Preparation and catalytic application of molybdenum-based amorphous alloy
By preparing molybdenum-based amorphous alloy, argon protection and single-roll belt swing method were used to prepare molybdenum-based amorphous alloy strips, and the addition of Mo elements was solved, and the problems of unstable structure and small surface area of amorphous alloy were improved. The catalytic activity and stability of oxygen evolution are obtained, and the efficient performance of electrocatalytic decomposition of water is achieved.
Patent Information
- Application Number
- CN202410972624.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-29
AI Technical Summary
In electrolytic hydroxyl alloys, due to structural instability, the catalytic activity of amorphous alloys decreases due to their small surface area, and the electrochemical reaction slow response, which limits their catalytic performance.
Molybdenum-based amorphous alloy, including elemental Ni, Co and Fe, as well as alloys FeB and NiP, is melted under argon protection and made by single-roller belt swing method in an induction furnace, and added Mo elements are used to optimize surface components to form abundant dangling bonds and active sites.
The catalytic activity and stability of oxygen evolution are improved, more active sites and reaction activities are provided, the performance of electrocatalytic decomposition of water is enhanced, and the performance of good mechanical properties can be used as a self-supporting electrode.
Smart Images

Figure CN119040773A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of oxygen evolution catalysis in electrolyzed water, and in particular to a molybdenum-based amorphous alloy and a preparation method thereof. Background Art
[0002] Hydrogen production technology by water electrolysis is regarded as an efficient and sustainable solution to alleviate the depletion of chemical energy. It can convert intermittent renewable energy into chemical energy for fuel production or chemical synthesis, thereby reducing dependence on fossil fuels. However, the oxygen evolution reaction (OER), an important half-reaction of water electrolysis, involves four-electron transfer, resulting in slow reaction kinetics, which is the main obstacle to the large-scale application of water electrolysis technology. In order to improve the efficiency of water electrolysis and achieve widespread commercial application, it is necessary to develop low-cost, stable and efficient OER electrocatalysts. Among the many OER electrocatalysts currently available, amorphous alloys have unique structures and high surface energy. Amorphous alloys, also known as "metallic glasses", not only generally have a wide and continuous range of formation components, but also have excellent physical and chemical properties, such as high strength and hardness, corrosion resistance, high surface catalytic activity, etc. These characteristics make them more advantageous as OER electrocatalysts. However, since amorphous alloys are a new type of material with short-range order and long-range disordered structural characteristics, they are composed of chaotic stacking of ordered atomic clusters and are thermodynamically metastable. During the reaction process, they always transform to their stable state (crystalline state) to varying degrees, resulting in a decrease in catalyst activity or selectivity. In particular, amorphous alloy strips have an independent and stable three-dimensional structure that does not require external support, and their stability is better than that of powder electrocatalysts and array electrocatalysts. However, amorphous strips have problems such as small surface area and slow electrochemical reaction response, which limits their catalytic performance. Therefore, it is necessary to optimize and improve their catalytic activity by designing new components and regulating surface composition. Summary of the invention
[0003] In view of this, the object of the present invention is to provide a molybdenum-based amorphous alloy and a preparation method thereof, which can solve the thermal stability problem of amorphous alloy catalysts and improve the OER catalytic performance and stability.
[0004] The molybdenum-based amorphous alloy of the present invention comprises a raw material of Ni, Co and Fe, and an alloy of FeB and NiP;
[0005] Furthermore, the purity of the elemental Ni, Co and Fe, and the alloys FeB and NiP in the raw materials is not less than 99.9%;
[0006] Furthermore, the chemical formula of the molybdenum-based amorphous alloy is Fe 34-x Co 25 Ni 25 Mo xP8B8, where x = 0, 3, 6, 9, 12;
[0007] Furthermore, the chemical formula of the molybdenum-based amorphous alloy is Fe 25 Co 25 Ni 25 Mo9P8B8;
[0008] Further, the molybdenum-based amorphous alloy is a strip structure;
[0009] Furthermore, the thickness of the molybdenum-based amorphous alloy is no more than 30 μm, and the width is 2-3 mm.
[0010] The method for preparing the molybdenum-based amorphous alloy of the present invention comprises the following steps:
[0011] S1, melting the raw materials under argon protection, and obtaining a master alloy ingot after cooling;
[0012] S2, preparing a molybdenum-based amorphous alloy by a single-roller strip spinning method in an induction furnace from a master alloy ingot;
[0013] Further, in step S1, the smelting temperature is 2400-2800°C;
[0014] Further, in step S2, the tangential speed of the single-roller belt-spinning machine used in the single-roller belt-spinning method is 30-40 m / s;
[0015] Further, in step S2, the tangential speed of the single-roller belt-spinning machine used in the single-roller belt-spinning method is 35 m / s.
