Modified solid electrolyte and application thereof in all-solid-state silicon-carbon lithium battery

By forming a Li2CO3 layer on the surface of garnet solid electrolyte and reacting with polyvinylphosphonic acid, a lithium ion decoupling layer is formed, which solves the problems of lithium ion transmission obstacles and insufficient interface contact, and improves the cycle life of all-solid silicon-carbon lithium batteries and conductivity.

CN119050468APending Publication Date: 2024-11-29SCNU QINGYUAN INSTITUTE OF SCIENCE & TECHNOLOGY INNOVATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411382718.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the application of existing garnet solid-state lithium batteries, there are problems of lithium ion transmission obstacles and insufficient interface contact caused by expansion/contraction of silicon carbon negative electrodes, resulting in electrode deformation and reduced lithium ion interface conductivity, affecting the cycle life of the battery.

Method used

By placing garnet Li6.4La3Zr1.4Ta0.6O12 powder in air to aged to form a Li2CO3 layer and reacting with polyvinyl phosphonic acid solution to form a modified solid electrolyte, removing the passivation layer and forming a lithium ion decoupling layer, promoting the promotion of Lithium ions migrate more rapidly, and modified solid electrolyte films are prepared through polyvinyl phosphonic acid solution to improve interface conductivity.

Benefits of technology

It effectively reduces lithium ion transmission obstacles and interface resistance, improves the cycle life and room temperature ion conductivity of all-solid silicon-carbon lithium batteries, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050468A_ABST
    Figure CN119050468A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of all-solid-state lithium batteries, and particularly discloses a modified solid-state electrolyte and application thereof in an all-solid-state silicon-carbon lithium battery, polyvinyl phosphonic acid reacts with an alkaline substance Li2CO3 on the surface of garnet Li < 6.4 > La3Zr1. 4Ta0. 6O12, an alkaline substance passivation layer on the surface of the garnet Li < 6.4 > La3Zr1. 4Ta0. 6O12 is removed, a lithium ion decoupling layer is formed on the surface of the garnet Li < 6.4 > La3Zr1. 4Ta0. 6O12, and the modified solid-state electrolyte is prepared. According to the invention, lithium ions in the garnet Li < 6.4 > La < 3 > Zr < 1.4 > Ta < 0.6 > O12 can be promoted to be decoupled more quickly, so that the lithium ions can be migrated to the surface of the garnet Li < 6.4 > La < 3 > Zr < 1.4 > Ta < 0.6 > O12 from the interior of the garnet Li < 6.4 > La < 3 > Zr < 1.4 > Ta < 0.6 > O12 more quickly; compared with a battery assembled by a composite solid electrolyte film prepared from unmodified LLZTO, a battery assembled by a composite solid electrolyte film prepared from the modified solid electrolyte has better cycle performance and higher specific capacity and capacity retention rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of all-solid-state lithium batteries, in particular to a modified solid electrolyte and its application in all-solid-state silicon-carbon lithium batteries. Background Art

[0002] With the rapid development of portable electronic devices and electric vehicles, existing lithium-ion batteries will not be able to meet the increasing demand for energy density, cycle life and safety. Using inorganic solid electrolytes (SSEs) to replace flammable and toxic liquid electrolytes is an ideal solution. So far, SSEs including garnet, NASICON, sulfide and perovskite have been comprehensively explored. Among them, garnet SSEs, such as Li 6.4 LqCy 1.4 Ta 0.6 O 12 and Li 6.5 LqCy 1.5 Nb 0.5 O 12 Because of its good chemical stability to lithium metal, wide electrochemical window and high lithium ion conductivity (up to 1mS cm -1 ) is expected to become one of the candidate materials for the next generation of high-safety solid-state lithium battery electrolytes.

