Nickel-based amorphous brazing filler metal for connecting high-nitrogen steel and titanium as well as preparation method and application of nickel-based amorphous brazing filler metal

A nickel-based amorphous brazing filler metal with specific elemental composition and preparation method addresses the challenge of connecting high nitrogen steel and titanium, achieving high strength and reliable joints for composite components.

CN119057307APending Publication Date: 2024-12-03NORTH CHINA UNIV OF WATER RESOURCES & ELECTRIC POWER +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411220771.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional fusion welding methods struggle to effectively connect high nitrogen steel and titanium due to their differing physical and chemical properties, and existing brazing methods do not achieve sufficient joint strength or reliability for composite components.

Method used

A nickel-based amorphous brazing filler metal with a composition of Ni 45wt%-55wt%, Ti 10wt%-18wt%, Zr 11wt%-22wt%, Cr 10wt%-15wt%, and V 5wt%-15wt% is developed, utilizing a single-roll strip spinning method for preparation, which enhances amorphous forming ability and reduces brittle intermetallic compound formation.

Benefits of technology

The new filler metal achieves high joint strength of 550-650 MPa, with fewer brittle compounds, good wettability, and suitability for narrow gaps, facilitating lightweight and reliable connections for medical implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057307A_ABST
    Figure CN119057307A_ABST
Patent Text Reader

Abstract

The invention relates to the field of high-nitrogen steel and titanium brazing, in particular to nickel-based amorphous brazing filler metal for connecting high-nitrogen steel and titanium and a preparation method and application of the nickel-based amorphous brazing filler metal. The nickel-based amorphous brazing filler metal for connecting the high-nitrogen steel and the titanium comprises the following components in percentage by mass: 45 to 55 weight percent of Ni, 10 to 18 weight percent of Ti, 11 to 22 weight percent of Zr, 10 to 15 weight percent of Cr and 5 to 15 weight percent of V. The nickel-based amorphous brazing filler metal for connecting the high-nitrogen steel and the titanium has the advantages of being good in amorphous forming capacity, few in brittle compound formation of a brazed joint, high in joint strength and the like, and can be used for brazed connection of the high-nitrogen steel and the titanium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high nitrogen steel and titanium brazing, and in particular to a nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium, and a preparation method and application thereof. Background Art

[0002] High nitrogen steel has excellent properties such as high strength, good toughness and good corrosion resistance. It is widely used in the fields of power, marine engineering, military equipment, etc., and has unique advantages in the field of biomedical materials due to its excellent biocompatibility. Titanium is famous for its light weight, high strength, good corrosion resistance and good biocompatibility. The development of composite components of high nitrogen steel and titanium can give full play to the complementary advantages of the two in performance and economy, and has great application prospects in the fields of aerospace and medical implants. Among them, in the field of medical metal implants, it is expected to achieve lightweight design and reduce the weight of implants; it can also further improve human affinity and effectively extend the service life of interventional devices. However, due to the differences in physical and chemical properties between high nitrogen steel and titanium, traditional fusion welding is difficult to achieve effective connection between the two, and the brazing method has the advantages of being suitable for a variety of joint forms and low residual stress, becoming an effective method for welding high nitrogen steel and titanium.

[0003] At present, the research on high nitrogen steel brazing is still in its infancy, and there is even less research on high nitrogen steel / titanium metal brazing. Nickel-based brazing filler metals can provide excellent high temperature corrosion resistance and strength for joints. Among them, Ni-Cr-B-Si brazing filler metals have excellent wetting ability on the surface of austenitic stainless steel and are often used for brazing 304 or 316 stainless steel. The literature "Zhu W, Jiang H, Zhang H, et al. Microstructure and strength of high nitrogen steel joints brazed with Ni-Cr-B-Si filler [J]. Materials Science and Technology, 2018, 34 (8): 926-933." When brazing high nitrogen steel with Ni-Cr-Si-B amorphous brazing filler metal, the BN compound in the brazing seam has a significant effect on the shear strength of the joint. When the brazing temperature is 1020 ° C, the optimal shear strength of the joint is only 176.7 MPa.

