.30 Comparative Example 3 2.71 1.11 0.00 28.11 Comparative Example 4 8.30 0.61 3.49 19:45 Comparative Example 5 7.59 0.72 1.04 26:12 Comparative Example 6 8.01 0.77 0.59 28.07
[0061] ML: Minimum torque, N·m (kgf·cm), indicates the fluidity of the rubber. The lower the ML, the better the fluidity, and vice versa.
[0062] MH: Maximum torque N·m (kgf·cm), which indicates the crosslinking density of the rubber. Generally, the lower the MH, the lower the degree of crosslinking, and the higher the MH, the higher the degree of crosslinking.
[0063] TS2: The time (min) from the start of the experiment to the time when the curve rises from the lowest torque to 0.2N·m (kgf·cm), which represents the operational safety of the rubber. The shorter the TS2, the easier it is for the rubber to die, and the product is more likely to have material shortages during production. On the contrary, the longer the TS2, although the operational safety is improved, the production efficiency will be lower and the cost will increase a lot.
[0064] TC90: The time (min) required for the sample to reach a certain degree of vulcanization. It is mainly used to evaluate the one-time vulcanization conditions of the rubber during molding production. If TC90 is too long, it means that the vulcanization speed is slow and the production efficiency is low.
[0065] Table 2 Mechanical properties test results of samples
[0066]
[0067] Note: Comparative Examples 1 and 3 are basically in an unvulcanized state and cannot be tested for mechanical properties.
[0068] By comparing the vulcanization test results of Examples 1-4 and Comparative Examples 1-6, it can be seen that the addition of magnesium oxide to the hydrazide curing system of Examples 1-4 of the present invention can effectively increase the vulcanization rate, promote crosslinking, and improve the crosslinking density.
[0069] Further comparison of Example 1, Comparative Example 2, and Comparative Example 3 revealed that in Comparative Example 2, the effect of using phthalamide as an accelerator for the hydrazide curing system to promote vulcanization was weak; in Comparative Example 3, the use of zinc oxide, which is also commonly used as an acid absorber, as an accelerator had no vulcanization promoting effect at all; compared with Comparative Examples 2 and 3, the technical solution of using magnesium oxide as an accelerator for the hydrazide curing system in Example 1 of the present invention significantly improved the vulcanization rate.
[0070] Further comparison of the mechanical properties of Examples 1-4 revealed that the tensile strength of the sample obtained in Example 1 of the present invention using perfluoroether rubber, terephthaloyl hydrazide and magnesium oxide as raw materials at a specific ratio was optimal.
[0071] In summary, the present invention provides a fast-vulcanized hydrazide-cured perfluoroelastic composition and its preparation method and application. The present invention uses hydrazide and magnesium oxide as a curing system and prepares a perfluoroelastic composition by adjusting the raw material ratio. The perfluoroelastic composition can not only be vulcanized quickly, but also has excellent mechanical properties, is suitable for commercial production, and has broad application prospects.
Claims
1. A modified perfluoroelastomer composition, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 100 parts of perfluoroelastomer, 0.05 to 7 parts of diacylhydrazine compound and 0.1 to 3 parts of magnesium oxide.
2. The modified perfluoroelastomer composition according to claim 1, It is characterized in that It is prepared from the following raw materials in parts by weight: 100 parts of perfluoroelastomer, 0.2-1.5 parts of diacylhydrazine compound, and 0.1-2 parts of magnesium oxide; Preferably, it is prepared from the following raw materials in parts by weight: 100 parts of perfluoroelastomer, 0.5 parts of dihydrazide compound, and 1 part of magnesium oxide.
3. The modified perfluoroelastomer composition according to claim 1, It is characterized in that The general structural formula of the dihydrazide compound is shown in Formula I: Where R is C 1-10 an alkylene group or an aryl group.
4. The modified perfluoroelastomer composition according to claim 3, It is characterized in that The R is C 1-5 an alkylene group or an aryl group.
5. The modified perfluoroelastomer composition according to any one of claims 1 to 4, It is characterized in that The perfluoroelastomer is a copolymerized unit of a nitrile-containing cure site monomer.
6. The modified perfluoroelastomer composition according to claim 5, It is characterized in that The perfluoroelastomer is perfluoroether rubber; The dihydrazide compound is selected from malonic dihydrazide, succinic dihydrazide, adipic dihydrazide, isophthalic dihydrazide, phthalic dihydrazide or terephthalic dihydrazide.
7. A method for preparing the modified perfluoroelastomer composition according to any one of claims 1 to 6, It is characterized in that The method comprises the following steps: plasticizing the perfluoroelastomer, adding a dihydrazide compound and magnesium oxide, mixing, rolling, thinning, sheeting, and vulcanizing to obtain the product.
8. The method according to claim 7, It is characterized in that The vulcanization conditions are: first vulcanization at a pressure of 10-25 MPa and a temperature of 160-200° C. for 5-40 minutes; then gradient vulcanization at a temperature of 100-300° C. for 0-48 hours.
9. The method according to claim 7, It is characterized in that The vulcanization conditions are: first vulcanize at a pressure of 16 MPa and a temperature of 170° C. for 10 minutes; then vulcanize at a gradient temperature of 180° C. for 4 hours, 230° C. for 8 hours, and 290° C. for 8 hours.
10. Use of the modified perfluoroelastomer composition according to any one of claims 1 to 6 in the preparation of aerospace and petrochemical materials.
Citation Information
Patent Citations
Fluororubber composition capable of effectively reducing cohesiveness with metal and preparation method of fluororubber composition
CN117304625A
Fluoroelastomer compounds
US20210292534A1
Cited By
Perfluoroether rubber resistant to strong alkaline solvent as well as preparation method and application of perfluoroether rubber
CN120464116A
Anti-cracking perfluoroether rubber as well as preparation method and application thereof
CN120464117A