[0003] Although garnet SSEs have significant advantages, two major issues need to be addressed before the practical application of garnet-based solid-state silicon-carbon lithium batteries (GSSBs): (1) The Li2CO3 passivation layer hinders the transport of lithium ions in garnet SSEs. When garnet SSEs are exposed to air, H + / Li + The conversion to LiOH occurs, which then captures CO2 from the atmosphere to generate Li2CO3 on the surface of garnet SSEs. (2) The compressive stress caused by the expansion / contraction of the silicon-carbon anode leads to severe curling and deformation of the electrode, which inevitably destroys the electrode / rigid garnet SSEs electrolyte interface contact and reduces the Li + The interfacial conductivity of ions leads to rapid capacity decay. Research in recent years has shown that ceramic solid electrolytes are always used under high external pressure (>10MPa) to maintain good contact with the Si electrode, which greatly hinders the practical application of ceramic solid electrolytes.

[0004] In order to address the above two challenges, the academic community has made many efforts. In order to overcome the first difficulty, many methods have been developed to reduce the interfacial impedance between garnet SSE and the electrode, such as inorganic surface coating, polymer surface coating, pretreatment in acidic aqueous solution (HCl, H3BO3, H3PO4, citric acid), and heat treatment at temperatures >700°C. Although inorganic surface coating and polymer coating can promote the solid-solid contact between garnet SSEs and silicon-carbon electrodes, the harmful lithium-ion insulating Li2CO3 passivation layer still exists. For the thermal treatment or acidic aqueous solution treatment of garnet SSEs to remove Li2CO3, the thermal treatment process is often accompanied by the loss of Li in garnet, while the acidic aqueous solution treatment is not conducive to water-sensitive garnet SSEs. In addition, the above strategies are also limited by electron attack / leakage. How to deal with the second difficulty about the insufficient interfacial contact caused by the expansion / contraction of the silicon-carbon negative electrode, which reduces the Li + The difficulty of interfacial conductivity of ions remains an unresolved issue. In this regard, garnet SSEs with rationally designed organic surface coatings are often used, such as PEO, PVDF, PAA, PDMS, and PVDF-HFP. Compared with inorganic coatings, these organic coatings can form an electron-blocking interface between garnet SSE and electrodes, but the ionic conductivity of organic coatings is poor at room temperature. In addition, nanoscale thickness of organic coatings is difficult to achieve. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a modified solid electrolyte and its application in an all-solid-state silicon-carbon-lithium battery.

[0006] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0007] One of the purposes of the present invention is to provide a modified solid electrolyte, firstly garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The powder was aged in air for 2 days. 6.4 LqCy 1.4 Ta 0.6 O 12 A 1-2 μm thick Li2CO3 layer is formed on the powder surface to obtain modified garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 Powder; then the modified garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12The powder is mixed with a polyvinyl phosphonic acid solution, with a mass ratio of the modified LLZTO powder to the polyvinyl phosphonic acid in the polyvinyl phosphonic acid solution (0.1-0.2):1, and reacted at 60-80° C. for 12 hours to obtain a modified solid electrolyte.

[0008] The principle of this scheme is: using polyvinylphosphonic acid (PVPA) and garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The Li2CO3 reaction on the surface removes the garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The alkaline passivation layer on the surface of garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The formation of a lithium ion decoupling layer on the surface can promote the garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The internal lithium ions are decoupled more quickly, allowing the lithium ions to be released from the garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 Internal migration to garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 surface.

[0009] Furthermore, the polyvinyl phosphonic acid solution is obtained by dissolving polyvinyl phosphonic acid in an alcohol solvent, and the mass fraction of polyvinyl phosphonic acid in the polyvinyl phosphonic acid solution is 95-97%.

[0010] Preferably, the alcohol solvent includes isopropanol.

[0011] A second object of the present invention is to provide an application of a modified solid electrolyte in the preparation of an all-solid-state silicon-carbon-lithium battery.

[0012] The third object of the present invention is to provide an all-solid-state silicon-carbon-lithium battery, comprising a positive electrode, a negative electrode, and a composite solid electrolyte located between the positive electrode and the negative electrode, wherein the composite solid electrolyte is a modified solid electrolyte film prepared using a modified solid electrolyte.

[0013] The principle of this scheme is: the lithium ion decoupling layer can also effectively suppress the internal short circuit of the modified solid electrolyte film caused by the physical gap and the volume expansion of the silicon-carbon negative electrode, thereby effectively improving the cycle life of the all-solid-state silicon-carbon lithium battery assembled by the modified solid electrolyte film.