[0004] High-performance nickel-based amorphous brazing filler metals for high-nitrogen steel brazing are still being explored. In order to prepare foil brazing filler metals with good amorphous forming ability, obtain high-quality and high-reliability high-nitrogen steel / titanium brazed joints, and explore the application of high-nitrogen steel / titanium medical composite human implants, it is necessary to further optimize the composition of nickel-based brazing filler metals, thereby improving the amorphous forming ability of the brazing filler metals and controlling the formation of brittle intermetallic compounds in the joints, in order to obtain safe, reliable, and long-life high-performance medical high-nitrogen steel / titanium composite components.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium, and a preparation method and application thereof. The nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium has the advantages of good amorphous forming ability, less formation of brittle compounds in the brazed joint, high joint strength, etc., and can be used for the brazing connection of high nitrogen steel and titanium.

[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0008] The first aspect of the present invention relates to a nickel-based amorphous solder for connecting high nitrogen steel and titanium, which comprises the following components by mass percentage:

[0009] Ni 45wt%-55wt%, Ti 10wt%-18wt%, Zr 11wt%-22wt%, Cr 10wt%-15wt% and V 5wt%-15wt%.

[0010] The nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium has the advantages of good amorphous forming ability, less formation of brittle compounds in the brazed joint, high joint strength, etc., and can be used for the brazing connection of high nitrogen steel and titanium.

[0011] Another aspect of the present invention also relates to a method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium, comprising the following steps:

[0012] (a) vacuum melting the raw materials to form alloy ingots;

[0013] (b) The alloy ingot is subjected to amorphous forming treatment by a single-roll strip spinning method.

[0014] The method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium is simple and feasible, easy to mass-produce and operate, and the prepared nickel-based amorphous solder has excellent performance.

[0015] Another aspect of the present invention also relates to the use of the nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium or the nickel-based amorphous brazing filler metal prepared by the preparation method of the nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium in brazing high nitrogen steel and titanium.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] (1) The nickel-based amorphous solder for connecting high nitrogen steel and titanium provided by the present invention selects the eutectic point based on the Ni-Ti binary phase diagram. The solder composition is near the Ni-Ti eutectic composition, which can reach a large supercooling zone and easily achieve "freezing" of the liquid structure, so that the solder has excellent amorphous forming ability, that is, the superplastic zone; the present invention reduces the Ti element content in the solder by atomic substitution, which can effectively reduce the formation of titanium-based brittle intermetallic compounds in the joint, and significantly improves the strength of the brazed joint to 550-650MPa.

[0018] (2) The nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium provided by the present invention has a bright surface, neat edges, uniform composition, good toughness, good wettability, etc., which is beneficial to the filling and brazing of narrow gap welded parts.

[0019] (3) The nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium provided by the present invention has a component of NiTiZrCrV series, which is different from the traditional NiCrSiB series. The Ti element in the brazing filler metal can form a good solid solution, the Zr element can reduce the melting point and improve the mechanical properties, and the V element can improve the wettability and fluidity of the brazing filler metal. There are fewer TiFe and TiFe2 brittle intermetallic compounds in the brazing seam structure, and most of them are titanium-based solid solutions, which greatly improves the shear strength of the high nitrogen steel / titanium joint.

[0020] (4) The method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium provided by the present invention is simple and feasible, easy to mass-produce and operate, and the prepared nickel-based amorphous solder has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is a macroscopic morphology of the nickel-based amorphous solder of Example 1;

[0023] Figure 2 is a DTA curve diagram of the nickel-based amorphous solder of Example 1;

[0024] Figure 3 The macroscopic morphology of the joint of high nitrogen steel and titanium metal brazed with nickel-based amorphous brazing filler metal of Example 1;

[0025] Figure 4 This is a microstructure diagram of a joint of high nitrogen steel and titanium metal brazed with nickel-based amorphous brazing filler metal according to Example 1;