[0016] The beneficial effects of the present invention are as follows: the formation of an amorphous phase in the molybdenum-based amorphous alloy of the present invention produces abundant dangling bonds, providing more active sites for the electrocatalytic water decomposition reaction. The addition of the Mo element can promote the surface reconstruction of the amorphous alloy, optimize the surface components of the amorphous alloy, and ultimately improve its catalytic performance. Therefore, the molybdenum-based amorphous alloy is a material with good oxygen evolution catalytic activity and stability, and has good mechanical properties, and can be directly used as a self-supporting electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0018] Figure 1 The Fe 34-x Co 25 Ni 25 Mo x XRD patterns of P8B8 (x = 0, 3, 6, 9, 12);
[0019] Figure 2 Fe obtained by the method of the present invention34-x Co 25 Ni 25 Mo x DTA curves of P8B8 (x=0,3,6,9,12);
[0020] Figure 3 Fe obtained by the method of the present invention 34-x Co 25 Ni 25 Mo x SEM images and EDS spectra of P8B8 (x=0,3,6,9,12);
[0021] Figure 4 The Fe 34-x Co 25 Ni 25 Mo x XPS spectrum of P8B8 (x=0,9);
[0022] Figure 5 The Fe 34-x Co 25 Ni 25 Mo x P8B8 (x=0,3,6,9,12) LSV polarization curves;
[0023] Figure 6 The Fe 34-x Co 25 Ni 25 Mo x P8B8 (x=0,3,6,9,12) Tafel slope;
[0024] Figure 7 The Fe 34-x Co 25 Ni 25 Mo x P8B8 (x=0,3,6,9,12) impedance spectroscopy (EIS);
[0025] Figure 8 The Fe 34-x Co 25 Ni 25 Mo x P8B8(x=0,3,6,9,12) double layer capacitor (C dl );
[0026] Fig. 9 The Fe 34-x Co 25 Ni 25 Mo x Stability (CP) of P8B8 (x=0, 3, 6, 9, 12). DETAILED DESCRIPTION
[0027] The single element and alloy are melted at high temperature under argon protection to obtain alloy ingots, and then a series of Fe 34-x Co 25 Ni 25 Mo x P8B8 (x=0, 3, 6, 9, 12) amorphous alloy strips are directly used as working electrodes with oxygen evolution reaction (OER) performance.
[0028] The specific preparation method is as follows:
[0029] 1) According to the chemical formula of the alloy material Fe 34-x Co 25 Ni 25 Mo x P8B8 (x = 0, 3, 6, 9, 12) raw materials are prepared; wherein the purity of the raw materials Fe, Co and Ni single substances, FeB, NiP alloys used are all above 99.9%, and each single substance and alloy needs to be polished before preparing the alloy to remove the surface oxide layer;
[0030] 2) The prepared single substance and alloy are placed in a non-consumable vacuum arc furnace to repeatedly melt the samples for multiple times, and the samples are melted for a total of 5 times to obtain a master alloy ingot; wherein, the furnace process is completed under the protection of a high-purity argon environment.
[0031] 3) The master alloy ingot was placed in a quartz tube with a small hole above a single-roller belt spinning machine. In an environment filled with high-purity argon, the master alloy was inductively melted and the molten alloy liquid was sprayed onto a copper roller with a rotation speed of 40m / s by using the pressure difference to obtain Fe 34-x Co 25 Ni 25 Mo x P8B8 (x=0, 3, 6, 9, 12) amorphous alloy strips; wherein the master alloy ingot needs to be polished before being placed in the quartz tube to remove the surface oxide layer;
[0032] Fe 34-x Co 25 Ni 25 Mo x The thickness of the P8B8 (x=0, 3, 6, 9, 12) amorphous alloy strips is ~30 μm and the width is ~2 mm;
[0033] Through the above preparation method, Fe 34-x Co 25 Ni 25 Mo xP8B8 (x = 0, 3, 6, 9, 12) amorphous alloy strips were directly used as working electrodes for OER catalyst testing:
[0034] Test method:
[0035] The electrochemical workstation three-electrode system was used, with amorphous alloy strip as the working electrode, Ag / AgCl electrode as the reference electrode, Pt wire as the counter electrode, and 1M KOH solution as the electrolyte. All electrochemical tests were carried out in an oxygen-saturated electrolyte environment. The electrochemical tests were linear voltammetry (LSV) and impedance spectroscopy (EIS). Cyclic voltammetry (CV) and chronopotentiometry (CP) were used to test stability.