[0014] Furthermore, the thickness of the modified solid electrolyte film is 20-50 μm.

[0015] Furthermore, the preparation method of the modified solid electrolyte film comprises:

[0016] S1, mixing polyvinylphosphonic acid with a solvent to obtain a glue solution having a polyvinylphosphonic acid concentration of 6 to 14%;

[0017] S2, adding the modified solid electrolyte to the glue solution, wherein the amount of the modified solid electrolyte is 0.5-20% of the mass of the polyvinylphosphonic acid, and mixing them thoroughly to obtain a mixed slurry;

[0018] S3, subjecting the mixed slurry to a film-forming treatment to obtain the composite solid electrolyte film.

[0019] Preferably, the solvent is one or more of isopropanol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and triethyl phosphate.

[0020] Preferably, the film-forming treatment is to place the mixed slurry on a substrate, apply a scraper, and remove the solvent.

[0021] Preferably, the solvent is removed by vacuum drying at 40-60°C.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention utilizes polyvinylphosphonic acid and garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The alkaline substance Li2CO3 on the surface reacts to remove garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The alkaline substance passivation layer on the surface and the lithium ion decoupling layer formed on its surface can promote the garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The internal lithium ions are decoupled more quickly, allowing the lithium ions to be released from the garnet Li 6.4 LqCy 1.4 Ta 0.6 O12 Internal migration to garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 surface.

[0024] 2. In the modified solid electrolyte film prepared by using the modified solid electrolyte of the present invention, the lithium ion decoupling layer on the surface of the modified solid electrolyte can be formed on the garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 It plays a bonding role with polyvinylphosphonic acid to form a dense interface layer, thereby reducing the physical gap caused by the different volume expansion coefficients during the charge and discharge process, greatly reducing the interface resistance of mass transfer between garnet-type solid electrolyte and polyvinylphosphonic acid, and constructing a smooth ion path inside polyvinylphosphonic acid, making garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 Internal lithium ions can be decoupled more quickly and transferred through the segmental movement of polyvinylphosphonic acid, thereby effectively improving the room temperature ionic conductivity of the modified solid electrolyte film, solving the problem of existing organic-inorganic composite solid electrolytes that lithium ions at the organic-inorganic interface cannot be quickly decoupled and transferred through the segmental movement of the polymer due to the different phase structures between garnet-type solid electrolytes and polyvinylphosphonic acid; at the same time, the lithium ion decoupling layer can also effectively suppress the internal short circuit of the modified solid electrolyte film caused by the physical gap and the volume expansion of the silicon-carbon negative electrode, thereby effectively improving the cycle life of the all-solid-state silicon-carbon lithium battery assembled with the modified solid electrolyte film. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the reaction mechanism of NMP and Li2CO3 on the surface of LLZTO in the present invention;

[0026] Figure 2 : is the element distribution diagram of LLZTO before and after modification of the present invention;

[0027] Figure 3 1 is the XRD diffraction pattern of LLZTO before (upper) and after (lower) modification of the present invention;

[0028] Figure 4 This is a TEM image of LLZTO modified in Example 3 of the present invention;

[0029] Figure 5 1 is an electrochemical performance cycle diagram of the modified solid electrolyte film prepared in Example 1 and Example 3 of the present invention;

[0030] Figure 6It is the electrochemical performance ratio diagram of the modified solid electrolyte film prepared in Example 1 and Example 3 of the present invention;

[0031] Figure 7 It is the EIS data diagram of the modified solid electrolyte film prepared in Example 1 and Example 3 of the present invention. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the invention.

[0033] Example 1

[0034] A certain amount of Li 6.4 LqCy 1.4 Ta 0.6 O 12 The powder (LLZTO) was aged in air for 2 days, and a Li2CO3 layer of about 1 to 2 μm thick was formed on the surface of the electrolyte to obtain the modified LLZTO powder. 9.6 g of polyvinylphosphonic acid (PVPA) was added to 10 g of isopropyl alcohol (IPA) to prepare a polyvinylphosphonic acid solution with a concentration of 96%. 1.44 g of the modified LLZTO powder was mixed with the polyvinylphosphonic acid solution and reacted at 70°C for 12 hours to obtain a modified solid electrolyte.

