Method for detecting metal of silicon wafer body
Through the metal detection method of silicon wafer body through tungsten-molybdenum alloy hammer crushing and multiple cleaning liquid treatment, the problems of pollution and low recovery in silicon wafer detection are solved, the detection accuracy and accuracy are improved, and the gap in silicon wafer matrix detection is filled. .
Patent Information
- Application Number
- CN202411348253.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art lacks matrix metal detection standards for silicon wafers, and the finished product of silicon wafers leads to problems such as risk of pollution and low spike recovery during the inspection process.
The silicon wafer was crushed by a tungsten-molybdenum alloy hammer, combined with the treatment of two cleaning solution and digestion solution, including the ratio of ultrapure nitric acid, hydrofluoric acid and hydrogen peroxide, and was detected by an inductively coupled plasma mass spectrometer.
It improves the accuracy and accuracy of metal detection of silicon wafers, removes surface metal impurities and slight organic pollution, enhances the purity and digestion effect of the sample, and fills the gap in silicon wafer matrix detection of downstream products of silicon materials.
Smart Images

Figure BDA0005061591030000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicon wafer detection, and in particular to a method for detecting metal in a silicon wafer. Background Art
[0002] Silicon material is a material commonly used in various fields such as electronics, semiconductors, and solar energy, among which surface metal and bulk metal are important indicators. Surface metal refers to the metal content on the surface of silicon material, which is generally based on the detection of glow discharge mass spectrometer (GDMS), in which the main detection is the elemental composition of the thin layer surface. Bulk metal refers to the metal elements contained in silicon material, which can be detected by inductively coupled plasma optical emission spectroscopy (ICP-OES) or inductively coupled plasma mass spectrometry (ICP-MS).
[0003] Silicon wafers are downstream products of silicon materials. Currently, there are surface metal and bulk metal testing standards for silicon materials (GB / T24583, GB / T 37049), as well as surface metal testing standards for silicon wafers (GB / T 39145) in China, but there are no base metal testing standards for silicon wafers.
[0004] Since silicon wafers are finished products, there are certain risks when using silicon wafers to prepare samples. For example, improper operation may cause contamination of the silicon wafers. At the same time, it is not applicable to treat silicon wafers according to the pre-treatment method of silicon materials, which will lead to low spike recovery rates of each element sample in actual detection.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The object of the present invention is to provide a method for detecting metal in a silicon wafer.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides a method for detecting metal in a silicon wafer, comprising:
[0009] S1. Sample preparation: using a tungsten-molybdenum alloy hammer to crush a silicon wafer sample, and then grinding the crushed sample to obtain a sample;
[0010] S2, sample pretreatment: adding the sample to a first cleaning solution for soaking, and then washing with ultrapure water until neutral; then adding a second cleaning solution for soaking again, and then washing with ultrapure water until neutral, and drying to obtain a pretreated sample, wherein the first cleaning solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water, and the second cleaning solution includes ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water;
[0011] S3, sample digestion: adding a digestion solution to the pretreated sample until the pretreated sample is completely dissolved, and after the digestion reaction is completed, heating and evaporating to obtain a digested sample, wherein the digestion solution includes ultrapure nitric acid and ultrapure hydrofluoric acid;
[0012] S4. Sample detection: Add recovery liquid to the digested sample to dissolve and recover the sample and fix the volume to obtain a detection solution. Sampling the detection solution into an inductively coupled plasma mass spectrometer to determine the content of the metal element to be analyzed in the solution. The recovery liquid includes ultrapure nitric acid, hydrochloric acid and ultrapure water.
[0013] In an optional embodiment, the volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the first cleaning solution is 1:0.8-1.2:1;
[0014] Preferably, the mass volume ratio of the sample to the first cleaning liquid is 1 g: 3-5 ml.
[0015] In an optional embodiment, the volume ratio of ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water in the second cleaning solution is 1:0.8-1.2:25;
[0016] Preferably, the mass volume ratio of the sample to the second cleaning liquid is 1 g: 3-5 ml.