[0036] The scanning speed of LSV is 1mV s -1 , the scanning range is 1.025-1.625V vs.RHE, and the reversible hydrogen potential is calculated as E vs.RHE =E Ag / AgCl +0.1989V+0.059*PH, overpotential η=E vs.RHE -1.23V. The Tafel slope is calculated by η=a+blog|j|, where b is the Tafel slope and j is the exchange current density; the double layer capacitance (C dl ) was calculated by cyclic voltammetry (CV) in the non-Faraday range, with a CV test range of 1.125-1.225 V vs. RHE and a scan rate of 20 mVs -1 , 25mVs -1 , 30mVs -1 , 35mVs -1 and 40mVs -1 , double layer capacitance (C dl ) is calculated as C dl =du / dv, the active surface area is half of the double layer capacitance; the stability is at a current density of 10mA cm -2 The test was conducted under the following conditions and the test time was 20h.
[0037] The physical analysis of the sample obtained above is as follows:
[0038] Synthetic Fe 34-x Co 25 Ni 25 Mo x The diffuse scattering peaks of the disordered structure of the P8B8 (x = 0, 3, 6, 9, 12) alloy strip series are characterized by Figure 1). At the same time, Mo-0 has obvious crystal diffraction peaks. The diffraction peaks at 44.28° and 51.32° correspond to the (110) and (200) crystal planes of FeNi3 (JCPDS card: 38-0419). 38-0419); while the diffraction peaks at 45.11° and 65.66° correspond to the Co 0.3 Fe 0.7 (JCPDS card: 48-1818) of the (110) and (200) planes, the disorder of the alloy increases with the increase of Mo content;
[0039] The differential thermal analysis (DTA) curve shows that Fe 34-x Co 25 Ni 25 Mo x The P8B8 (x=0, 3, 6, 9, 12) amorphous alloy strips show a clear glass transition endothermic peak, which confirms that the sample has undergone a glass transition and also proves that the addition of Mo can effectively improve the amorphous forming ability.
[0040] Table 1Fe 34-x Co 25 Ni 25 Mo x Thermodynamic parameters of P8B8 (x=0,3,6,9,12) amorphous alloy strips
[0041] <![CDATA[Fe 34-x Co 25 In 25 Know x P8B8]]> <![CDATA[T g (K)]]> <![CDATA[T x (K)]]> <![CDATA[ΔT x (K)]]> x=0 628 655 27 x=3 610 659 49 x=6 621 671 50 x=9 658 716 58 x=12 606 658 52
[0042] On the one hand, the formation of amorphous phase in the material will produce a large number of defects, providing more active sites for electrocatalytic water decomposition; on the other hand, the large number of dangling bonds and abundant unsaturated surface atoms generated by the amorphous phase also provide a large number of adsorption sites for reactants. 34-x Co 25 Ni 25 Mo x P8B8 (x=0,3,6,9,12) amorphous alloy strips may have better OER performance as catalysts;
[0043] From the SEM images, it can be seen that when x = 9 and x = 12, obvious cracks appear on its surface, which may increase its active surface area. 34-x Co 25 Ni 25 Mo x The EDS elemental diagram of P8B8 (x=0,3,6,9,12) shows that all elements are evenly distributed;
[0044] The oxidation states of the alloys with x=0 and x=9 were analyzed by X-ray photoelectron spectroscopy (XPS). Comparing the high-resolution XPS spectra of x=0 and x=9, the Ni 2+ 2p 3 / 2 、Co 2+ 2p 3 / 2 and Fe 2+ 2p 3 / 2 The binding energies of the two metals shifted to higher values by 0.3 eV, 0.1 eV, and 0.4 eV, respectively. This is because the d orbital of the high-valent metal Mo is occupied by Ni 2+ 、Co 2+ and Fe 2+ The outer electrons of Mo are strongly attracted, thus enhancing the oxidation state of the metal ion in the hydroxide or oxyhydroxide. Mo element exists in 0 plus and +4 valences, and the contents of B species and O species are very close;
[0045] Fe 34-x Co 25 Ni 25 Mo x P8B8 (x=0, 3, 6, 9, 12) amorphous alloy strips were used as working electrodes, and their OER electrocatalytic activities were measured in 1.0M KOH electrolyte. The LSV polarization curves showed that when the current density reached 10 mA cm -2 When x=9, the amorphous alloy strip exhibits the best OER performance with an overpotential of 352 mV.