[0035] Example 2

[0036] In an argon-filled glove box, 0.05 g of polyvinylphosphonic acid (PVPA) was added to isopropyl alcohol (IPA) to prepare a 5% glue solution; 9.95 g of the modified solid electrolyte prepared in Example 1 was added to the glue solution, and stirred for 12 hours to obtain a slurry; the mixed slurry was poured on a glass plate and scraped with a scraper with a scraper height of 200 μm, and then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a modified solid electrolyte film.

[0037] Example 3

[0038] In an argon-filled glove box, 0.1 g of polyvinylphosphonic acid (PVPA) was added to isopropyl alcohol (IPA) to prepare a 10% glue solution; 9.9 g of the modified solid electrolyte prepared in Example 1 was added to the glue solution, and stirred for 12 hours to obtain a slurry; the mixed slurry was poured onto a glass plate and scraped with a scraper with a scraper height of 200 μm, and then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a modified solid electrolyte film.

[0039] Example 4

[0040] In an argon-filled glove box, 0.15 g of polyvinylphosphonic acid (PVPA) was added to isopropyl alcohol (IPA) to prepare a 15% glue solution; 9.85 g of the modified solid electrolyte prepared in Example 1 was added to the glue solution, and stirred for 12 hours to obtain a slurry; the mixed slurry was poured onto a glass plate and scraped with a scraper with a scraper height of 200 μm, and then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a modified solid electrolyte film.

[0041] Example 5

[0042] In an argon-filled glove box, 0.2 g of polyvinylphosphonic acid (PVPA) was added to isopropyl alcohol (IPA) to prepare a glue solution with a concentration of 20%; 9.8 g of the modified solid electrolyte prepared in Example 1 was added to the glue solution, and stirred for 12 hours to obtain a slurry; the mixed slurry was poured on a glass plate and scraped with a scraper with a scraper height of 200 μm, and then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a modified solid electrolyte film.

[0043] Example 6

[0044] In an argon-filled glove box, 0.25 g of polyvinylphosphonic acid (PVPA) was added to isopropyl alcohol (IPA) to prepare a 10% glue solution; 9.75 g of the modified solid electrolyte prepared in Example 1 was added to the glue solution, and stirred for 12 hours to obtain a slurry; the mixed slurry was poured onto a glass plate and scraped with a scraper with a scraper height of 200 μm, and then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a modified solid electrolyte film.

[0045] Comparative Example 1

[0046] In an argon-filled glove box, 0.1 g of poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP) was added to isopropyl alcohol (IPA) to prepare a 10% gel solution; 9.9 g of modified garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The mixed slurry was poured onto a glass plate and coated with a scraper having a height of 200 μm. The slurry was then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a composite solid electrolyte film.

[0047] Comparative Example 2

[0048] In an argon-filled glove box, 0.1 g of polyvinylidene fluoride (PVDF) was added to isopropyl alcohol (IPA) to prepare a 10% gel solution. 9.9 g of modified garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The mixed slurry was poured onto a glass plate and coated with a scraper having a height of 200 μm. The slurry was then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a composite solid electrolyte film.

[0049] Comparative Example 3

[0050] In an argon-filled glove box, 0.1 g of polyethylene oxide (PEO) was added to isopropyl alcohol (IPA) to prepare a 10% gel solution. 9.9 g of modified garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The mixed slurry was poured onto a glass plate and coated with a scraper having a height of 200 μm. The slurry was then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a composite solid electrolyte film.

[0051] Comparative Example 4

[0052] In an argon-filled glove box, 0.1 g of polyacrylonitrile (PAN) was added to isopropyl alcohol (IPA) to prepare a 10% gel solution. 9.9 g of modified garnet Li 6.4 LqCy 1.4 Ta 0.6 O 12 The mixed slurry was poured onto a glass plate and coated with a scraper having a height of 200 μm. The slurry was then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a composite solid electrolyte film.