[0026] Figure 5 This is an elemental surface scan of a joint of high nitrogen steel and titanium metal brazed with nickel-based amorphous brazing filler metal according to Example 1;

[0027] Figure 6 The mechanical properties of the joint of high nitrogen steel and titanium metal brazed with nickel-based amorphous brazing filler metal of Example 1 at different temperatures;

[0028] Figure 7 The microscopic morphology of the surface of the high nitrogen steel substrate after shear fracture of high nitrogen steel and titanium metal brazed by the nickel-based amorphous brazing filler metal of Example 1;

[0029] Figure 8 The microscopic morphology of the titanium metal substrate surface after shear fracture of high nitrogen steel and titanium metal brazed with the nickel-based amorphous brazing filler metal of Example 1. DETAILED DESCRIPTION

[0030] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0031] One aspect of the present invention relates to a nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium, comprising the following components by mass percentage:

[0032] Ni 45wt%-55wt%, Ti 10wt%-18wt%, Zr 11wt%-22wt%, Cr 10wt%-15wt% and V 5wt%-15wt%.

[0033] In some specific embodiments, based on mass percentage, Ni may be, for example, but not limited to, 45 wt%, 47 wt%, 49 wt%, 51 wt%, 53 wt% or 55 wt%.

[0034] In some specific embodiments, based on mass percentage, Ti may be, for example, but not limited to, 10 wt %, 12 wt %, 14 wt %, 16 wt % or 18 wt %.

[0035] In some specific embodiments, based on mass percentage, Zr may be, for example, but not limited to, 11 wt %, 12 wt %, 14 wt %, 16 wt %, 18 wt %, 20 wt % or 22 wt %.

[0036] In some specific embodiments, by mass percentage, Cr may be, for example, but not limited to, 10 wt %, 11 wt %, 12 wt %, 13 wt %, 14 wt % or 15 wt %.

[0037] In some specific embodiments, V may be, by mass percentage, for example, but not limited to, 5 wt%, 7 wt%, 9 wt%, 11 wt%, 13 wt% or 15 wt%.

[0038] The nickel-based amorphous solder for connecting high nitrogen steel and titanium provided by the present invention has a design concept of composition derived from the cluster plus connected atomic structure model, which is different from the traditional mode of experience-guided experiment and trial and error. It is a new mode of solder composition design based on theoretical prediction and experimental verification. It can effectively analyze the composition of nickel-based amorphous alloys, and provides a simple and accurate way for the composition design of multi-element nickel-based amorphous solders.

[0039] Nickel-based amorphous solder composition design: Based on the cluster + connected atom model, the Ni-Ti eutectic point is selected in the Ni-Ti binary phase diagram to obtain a high-density cluster formula of [Ni-Ti4Ni8]Ti, and the Ni and Ti atoms in the solder cluster formula are replaced by similar elements with Cr atoms, Zr atoms, and V atoms, respectively, to obtain [Ni-Ti 5-y-z Ni 8-x Cr x ]Zr y V z , x can take values ​​ranging from 1 to 3; y can take values ​​ranging from 1 to 3; z can take values ​​ranging from 1 to 2. In the present invention, the value of x is 2; the value of y is ranging from 1 to 2; the value of z is ranging from 1 to 2, and then the atomic percentage of each element is obtained, and after converting it into the mass percentage of the corresponding element, the solder composition expression Ni is obtained. a Ti b Zr c Cr d V e , wherein a is 45-55wt.%, b is 10-18wt.%, c is 11-22wt.%, d is 10-15wt.%, e is 5-15wt.%, and a+b+c+d+e=100.

[0040] The present invention selects the eutectic point based on the Ni-Ti binary phase diagram, and the solder composition is near the Ni-Ti eutectic composition, which can reach a large supercooling zone and easily realize the "freezing" of the liquid structure, so that the solder has excellent amorphous forming ability, that is, the superplastic zone; the present invention reduces the Ti element content in the solder by atomic replacement, which can effectively reduce the generation of titanium-based brittle metal compounds in the joint, and significantly improve the strength of the brazed joint, which can reach 550-650MPa.