[0017] In an optional embodiment, the digestion solution comprises ultrapure nitric acid and ultrapure hydrofluoric acid in a volume ratio of 1:3.2-4.8;
[0018] Preferably, the mass volume ratio of the pretreated sample to the digestion solution is 1 g: 10-20 ml.
[0019] In an optional embodiment, the volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the recovery liquid is 1:0.8-1.2:50;
[0020] Preferably, the mass volume ratio of the digested sample to the recovered liquid is 1 g: 4-6 ml;
[0021] Preferably, the recovery amount of mercury in the test solution is greater than 80%.
[0022] In an optional embodiment, the resistivity of the ultrapure water is greater than 18.2 MΩ·cm; the mass fraction concentration of the ultrapure nitric acid is 69-70%; the mass fraction concentration of the hydrochloric acid is 35-40%; and the mass fraction concentration of the ultrapure hydrofluoric acid is 40-50%.
[0023] In an optional embodiment, the grinding includes placing the crushed sample into a PE bag for isolation and then grinding it.
[0024] In an optional embodiment, before grinding the crushed sample, the crushed sample is placed in a beaker and mixed, and then divided into two parts using a quartering method, and each part is put into a PE bag for isolation, and then ground, one part is used for sample testing, and the other is used for sample retesting.
[0025] In an optional embodiment, the drying includes placing the cleaned sample on an electric heating plate at 100-110° C. for drying.
[0026] In an optional embodiment, the heating and evaporation to dryness comprises placing the digested sample on a 180-220° C. electric heating plate for heating and evaporation to dryness.
[0027] In an optional embodiment, the silicon wafer sample includes at least one of a silicon single crystal polished wafer, a silicon epitaxial wafer, a silicon annealed wafer and a silicon diffusion wafer.
[0028] The present invention has the following beneficial effects:
[0029] The detection method of silicon chip body metal provided by the present invention, which crushes the silicon chip sample by a tungsten-molybdenum alloy hammer, does not introduce new metal elements, and ensures the purity of the silicon chip sample during the preparation process. In addition, the present invention uses two cleaning solutions for immersion cleaning, adds hydrochloric acid to the first cleaning solution, and adds hydrogen peroxide to the second cleaning solution. The hydrogen peroxide has oxidizing properties. The metal impurities on the surface of the silicon chip can be well removed by cleaning with two cleaning solutions, and the particles on the surface can be removed by oxidation and etching. It can also remove slight organic pollutants and some metalized pollutants, thereby improving the accuracy of the detection results of the silicon chip body metal and avoiding the interference of the surface metal. At the same time, the present invention also limits the digestion solution and the recovery solution, improves the digestion and dissolution effect of the silicon chip body metal, and improves the detection accuracy of the silicon chip body metal. The detection method of silicon chip body metal provided by the present invention fills the gap in the current substrate detection of silicon wafers, a downstream product of silicon materials, and is easy to promote. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0031] The present invention provides a method for detecting metal in a silicon wafer, comprising:
[0032] S1. Sample preparation.
[0033] The silicon wafer sample is crushed by using a tungsten-molybdenum alloy hammer, and then the crushed sample is ground to obtain the sample.
[0034] In the present invention, a tungsten-molybdenum alloy hammer is used to crush the silicon wafer sample, and the crushed particle size is 2-5mm. Since the analysis of metal elements in the silicon wafer sample does not include tungsten and molybdenum, there is no need to consider the contamination of the sample by tungsten and molybdenum during the sampling process; and the hardness of the silicon wafer sample is about 6.5 and the texture is brittle, while the hardness of the tungsten-molybdenum alloy is as high as 20 or more and the texture is hard. It is easy to use the tungsten-molybdenum alloy to break the silicon wafer sample, and there will be no tungsten-molybdenum debris adhering to the surface of the broken sample of the silicon wafer sample, so there is no need to consider the influence of tungsten and molybdenum elements on the test results. When conventional glass rods or wooden rods are used for grinding, the grinding particle size does not meet the requirements, and multiple grindings are required, which prolongs the crushing time. In this process, impurities are easily introduced.