[0053] Comparative Example 5

[0054] In an argon-filled glove box, 0.1 g of polymethacrylate (PMMA) was added to isopropyl alcohol (IPA) to prepare a 10% gel solution. 9.9 g of modified garnet Li 6.4 LqCy 1.4 Ta0.6 O 12 The mixed slurry was poured onto a glass plate and coated with a scraper having a height of 200 μm. The slurry was then placed in a vacuum oven at 60°C for drying to remove excess IPA solvent. The drying time was 12 hours to obtain a composite solid electrolyte film.

[0055] In order to more clearly illustrate the technical solutions and advantages of the present invention, various performance tests were performed on the solid electrolyte films prepared in the above-mentioned Examples 1 to 6 and Comparative Examples 1 to 5. The methods of various performance tests are as follows:

[0056] Electrochemical impedance spectroscopy (EIS) and room temperature ionic conductivity: The room temperature ionic conductivity of the present invention is tested on an electrochemical workstation (Solartron, 1470E), and the test method is: using two stainless steel metals, assembling SS / solid electrolyte film / SS battery, testing its electrochemical impedance spectrum, and calculating its room temperature ionic conductivity based on the measured electrochemical impedance spectrum. Test conditions: amplitude 10mV, frequency 100kHz-0.1Hz, test temperature 25°C.

[0057] Activation energy: The activation energy of a material is calculated from the ionic conductivity of the material at different temperatures. The ionic conductivity of this patent is tested using an electrochemical workstation (Solartron, 1470E). The test method is: use two stainless steel metals, assemble SS / solid electrolyte film / SS battery, test its electrochemical impedance spectrum, and then calculate its room temperature ionic conductivity. Test conditions: amplitude 10mV, frequency 100kHz-0.1Hz. Test temperature: 30℃, 40℃, 50℃, 60℃, 70℃, 80℃.

[0058] Discharge capacity of battery:

[0059] The assembly steps of the battery are as follows: first, mix silicon carbon (Si / C), conductive carbon black and PVDF in a ratio of 8:1:1, add an appropriate amount of PVPA solution, stir and mix, and then apply to obtain the positive electrode material; then, cut the positive electrode into discs with a diameter of 12 mm; finally, assemble the Li sheet, solid electrolyte film and positive electrode sheet in sequence to obtain an all-solid-state silicon-carbon lithium battery.

[0060] The battery test steps are as follows: use the charging and discharging equipment to perform charge and discharge tests on the battery. The specific test steps are: leave it for 12 hours; discharge at 0.1C to a voltage of 0.01V; leave it for 5 minutes; charge at 0.1C to a voltage of 1.5V; leave it for 5 minutes; repeat 3 times; and finally perform a long cycle test at 0.5 / 0.5C.

[0061] The preparation parameters and properties of the solid electrolyte films of the embodiments and comparative examples of the present invention are shown in Table 1.

[0062] Table 1 Preparation parameters and properties of composite solid electrolyte films of various embodiments of the present invention and comparative examples

[0063]

[0064]

[0065] The present invention conducted EDS element analysis on LLZTO before and after modification in Example 3. Figure 2 , among which, the element distribution before modification (top) and the P element distribution after modification (bottom), it can be seen that obvious P elements appeared on the surface of the modified LLZTO, which indicates that polyvinylphosphonic acid (PVPA) did react with the alkaline substances on the surface of LLZTO, and the generated substances were wrapped on the surface of LLZTO.

[0066] In addition, the present invention also performs XRD diffraction test on the LLZTO powder before and after modification in Example 1, as shown in FIG. Figure 3 As shown in the figure, the LLZTO powder before modification has obvious characteristic diffraction peaks of Li2CO3 at 21.35° and 31.81°, which indicates that Li2CO3 does exist on the surface of LLZTO before modification, which is consistent with the EDS data. However, when LLZTO is modified with polyvinylphosphonic acid (PVPA), the characteristic diffraction peaks of LLZTO at 21.35° and 31.81° are basically invisible, indicating that Li2CO3 participates in the reaction during the modification of LLZTO by polyvinylphosphonic acid (PVPA), and there is no obvious Li2CO3 residue on the surface of the modified LLZTO. TEM analysis was performed on the modified LLZTO in Example 3, as shown in the figure. Figure 4 ,Polyvinylphosphonic acid (PVPA) did react with the alkaline substances on the surface of LLZTO, and the thickness of the decoupling layer of the generated substances wrapped on the surface of LLZTO was ~5nm.