[0041] The nickel-based solder component of the present invention is NiTiZrCrV series, which is different from the traditional NiCrSiB series. The Ti element in the solder can form a good solid solution, the Zr element can reduce the melting point and improve the mechanical properties, and the V element can improve the wettability and fluidity of the solder. There are fewer TiFe and TiFe2 brittle intermetallic compounds in the solder seam structure, and most of them are titanium-based solid solutions, which greatly improves the shear strength of the high nitrogen steel / titanium joint.

[0042] The nickel content in the nickel-based amorphous solder provided by the present invention is reduced from 82% in BNi2 to 45-55%. The significant reduction in nickel content can effectively reduce the harm caused to the human body by the dissolution of Ni in metal implants. The solder of the present invention uses the Cr element with lower density to replace the Ni element, which can achieve the lightweight and portability of the high nitrogen steel / titanium composite interventional device.

[0043] The nickel-based amorphous solder provided by the present invention is mainly used for brazing connection of high-nitrogen steel and titanium dissimilar materials, which can realize lightweight medical metal implants such as heart stents and artificial joints, and provide a basis for preparing high-reliability and high-life biomedical heterogeneous metal welding.

[0044] Furthermore, the nickel-based amorphous solder for connecting high nitrogen steel and titanium comprises the following components by mass percentage:

[0045] Ni 48wt%-52wt%, Ti 12wt%-16wt%, Zr 13wt%-20wt%, Cr 11wt%-13wt% and V 8wt%-13wt%.

[0046] Furthermore, the thickness of the nickel-based amorphous solder used to connect the high nitrogen steel and titanium is 50-60 μm.

[0047] In some specific embodiments, the thickness of the nickel-based amorphous solder for connecting high nitrogen steel and titanium may be, for example, but not limited to, 50 μm, 52 μm, 54 μm, 56 μm, 58 μm or 60 μm.

[0048] Furthermore, the melting point of the nickel-based amorphous solder used to connect the high nitrogen steel and titanium is 1035-1064°C.

[0049] In some specific embodiments, the melting point of the nickel-based amorphous brazing filler metal used to connect the high nitrogen steel to titanium may be, for example, but not limited to, 1035°C, 1040°C, 1045°C, 1050°C, 1060°C or 1064°C.

[0050] Another aspect of the present invention also relates to a method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium, comprising the following steps:

[0051] The raw materials are vacuum melted to form alloy ingots;

[0052] The alloy ingot is subjected to amorphous forming treatment by a single-roller strip-spinning method.

[0053] The method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium is simple and feasible, easy to mass-produce and operate, and the prepared nickel-based amorphous solder has excellent performance.

[0054] Furthermore, the purity of each raw material of the nickel-based amorphous solder is greater than 99.0%.

[0055] Furthermore, the vacuum smelting is performed 4 to 6 times to ensure uniform smelting of the raw materials.

[0056] Furthermore, the rotation speed of the copper roller in the single-roller belt-spinning method is 30 to 35 m / s.

[0057] In some specific embodiments, the rotation speed of the copper roller in the single-roller belt-spinning method can be, for example, but not limited to, 30 m / s, 31 m / s, 32 m / s, 33 m / s, 34 m / s or 35 m / s.

[0058] Another aspect of the present invention also relates to the use of the nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium or the nickel-based amorphous brazing filler metal prepared by the preparation method of the nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium in brazing high nitrogen steel and titanium.

[0059] The application effect of the brazing connection method of high nitrogen steel and titanium: on the one hand, high nitrogen steel is the mainstream material of medical metal implants, and the use of low-density titanium to achieve high nitrogen steel / titanium composite component connection can effectively reduce the weight of human implants and achieve lightweight and portability; on the other hand, titanium has an elastic modulus and biocompatibility similar to human bones, and the reliable connection application of the two can further improve the biocompatibility of orthopedic joint implants and extend the service life of the equipment. It can provide certain help and reference value for the development of high-performance and high-reliability high nitrogen steel / titanium medical composite implants.