[0035] Furthermore, after crushing, the crushed sample was placed in a beaker and mixed, and then divided into two parts using the quartering method, and respectively put into PE bags for isolation, and then ground, one of which was used for sample testing, and the other was used for sample retesting.
[0036] Subsequently, the crushed samples are placed in PE bags for isolation and then ground. The PE bags can isolate the crushed samples from the grinding equipment, ensuring the cleanliness of the crushed samples and preventing them from being contaminated during the grinding process.
[0037] S2. Sample pretreatment.
[0038] Weigh about 5.0-10.0 g of sample, accurate to 0.1 g, and put it into a 50 mL PFA beaker. Add the sample into the first cleaning solution for soaking, and then wash it with ultrapure water until it is neutral; then add the second cleaning solution for soaking again, and then wash it with ultrapure water until it is neutral; dry it to obtain a pretreated sample.
[0039] Wherein, the first cleaning solution comprises ultrapure nitric acid, hydrochloric acid and ultrapure water, and the volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the first cleaning solution is 1:0.8-1.2:1; preferably, the mass volume ratio of the sample to the first cleaning solution is 1g:3-5ml. The resistivity of ultrapure water is greater than 18.2MΩ·cm; the mass fraction concentration of ultrapure nitric acid is 69-70%; the mass fraction concentration of hydrochloric acid is 35-40%. In some embodiments of the present invention, the volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water can be, for example, any one of 1:0.8:1, 1:0.9:1, 1:1:1, 1:1.1:1, 1:1.2:1 or a range value between any two of them. When the components or dosage of the first cleaning solution are not within the scope of the present application, its cleaning effect is poor. The mass volume ratio of the sample to the first cleaning solution can be, for example, any one of 1g:3ml, 1g:4ml, 1g:5ml or a range value between any two of them.
[0040] The second cleaning solution includes ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water. The volume ratio of ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water in the second cleaning solution is 1:0.8-1.2:25; preferably, the mass volume ratio of the sample to the second cleaning solution is 1g:3-5ml. The mass fraction concentration of ultrapure hydrofluoric acid is 40-50%, and the mass fraction concentration of hydrogen peroxide is 30%. In some embodiments of the present invention, the volume ratio of ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water can be, for example, any one of 1:0.8:25, 1:0.9:25, 1:1:25, 1:1.1:25, 1:1.2:25 or a range value between any two. When the components or dosage of the second cleaning solution are not within the scope of the present application, its cleaning effect is poor. The mass volume ratio of the sample to the second cleaning solution can be, for example, any one of 1g:3ml, 1g:4ml, 1g:5ml or a range value between any two.
[0041] Drying includes placing the cleaned sample on a 100-110°C electric heating plate for drying.
[0042] In the present invention, two cleaning solutions are used for immersion cleaning, wherein hydrochloric acid is added to the first cleaning solution, and the combination of hydrochloric acid and ultrapure nitric acid can effectively remove metal impurities on the surface of the silicon wafer. Further, hydrogen peroxide is added to the second cleaning solution, and hydrogen peroxide has oxidizing properties, which can remove surface particles by oxidation and etching, and can also remove slight organic pollutants and some metalized pollutants. Compared with one cleaning, the cleaning effect is better through two cleaning solutions, and the residual surface impurity elements are greatly reduced, thereby making the detection result more accurate.
[0043] S3. Sample digestion.
[0044] Use an electronic balance to accurately weigh 0.5-1g of the cleaned and dried pretreated sample, accurate to 0.0001g, and place it in a clean and dry 50mL PFA beaker. Use a pipette to add a certain amount of digestion solution in batches until the pretreated sample is completely dissolved. After the digestion reaction is completed, heat and evaporate to dryness to obtain a digested sample. The digestion solution includes ultrapure nitric acid and ultrapure hydrofluoric acid.