[0067] In summary, combined with EDS, XRD and TEM data, it is proved that Li2CO3 and polyvinylphosphonic acid (PVPA) reacted in this step, and no obvious Li2CO3 remained after the reaction.

[0068] In order to better understand the reaction mechanism of polyvinylphosphonic acid (PVPA) and alkaline substances on the surface of LLZTO, Figure 1The schematic diagram of the reaction mechanism of polyvinylphosphonic acid (PVPA) and Li2CO3 on the surface of LLZTO shows that Li2CO3 exists on the surface of LLZTO before modification. After modification with polyvinylphosphonic acid (PVPA), polyvinylphosphonic acid (PVPA) reacts with alkaline substances on the surface of LLZTO. On the one hand, without the barrier of Li2CO3, lithium ions can migrate better from LLZTO to the surface; on the other hand, the formed lithium ion decoupling layer acts as a link between LLZTO and LLZTO, and plays the role of a connecting buffer layer, which is equivalent to rebuilding a new ion path, allowing ions to decouple and transport more quickly inside the electrolyte.

[0069] From Table 1, Figure 5 and Figure 6 It can be seen that in Example 1 to Example 6 (when modified LLZTO powder is added to the polyvinylphosphonic acid (PVPA) matrix, as the content of the polyvinylphosphonic acid (PVPA) matrix increases (0.5%-2.5%), the room temperature ionic conductivity of the composite electrolyte film shows a trend of first increasing and then decreasing. This is mainly because when the content of the polyvinylphosphonic acid (PVPA) matrix is ​​small, the modified LLZTO can reconstruct the ion path inside the composite solid electrolyte film, and also improve the compatibility between the heterogeneous interfaces. Therefore, the room temperature ionic conductivity of the composite electrolyte film is greatly improved. When the addition amount of the polyvinylphosphonic acid (PVPA) matrix in Example 3 is 1.0%, the room temperature ionic conductivity of the composite solid electrolyte film is improved the most, and its room temperature ionic conductivity reaches 6.5×10 -3 S / cm, which is 22.4 times higher than that of the electrolyte film without the addition of polyvinylphosphonic acid (PVPA) matrix in Example 1. However, when the content of the polyvinylphosphonic acid (PVPA) matrix is ​​further increased, the particles of the modified LLZTO will agglomerate in the polymer matrix, resulting in a decrease in dispersion uniformity, which in turn has a certain blocking effect on the ion "highway", resulting in a certain degree of decrease in room temperature ionic conductivity.

[0070] Further, by Figure 7It can be seen that in Example 3, the ionic impedance of the composite electrolyte obtained by adding modified LLZTO powder to the polyvinylphosphonic acid (PVPA) matrix is ​​also the smallest. This is because the polyvinylphosphonic acid (PVPA) matrix reacts with the alkaline substances on the surface of LLZTO. At the same time, due to the presence of the polar group of -H in the structural formula of the polyvinylphosphonic acid (PVPA) matrix, the PVPA matrix also belongs to a polar molecule. At the same time, PVPA has -C=C-, so it can play a bonding role at the heterogeneous interface between LLZTO and LLZTO, forming a dense interface layer, further enhancing the connection between LLZTO and LLZTO particles, thereby reducing the physical gap caused by the different volume expansion coefficients during the charge and discharge process, which not only greatly reduces the interface resistance of mass transfer between LLZTO and LLZTO, but also effectively suppresses the internal short circuit of the electrolyte caused by the physical gap, thereby effectively improving the cycle life of the battery.

[0071] Depend on Figure 5 It can be seen that the battery assembled with the composite solid electrolyte film prepared in Example 3 can achieve a specific capacity of 453.9 mAh / g after running 100 cycles at room temperature, and the capacity retention rate is 99.93%. However, the battery assembled with the solid electrolyte film prepared in Example 1 failed after running 100 cycles at room temperature, and the discharge specific capacity decreased to 206.74 mAh / g, and the capacity retention rate was only 54.39%. It can be seen that compared with the battery assembled with the composite solid electrolyte film prepared with unmodified LLZTO, the battery assembled with the composite solid electrolyte film prepared with the modified LLZTO of the present invention has a cycle number increased by 2.2 times, a capacity retention rate increased by 45.54%, and the electrical performance of the battery has been significantly improved.