[0060] Furthermore, the brazing temperature is 1050-1150°C.

[0061] In some specific embodiments, the brazing temperature may be, for example, but not limited to, 1050°C, 1060°C, 1070°C, 1080°C, 1090°C, 1100°C, 1110°C, 1120°C, 1130°C, 1140°C or 1150°C.

[0062] Furthermore, the shear strength of the brazed joint obtained by brazing is 550-650 MPa.

[0063] Furthermore, the type of the high nitrogen steel is not limited to a specific type, the titanium includes metallic titanium and / or titanium alloy, and the brazing connection method of the high nitrogen steel and titanium is applicable to all brazing connections between high nitrogen steel and titanium in the art.

[0064] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0065] Example 1

[0066] The composition design principle of nickel-based amorphous solder for connecting high nitrogen steel and titanium provided in this embodiment is as follows:

[0067] Based on the [Ni-Ti4Ni8]Ti cluster formula, two Cr atoms are used to replace two Ni atoms, one Zr atom is used to replace one Ti atom, and one V atom is used to replace one Ti atom to obtain [Ni-Ti3VNi6Cr2]Zr, and its corresponding alloy mass fraction is Ni 51.38 Ti 17.94 Zr 11.34 Cr 13.02 V 6.33 .

[0068] The method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium provided in this embodiment comprises the following steps:

[0069] 1. Weigh each element according to its mass percentage for material preparation, and the purity of the selected element should be greater than 99.0%;

[0070] 2. Mix the single elements and place them in a vacuum arc furnace for smelting, and evacuate to 5.0×10 -3 After Pa, argon gas is filled for protection, and the argon pressure is 0.05MPa. The smelting is performed at least four times to ensure uniformity;

[0071] 3. After the alloy ingot is crushed, 10g is taken and loaded into a flat quartz glass tube. Then the quartz tube is placed in the induction heating coil of the fast cooling belt throwing equipment and vacuumed to 5.0×10 -3 After Pa, argon gas is filled for protection, and the pressure of argon gas is 0.05MPa;

[0072] 4. After induction melting, the amorphous foil strip solder with a thickness of about 55 μm was prepared by spraying it onto the surface of a copper roller rotating at a speed of 33 m / s.

[0073] Figure 1 This is a macroscopic picture of the solder of this embodiment. Figure 1 It can be seen that the solder has a bright surface, neat edges and good toughness, which is conducive to filling gaps and brazing of narrow gap welds.

[0074] Figure 2 is the DTA curve of the solder of this embodiment, Figure 2 It can be seen that the melting point range of the solder is 1035~1064℃.

[0075] The nickel-based amorphous solder prepared above is used for brazing high nitrogen steel and titanium, comprising the following steps:

[0076] 1. Cut high nitrogen steel and titanium into 10×10×5mm pieces by wire cutting. 3 and 5×5×5mm 3 The sample to be welded is of size, and the surface to be welded is polished flat with 600 mesh silicon carbide sandpaper, then ultrasonically cleaned in acetone solution and dried; the high nitrogen steel model is P580 high nitrogen steel, and the chemical composition is: Mn 22wt%, Cr 20.5wt%, Ni 2.5wt%, Mo 1.5wt%, N0.75wt%, C 0.06wt% and the balance is Fe;

[0077] 2. Place the nickel-based amorphous solder between the samples to be welded to form a sandwich structure to form the welded parts;

[0078] 3. Place the parts to be welded in a vacuum brazing furnace and evacuate to 6×10 -3 Heating was started after Pa, and the mixture was heated to 800°C at 10°C / min and kept at this temperature for 10 min. Then, the mixture was heated to 1090°C at 20°C / min and kept at this temperature for 10 min. The mixture was cooled in the furnace and then taken out.

[0079] Figure 3 This is the macroscopic morphology of the high nitrogen steel / titanium brazed joint of this embodiment. It can be seen that the brazing filler metal climbs significantly on the titanium metal, has good filling ability, and is firmly bonded at the brazing seam to form an interface layer. No defects such as incomplete filling and poor forming are found.