[0045] The digestion solution includes ultrapure nitric acid and ultrapure hydrofluoric acid in a volume ratio of 1:3.2-4.8; preferably, the mass volume ratio of the pretreated sample to the digestion solution is 1g:10-20ml. In some embodiments of the present invention, the volume ratio of ultrapure nitric acid and ultrapure hydrofluoric acid can be, for example, any one of 1:3.2, 1:3.5, 1:4, 1:4.2, 1:4.5, 1:4.8, or a range value between any two of them. The mass volume ratio of the pretreated sample to the digestion solution can be, for example, any one of 1g:10ml, 1g:12ml, 1g:15ml, 1g:18ml, 1g:20ml, or a range value between any two of them.
[0046] Since the purity of single crystal silicon is higher than that of silicon material, in the present invention, the ratio of ultrapure nitric acid to ultrapure hydrofluoric acid in the digestion solution is changed, the ratio of ultrapure hydrofluoric acid is appropriately increased, and the ratio of ultrapure nitric acid is reduced, which is more conducive to increasing the amount of insoluble metal elements in the single crystal silicon wafer converted into dissolved ion forms, thereby facilitating the improvement of the accuracy of subsequent detection. When the amount of ultrapure hydrofluoric acid in the digestion solution is too much or too low, the digestion effect is poor, and the metal in the pre-treated sample cannot be effectively digested, resulting in inaccurate detection and low detection results.
[0047] Heating and evaporating to dryness includes placing the digested sample on a 180-220°C electric heating plate and heating and evaporating to dryness.
[0048] S4. Sample testing.
[0049] A recovery solution is added to the digested sample to dissolve and recover the sample and adjust the volume to obtain a detection solution. The detection solution is sampled and put into an inductively coupled plasma mass spectrometer to determine the content of the metal element to be analyzed in the solution. The recovery solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water.
[0050] The volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the recovery liquid is 1:0.8-1.2:50; preferably, the mass volume ratio of the digested sample to the recovery liquid is 1g:4-6ml; in the present invention, by adding a small amount of hydrochloric acid, it can increase the recovery of mercury element, preferably, the recovery of mercury in the detection solution is greater than 80%. In other embodiments of the present invention, the volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the recovery liquid can be, for example, any one of 1:0.8:50, 1:0.9:50, 1:1:50, 1:1.1:50, 1:1.2:50 or a range value between any two of them. The mass volume ratio of the digested sample to the recovery liquid can be, for example, any one of 1g:4ml, 1g:5ml, 1g:6ml or a range value between any two of them.
[0051] It should be understood that the subsequent method of taking samples and measuring them in an inductively coupled plasma mass spectrometer is the same as the method of detecting silicon materials, and the method of analyzing the results is also the same as the method of detecting silicon materials.
[0052] The silicon wafer sample in the present invention includes but is not limited to at least one of a silicon single crystal polished wafer, a silicon epitaxial wafer, a silicon annealed wafer and a silicon diffusion wafer.
[0053] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0054] The reagents involved in the subsequent examples and comparative examples are as follows: ultrapure water: resistivity greater than 18.2 MΩ·cm; ultrapure nitric acid: mass fraction 69%; ultrapure hydrofluoric acid: mass fraction 49%; hydrochloric acid: mass fraction 37%; hydrogen peroxide: mass fraction 30%.
[0055] Example 1
[0056] This embodiment provides a method for detecting metal in a silicon wafer, which includes:
[0057] S1. Sample preparation: Samples are crushed in a special clean grinding room. Keep the room clean, dust-free, and free of volatile chemicals. Use a tungsten-molybdenum alloy hammer to crush silicon wafer samples. The crushed particle size is 2-5mm. Place the crushed sample in a PFA beaker and mix it evenly. Then divide it into two parts using the quartering method, put them into PE bags for isolation, and then grind them. One part is used for sample testing, and the other is used for sample retention and retesting.