[0072] Furthermore, by comparing Example 3 with Comparative Examples 1 to 5, it can be seen that, under the same other conditions, the room temperature ionic conductivity of the composite solid electrolyte film prepared using the polyvinylphosphonic acid (PVPA) matrix is ​​significantly greater than the room temperature ionic conductivity of the composite solid electrolyte film using the poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), polyacrylonitrile (PAN), and polymethyl methacrylate (PMMA) matrix. This is because the modified LLZTO powder can reconstruct the ion pathway inside the composite solid electrolyte film, forming a faster ion "highway" inside the composite solid electrolyte film, while also improving the compatibility between heterogeneous interfaces, reducing the interface resistance of mass transfer between LLZTO and LLZTO, and greatly improving the room temperature ionic conductivity of the composite solid electrolyte film.

[0073] In summary, the battery assembled with the composite solid electrolyte film prepared by using the modified solid electrolyte of the present invention has better cycle performance, higher specific capacity and capacity retention rate than the battery assembled with the composite solid electrolyte film prepared by using the unmodified LLZTO.

[0074] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A modified solid electrolyte, characterized in that: First, garnet Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 The powder was aged in air for 2 days. 6.4 Ln3Z 1.4 Ta 0.6 O 12 A 1-2 μm thick Li2CO3 layer is formed on the powder surface to obtain modified garnet Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 Powder; then the modified garnet Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 The powder is mixed with a polyvinyl phosphonic acid solution, with a mass ratio of the modified LLZTO powder to the polyvinyl phosphonic acid in the polyvinyl phosphonic acid solution (0.1-0.2):1, and reacted at 60-80° C. for 12 hours to obtain a modified solid electrolyte.

2. The modified solid electrolyte according to claim 1, characterized in that: The polyvinyl phosphonic acid solution is obtained by dissolving polyvinyl phosphonic acid in an alcohol solvent, and the mass fraction of the polyvinyl phosphonic acid in the polyvinyl phosphonic acid solution is 95-97%.

3. The modified solid electrolyte according to claim 1, characterized in that: The alcohol solvent includes isopropyl alcohol.

4. Use of a modified solid electrolyte as described in any one of claims 1 to 3 in the preparation of an all-solid-state silicon-carbon-lithium battery.

5. An all-solid-state silicon-carbon-lithium battery, comprising a positive electrode, a negative electrode, and a composite solid electrolyte located between the positive electrode and the negative electrode, characterized in that: The composite solid electrolyte is a modified solid electrolyte film made using the modified solid electrolyte as described in any one of claims 1 to 3.

6. The all-solid-state silicon-carbon-lithium battery according to claim 5, characterized in that: The thickness of the modified solid electrolyte film is 20-50 μm.

7. The all-solid-state silicon-carbon-lithium battery according to claim 5, characterized in that: The preparation method of the modified solid electrolyte film comprises: S1, mixing polyvinylphosphonic acid with a solvent to obtain a glue solution having a polyvinylphosphonic acid concentration of 6 to 14%; S2, adding the modified solid electrolyte to the glue solution, wherein the amount of the modified solid electrolyte is 0.5-20% of the mass of the polyvinylphosphonic acid, and mixing them thoroughly to obtain a mixed slurry; S3, subjecting the mixed slurry to a film-forming treatment to obtain the composite solid electrolyte film.

8. The all-solid-state silicon-carbon-lithium battery according to claim 7, characterized in that: The solvent is one or more of isopropanol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and triethyl phosphate.

9. The all-solid-state silicon-carbon-lithium battery according to claim 7, characterized in that: The film-forming process is to place the mixed slurry on a substrate, apply it by scraping, and then remove the solvent.

10. The all-solid-state silicon-carbon-lithium battery according to claim 9, characterized in that: The solvent removal is performed by vacuum drying at 40-60°C.