[0080] Figure 4 This is the microstructure diagram of the high nitrogen steel / titanium brazed joint of this embodiment. It can be seen that there is obvious mutual diffusion between the brazing filler metal, high nitrogen steel and titanium, indicating that the brazing filler metal and the two base materials have good metallurgical effects, and the reaction phases in the joint structure are mostly titanium-based solid solutions, and there are fewer brittle phases such as TiFe and TiFe2, which lays the foundation for excellent mechanical properties.

[0081] Figure 5 This is an element surface scan of the high nitrogen steel / titanium brazing joint of this embodiment. The alloy elements Ni, Ti, Zr, Cr, V, and Fe in the base material and the brazing filler metal are evenly distributed in the joint area, indicating that the base material and the brazing filler metal diffuse sufficiently with no component segregation.

[0082] Example 2

[0083] The composition design principle of nickel-based amorphous solder for connecting high nitrogen steel and titanium provided in this embodiment is as follows:

[0084] Based on the [Ni-Ti4Ni8]Ti cluster formula, two Cr atoms are used to replace two Ni atoms, two Zr atoms are used to replace two Ti atoms, and one V atom is used to replace one Ti atom to obtain [Ni-Ti2VZrNi6Cr2]Zr, and its corresponding alloy mass fraction is Ni 48.68 Ti 11.36 Zr 21.64 Cr 12.33 V 6.00 .

[0085] The method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium provided in this embodiment comprises the following steps:

[0086] 1-3, same as Example 1;

[0087] 4. After induction melting, the amorphous foil strip solder with a thickness of about 50 μm was prepared by spraying it onto the surface of a copper roller rotating at a speed of 30 m / s.

[0088] The nickel-based amorphous brazing filler metal prepared above is used for brazing high nitrogen steel and titanium, comprising the following steps:

[0089] 1-2, same as Example 1;

[0090] 3. Place the parts to be welded in a vacuum brazing furnace and evacuate to 6×10 -3 Heating was started after Pa, and the mixture was heated to 800°C at 10°C / min and kept at this temperature for 10 min. Then, the mixture was heated to 1060°C at 20°C / min and kept at this temperature for 10 min. The mixture was cooled in the furnace and then taken out.

[0091] Example 3

[0092] The composition design principle of nickel-based amorphous solder for connecting high nitrogen steel and titanium provided in this embodiment is as follows:

[0093] Based on the [Ni-Ti4Ni8]Ti cluster formula, two Cr atoms are used to replace two Ni atoms, one Zr atom is used to replace one Ti atom, and two V atoms are used to replace two Ti atoms to obtain [Ni-Ti2V2Ni6Cr2]Zr, and its corresponding alloy mass fraction is Ni 51.14 Ti 11.92 Zr 11.29 Cr 12.96 V 12.69 .

[0094] The method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium provided in this embodiment comprises the following steps:

[0095] 1-3, same as Example 1;

[0096] 4. After induction melting, the amorphous foil strip solder with a thickness of about 60 μm was prepared by spraying it onto the surface of a copper roller rotating at a speed of 35 m / s.

[0097] The nickel-based amorphous solder prepared above is used for brazing high nitrogen steel and titanium, comprising the following steps:

[0098] 1-2, same as Example 1;

[0099] 3. Place the parts to be welded in a vacuum brazing furnace and evacuate to 6×10 -3 Heating was started after Pa, and the mixture was heated to 800°C at 10°C / min and kept at this temperature for 10 min. Then, the mixture was heated to 1090°C at 20°C / min and kept at this temperature for 20 min. The mixture was cooled in the furnace and then taken out.

[0100] Comparative Example 1

[0101] Conventional nickel-based amorphous solder (brand: BNi2, main components Ni-Cr7-Si4.5-B3.2-Fe3, wt%), brazing method is the same as Example 1.