[0058] S2. Sample pretreatment: Weigh about 5.0-10.0g of sample, accurate to 0.1g, put it into a 50mL PFA beaker, add the first cleaning solution to soak the sample, the first cleaning solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water in a volume ratio of 1:1:1, the mass volume ratio of the sample to the first cleaning solution is 1g:4ml, and then wash it with ultrapure water until neutral. Then add the second cleaning solution, the second cleaning solution includes ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water in a volume ratio of 1:1:25, the mass volume ratio of the sample to the second cleaning solution is 1g:4ml, soak it again, and then wash it with ultrapure water until neutral. Place the sample on the electric heating plate, set the temperature of the heating plate thermostat to 105℃ for drying, and obtain the pretreated sample for use in weighing.
[0059] S3. Sample digestion.
[0060] Use an electronic balance to accurately weigh 0.5-1g of the cleaned and dried pre-treated sample to an accuracy of 0.0001g, place it in a clean and dry 50mL PFA beaker, and use a pipette to add a certain amount of digestion solution in batches. The digestion solution includes ultrapure nitric acid and ultrapure hydrofluoric acid in a volume ratio of 1:4, and the mass volume ratio of the pre-treated sample to the digestion solution is 1g:15ml. After the pre-treated sample is completely dissolved and the digestion reaction is completed, place the digested sample on a 200℃ electric heating plate for heating and evaporation to dryness to obtain a digested sample.
[0061] S4. Sample testing.
[0062] A recovery solution is added to the digested sample to dissolve, recover and fix the volume. The volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the recovery solution is 1:1:50. The mass volume ratio of the digested sample and the recovery solution is 1g:5ml to obtain a detection solution. The detection solution is sampled into an inductively coupled plasma mass spectrometer (Agilent 8900ICPMS) to determine the content of the metal elements to be analyzed in the solution. The recovery solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water.
[0063] Example 2
[0064] This embodiment provides a method for detecting metal in a silicon wafer, which includes:
[0065] S1. Sample preparation: Samples are crushed in a special clean grinding room. Keep the room clean, dust-free, and free of volatile chemicals. Use a tungsten-molybdenum alloy hammer to crush silicon wafer samples. The crushed particle size is 2-5mm. Place the crushed sample in a PFA beaker and mix it evenly. Then divide it into two parts using the quartering method, put them into PE bags for isolation, and then grind them. One part is used for sample testing, and the other is used for sample retention and retesting.
[0066] S2. Sample pretreatment: Weigh about 5.0-10.0g of sample, accurate to 0.1g, put it into a 50mL PFA beaker, add the first cleaning solution to soak the sample, the first cleaning solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water in a volume ratio of 1:0.8:1, the mass volume ratio of the sample to the first cleaning solution is 1g:3ml, and then wash it with ultrapure water until neutral. Then add the second cleaning solution, the second cleaning solution includes ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water in a volume ratio of 1:0.8:25, the mass volume ratio of the sample to the second cleaning solution is 1g:3ml, soak it again, and then wash it with ultrapure water until neutral. Place the sample on the electric heating plate, set the temperature of the heating plate thermostat to 100℃ for drying, and obtain the pretreated sample for standby weighing.
[0067] S3. Sample digestion.
[0068] Use an electronic balance to accurately weigh 0.5-1g of the cleaned and dried pre-treated sample to an accuracy of 0.0001g, place it in a clean and dry 50mL PFA beaker, and use a pipette to add a certain amount of digestion solution in batches. The digestion solution includes ultrapure nitric acid and ultrapure hydrofluoric acid in a volume ratio of 1:3.2, and the mass volume ratio of the pre-treated sample to the digestion solution is 1g:10ml. After the pre-treated sample is completely dissolved, after the digestion reaction is completed, place the digested sample on a 180℃ electric heating plate for heating and evaporation to dryness to obtain a digestion sample.
[0069] S4. Sample testing.
[0070] A recovery solution is added to the digested sample to dissolve, recover and fix the volume. The volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the recovery solution is 1:0.8:50. The mass volume ratio of the digested sample to the recovery solution is 1g:4ml to obtain a detection solution. The detection solution is sampled into an inductively coupled plasma mass spectrometer (Agilent 8900ICPMS) to determine the content of the metal element to be analyzed in the solution. The recovery solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water.