[0046] Calculated Fe 34-x Co 25 Ni 25 Mo x The Tafel slopes of the P8B8 (x=0, 3, 6, 9, 12) amorphous alloy strips are shown in Figure 2. The amorphous alloy strip with x=9 exhibits the smallest Tafel slope (47.63 mV dec -1 ), indicating that it has the fastest reaction kinetics;
[0047] Fe 34-x Co 25 Ni 25 Mo x The impedance spectrum of the P8B8 (x=0,3,6,9,12) amorphous alloy strips shows that the charge transfer resistance (R ct )(6.01ohm) is the smallest, indicating the fastest charge transfer capability;
[0048] The Fe 34-x Co 25 Ni 25 Mo xDouble layer capacitance (C) of P8B8 (x=0,3,6,9,12) amorphous alloy strip electrocatalyst dl ) value, and also the double-layer capacitance value of the amorphous alloy strip when x=9 is small, indicating that it has the largest electrochemically active surface area;
[0049] The Fe 34-x Co 25 Ni 25 Mo x The stability of the P8B8 (x = 0, 3, 6, 9, 12) amorphous alloy strip electrocatalyst is also the smallest potential decay and the lowest potential of the amorphous alloy strip when x = 9. This shows that by optimizing the Mo component, the alloy has enhanced OER activity and also has the best stability;
[0050] Table 2Fe 34-x Co 25 Ni 25 Mo x Electrochemical performance evaluation parameters of P8B8 (x=0,3,6,9,12) amorphous alloys
[0051] <![CDATA[Fe 34-x Co 25 In 25 Know x P8B8]]> <![CDATA[η 10 (K)]]> <![CDATA[Tafel slope (mV dec -1 )]]> <![CDATA[R ct (ohm)]]> <![CDATA[C dl (mFcm -2 )]]> x=0 383 66.59 10.84 0.19 x=3 374 58.61 9.25 0.35 x=6 357 51.87 7.19 0.51 x=9 352 47.63 6.01 0.52 x=12 366 56.74 7.94 0.36
[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A molybdenum-based amorphous alloy, characterized in that: The molybdenum-based amorphous alloy raw materials include simple substances Ni, Co and Fe, and alloys FeB and NiP.
2. The molybdenum-based amorphous alloy according to claim 1, characterized in that: The purity of the single elements Ni, Co and Fe, and the alloys FeB and NiP in the raw materials is not less than 99.9%.
3. The molybdenum-based amorphous alloy according to claim 1, characterized in that: The chemical formula of the molybdenum-based amorphous alloy is Fe 34-x Co 25 Ni 25 Mo x P8B8, where x=0,3,6,9,12.
4. The molybdenum-based amorphous alloy according to claim 3, characterized in that: The chemical formula of the molybdenum-based amorphous alloy is Fe 25 Co 25 Ni 25 Mo9P8B8.
5. The molybdenum-based amorphous alloy according to claim 1, characterized in that: The molybdenum-based amorphous alloy is a strip structure.
6. The molybdenum-based amorphous alloy according to claim 5, characterized in that: The thickness of the molybdenum-based amorphous alloy is no more than 30 μm, and the width is 2-3 mm.
7. The method for preparing a molybdenum-based amorphous alloy according to claim 1, characterized in that: The following steps are involved: S1, melting the raw materials under argon protection, and obtaining a master alloy ingot after cooling; S2, the master alloy ingot is prepared in an induction furnace by a single-roller strip spinning method to obtain a molybdenum-based amorphous alloy.
8. The method for preparing a molybdenum-based amorphous alloy according to claim 7, characterized in that: In step S1, the smelting temperature is 2400-2800°C.
9. The method for preparing a molybdenum-based amorphous alloy according to claim 8, characterized in that: In step S2, the tangential speed of the single-roller belt-spinning machine used in the single-roller belt-spinning method is 30-40 m / s.
10. The method for preparing a molybdenum-based amorphous alloy according to claim 9, characterized in that: In step S2, the tangential speed of the single-roller belt-spinning machine used in the single-roller belt-spinning method is 35 m / s.