[0102] Comparative Example 2

[0103] The Ni-Ti based amorphous solder provided in this comparative example comprises the following components by weight percentage:

[0104] Ni 55.01wt%, Ti 5.61wt%, Zr 21.37wt%, Cr 6.09wt% and V 11.92wt%.

[0105] The preparation method of the brazing filler metal and the method for brazing high nitrogen steel and titanium are the same as those in Example 1.

[0106] Experimental Example 1

[0107] Brazing performance test: A universal testing machine was used to perform compression shear tests on high nitrogen steel / titanium joints brazed at different temperatures with the nickel-based brazing filler material of Example 1 of the present invention to evaluate the shear performance of the brazed joints. Three brazed joints were selected for shear tests under different process parameters, and the average value of the three samples was taken.

[0108] Figure 6 This is a graph showing the change in mechanical properties of a high nitrogen steel / titanium metal joint brazed with nickel-based amorphous brazing filler metal of Example 1 of the present invention at different temperatures for 10 minutes. As can be seen from the figure, with increasing temperature, the shear strength first increases and then decreases, and at 1090°C the shear strength reaches a peak value of 605.23 MPa.

[0109] Figure 7 and Figure 8This is the surface fracture morphology of the two base materials after shear fracture in Example 1 of the present invention. It can be seen from the figure that there are obvious cleavage steps and river patterns on the surfaces of the two base materials, showing a typical brittle fracture mode.

[0110] Experimental Example 2

[0111] The shear strength of the brazed joints obtained by brazing in each embodiment and comparative example was tested, and the results are shown in Table 1.

[0112] Table 1

[0113] Shear strength / MPa Example 2 593.56 Example 3 582.92 Comparative Example 1 176.7 Comparative Example 2 450.8

[0114] By comparison, it was found that when the brazing filler metal of the embodiment of the present invention was used for brazing high nitrogen steel / titanium heterogeneous joints, the shear strength was higher than that of the control example. The excellent mechanical properties of the nickel-based amorphous brazing filler metal for brazing high nitrogen steel and titanium provided by the present invention are helpful to improve the service life and service time of medical metal high nitrogen steel / titanium functional composite implants.

[0115] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium, characterized in that: Calculated by mass percentage, it includes the following components: Ni 45wt%-55wt%, Ti 10wt%-18wt%, Zr 11wt%-22wt%, Cr 10wt%-15wt% and V 5wt%-15wt%.

2. The nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium according to claim 1, characterized in that: Calculated by mass percentage, it includes the following components: Ni 48wt%-52wt%, Ti 12wt%-16wt%, Zr 13wt%-20wt%, Cr 11wt%-13wt% and V 8wt%-13wt%.

3. The nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium according to claim 1 or 2, characterized in that: The thickness of the nickel-based amorphous solder used for connecting the high nitrogen steel and titanium is 50-60 μm.

4. The nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium according to claim 1 or 2, characterized in that: The melting point of the nickel-based amorphous solder used for connecting the high nitrogen steel and titanium is 1035-1064°C.

5. The method for preparing a nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium according to any one of claims 1 to 4, characterized in that: The following steps are involved: (a) vacuum melting the raw materials to form alloy ingots; (b) The alloy ingot is subjected to amorphous forming treatment by a single-roll strip spinning method.

6. The method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium according to claim 5, characterized in that: The vacuum melting is performed 4 to 6 times.

7. The method for preparing the nickel-based amorphous solder for connecting high nitrogen steel and titanium according to claim 5, characterized in that: The copper roller rotation speed of the single roller belt throwing method is 30-35 m / s.

8. Use of the nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium as described in any one of claims 1 to 4 or the nickel-based amorphous brazing filler metal for connecting high nitrogen steel and titanium as described in any one of claims 5 to 7 in brazing high nitrogen steel and titanium.

9. The use according to claim 8, characterized in that: The brazing temperature is 1050-1150°C.

10. The use according to claim 8, characterized in that: The shear strength of the brazed joint obtained by the brazing is 550-650 MPa.