[0071] Example 3
[0072] This embodiment provides a method for detecting metal in a silicon wafer, which includes:
[0073] S1. Sample preparation: Samples are crushed in a special clean grinding room. Keep the room clean, dust-free, and free of volatile chemicals. Use a tungsten-molybdenum alloy hammer to crush silicon wafer samples. The crushed particle size is 2-5mm. Place the crushed sample in a PFA beaker and mix it evenly. Then divide it into two parts using the quartering method, put them into PE bags for isolation, and then grind them. One part is used for sample testing, and the other is used for sample retention and retesting.
[0074] S2. Sample pretreatment: Weigh about 5.0-10.0g of sample, accurate to 0.1g, put it into a 50mL PFA beaker, add the first cleaning solution to soak the sample, the first cleaning solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water in a volume ratio of 1:1.2:1, the mass volume ratio of the sample to the first cleaning solution is 1g:5ml, and then wash it with ultrapure water until neutral. Then add the second cleaning solution, the second cleaning solution includes ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water in a volume ratio of 1:1.2:25, the mass volume ratio of the sample to the second cleaning solution is 1g:5ml, soak it again, and then wash it with ultrapure water until neutral. Place the sample on the electric heating plate, set the temperature of the heating plate thermostat to 110℃ for drying, and obtain the pretreated sample for use in weighing.
[0075] S3. Sample digestion.
[0076] Use an electronic balance to accurately weigh 0.5-1g of the cleaned and dried pre-treated sample to an accuracy of 0.0001g, place it in a clean and dry 50mL PFA beaker, and use a pipette to add a certain amount of digestion solution in batches. The digestion solution includes ultrapure nitric acid and ultrapure hydrofluoric acid in a volume ratio of 1:4.8, and the mass volume ratio of the pre-treated sample to the digestion solution is 1g:20ml. After the pre-treated sample is completely dissolved, after the digestion reaction is completed, place the digested sample on a 220℃ electric heating plate for heating and evaporation to dryness to obtain a digestion sample.
[0077] S4. Sample testing.
[0078] A recovery solution is added to the digested sample to dissolve, recover and fix the volume. The volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the recovery solution is 1:1.2:50. The mass volume ratio of the digested sample to the recovery solution is 1g:6ml to obtain a detection solution. The detection solution is sampled into an inductively coupled plasma mass spectrometer (Agilent 8900ICPMS) to determine the content of the metal element to be analyzed in the solution. The recovery solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water.
[0079] Comparative Example 1
[0080] This comparative example provides a detection method, which is basically the same as Example 1, except that in this comparative example, a plexiglass rod is directly used to break the silicon wafer sample.
[0081] Comparative Example 2
[0082] This comparative example provides a detection method, which is basically the same as Example 1, except that the operation of isolating with a PE bag is omitted in this comparative example.
[0083] Comparative Example 3
[0084] This comparative example provides a detection method, which is basically the same as Example 1, except that only one cleaning solution (the volume ratio of HNO3, HF and H2O is 2:3:60) is used for cleaning in this comparative example. Specifically, step S2 in this comparative example is different from that in Example 1. Step S2 of this comparative example includes: weighing about 5.0-10.0g of sample, accurate to 0.1g, putting it into a 50mL PFA beaker, adding the sample into the cleaning solution for soaking, the cleaning solution includes HNO3, HF and H2O in a volume ratio of 2:3:60, the mass volume ratio of the sample to the cleaning solution is 1g:5ml, and then washing with ultrapure water until neutral. Place the sample on an electric heating plate, set the temperature of the heating plate thermostat at 100-110℃ for drying, and obtain a pretreated sample for standby weighing.
[0085] Comparative Example 4
[0086] This comparative example provides a detection method, which is basically the same as Example 1, except that in this comparative example, only the first cleaning solution (ultrapure nitric acid, hydrochloric acid and ultrapure water in a volume ratio of 1:1:1) is used for cleaning.
[0087] Comparative Example 5
[0088] This comparative example provides a detection method, which is basically the same as Example 1, except that in this comparative example, only the second cleaning liquid (ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water in a volume ratio of 1:1:25) is used for cleaning.
[0089] Comparative Example 6
[0090] This comparative example provides a detection method, which is basically the same as Example 1, except that the digestion solution in this comparative example includes ultrapure nitric acid and ultrapure hydrofluoric acid in a volume ratio of 1:2.
[0091] Comparative Example 7
[0092] This comparative example provides a detection method, which is basically the same as Example 1, except that the digestion solution in this comparative example comprises ultrapure nitric acid and ultrapure hydrofluoric acid in a volume ratio of 1:5.
[0093] Comparative Example 8
[0094] This comparative example provides a detection method, which is basically the same as Example 1, except that the recovery liquid in this comparative example comprises ultrapure nitric acid and ultrapure water in a volume ratio of 1:50.
[0095] Comparative Example 9
[0096] This comparative example provides a detection method, which is basically the same as Example 1, except that the recovery liquid in this comparative example includes ultrapure nitric acid, hydrochloric acid and ultrapure water in a volume ratio of 1:2:50.
[0097] Experimental Example 1
[0098] The detection solutions of the above-mentioned Examples 1-3 and Comparative Examples 1-9 were respectively tested, and the detection solutions were sampled into an inductively coupled plasma mass spectrometer (Agilent 8900ICPMS) to determine the content (unit: ng / g) of the metal element to be analyzed in the solution. Please refer to Table 1 for the test results.
[0099] Table 1. Statistical table of the test results of the metal elements to be analyzed in the test solutions of different examples
[0100]
[0101]
[0102] As can be seen from the above table, referring to GB / T 37049-2018, the determination of the matrix metal impurity content in polycrystalline silicon is used to compare the silicon wafer detection. The detection results of Examples 1-3 of the present invention are more accurate, while Comparative Example 1 uses a glass rod to crush the silicon wafer sample, and its crushing effect is not good. It needs to be crushed repeatedly to achieve the required crushing particle size. Impurities will be introduced during the multiple crushing processes, resulting in a high test result; Comparative Example 2 did not use PE bags for isolation and grinding, resulting in a high result due to sample contamination; Comparative Examples 3, 4, and 5 had poor cleaning effects, resulting in residual impurity elements on the surface, resulting in high test results; the volume ratio of the digestion solution in Comparative Examples 6 and 7 is not within the scope of the present invention, resulting in poor digestion effect and low test results; Comparative Examples 8 and 9 have poor recovery liquid effects and low test results.
[0103] Experimental Example 2
[0104] The detection solutions of Examples 1-3 of the present invention and Comparative Examples 8-9 were spiked and tested. The recovery rates (in %) were shown in Table 2:
[0105] Table 2. Statistical table of recovery results of spiked detection for different examples
[0106] Example iron chromium nickel copper Zinc sodium mercury Example 1 92 88 96 98 98 93 87 Example 2 90 90 92 98 94 93 88 Example 3 92 85 92 96 97 95 83 Comparative Example 8 85 82 90 92 87 90 65 Comparative Example 9 87 83 88 91 90 94 73
[0107] It can be seen from the above table that the recovery rates of various metal elements in the embodiments of the present invention are relatively high, especially the recovery rate of mercury is also relatively high.
[0108] In summary, the detection method of silicon chip body metal provided by the present invention, which crushes the silicon chip sample by a tungsten-molybdenum alloy hammer, does not introduce new metal elements, and ensures the purity of the silicon chip sample during the preparation process. In addition, the present invention adopts two cleaning solutions for immersion cleaning, adding hydrochloric acid to the first cleaning solution and adding hydrogen peroxide to the second cleaning solution. Hydrogen peroxide is oxidizing, and the metal impurities on the surface of the silicon chip can be well removed by cleaning with two cleaning solutions. The particles on the surface are removed by oxidation and etching, and slight organic pollutants and partially metalized pollutants can also be removed, thereby improving the accuracy of the detection results of the silicon chip body metal and avoiding the interference of the surface metal. At the same time, the present invention also limits the digestion solution and the recovery solution, improves the digestion and dissolution effect of the silicon chip body metal, and improves the detection accuracy of the silicon chip body metal. The detection method of silicon chip body metal provided by the present invention fills the gap in the current substrate detection of silicon wafers, a downstream product of silicon materials, and is easy to promote.
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for detecting metal in a silicon wafer, characterized in that: It includes: S1. Sample preparation: using a tungsten-molybdenum alloy hammer to crush a silicon wafer sample, and then grinding the crushed sample to obtain a sample; S2, sample pretreatment: adding the sample into the first cleaning solution for soaking, and then washing with ultrapure water until neutral; Then, the second cleaning solution is added and soaked again, and then the sample is washed with ultrapure water until it becomes neutral and dried to obtain a pretreated sample, wherein the first cleaning solution includes ultrapure nitric acid, hydrochloric acid and ultrapure water, and the second cleaning solution includes ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water; S3, sample digestion: adding a digestion solution to the pretreated sample until the pretreated sample is completely dissolved, and after the digestion reaction is completed, heating and evaporating to obtain a digested sample, wherein the digestion solution includes ultrapure nitric acid and ultrapure hydrofluoric acid; S4. Sample detection: Add recovery liquid to the digested sample to dissolve and recover the sample and fix the volume to obtain a detection solution. Sampling the detection solution into an inductively coupled plasma mass spectrometer to determine the content of the metal element to be analyzed in the solution. The recovery liquid includes ultrapure nitric acid, hydrochloric acid and ultrapure water.
2. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the first cleaning solution is 1:0.8-1.2:1; Preferably, the mass volume ratio of the sample to the first cleaning liquid is 1 g: 3-5 ml.
3. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The volume ratio of ultrapure hydrofluoric acid, hydrogen peroxide and ultrapure water in the second cleaning solution is 1:0.8-1.2:25; Preferably, the mass volume ratio of the sample to the second cleaning liquid is 1 g: 3-5 ml.
4. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The digestion solution comprises ultrapure nitric acid and ultrapure hydrofluoric acid in a volume ratio of 1:3.2-4.8; Preferably, the mass volume ratio of the pretreated sample to the digestion solution is 1 g: 10-20 ml.
5. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The volume ratio of ultrapure nitric acid, hydrochloric acid and ultrapure water in the recovery liquid is 1:0.8-1.2:50; Preferably, the mass volume ratio of the digested sample to the recovered liquid is 1 g: 4-6 ml; Preferably, the recovery amount of mercury in the test solution is greater than 80%.
6. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The resistivity of the ultrapure water is greater than 18.2 MΩ·cm; the mass fraction concentration of the ultrapure nitric acid is 69-70%; the mass fraction concentration of the hydrochloric acid is 35-40%; and the mass fraction concentration of the ultrapure hydrofluoric acid is 40-50%.
7. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The grinding includes putting the crushed sample into a PE bag for isolation and then grinding; Preferably, before grinding the crushed sample, the method further includes placing the crushed sample in a beaker and mixing it, then dividing it into two parts by quartering method, putting them into PE bags for isolation, and then grinding them, one of which is used for sample testing and the other is used for sample retesting.
8. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The drying comprises placing the cleaned sample on a 100-110° C. electric heating plate for drying.
9. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The heating evaporation to dryness comprises placing the digested sample on an electric heating plate at 180-220° C. for heating and evaporation to dryness.
10. The method for detecting metal in a silicon wafer according to claim 1, characterized in that: The silicon wafer sample includes at least one of a silicon single crystal polished wafer, a silicon epitaxial wafer, a silicon annealed wafer and a silicon diffusion wafer.
Citation Information
Cited By
Pretreatment method for impurity element analysis of high-purity silicon material and application thereof
CN119618768A