Method for extracting and separating lithium

By introducing carbonyl compounds containing alkoxy groups into neutral phosphorus extractants and combining transition metals, the lithium extraction rate and separation coefficient of low lithium concentration and high magnesium lithium are solved in the prior art compared with salt lake brine. The problem of efficient lithium separation and cost reduction has been achieved.

CN119061266APending Publication Date: 2024-12-03GRIREM ADVANCED MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310608254.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively extract lithium from salt lake brines with low lithium concentration and high magnesium-lithium ratio. Especially when most salt lakes in China have high magnesium-lithium ratio, the existing extraction system is at low lithium concentration. The extraction rate and separation coefficient decreased significantly.

Method used

Introducing carbonyl compounds containing alkoxy groups as collagens into neutral phosphorus extractants, enhancing the selective coordination ability of the mixed extractant and lithium ions, and combining the use of diluents and transition metals, through countercurrent extraction or Fractionation and extraction can achieve efficient separation of lithium.

Benefits of technology

It significantly improves the extraction rate of lithium and the separation coefficient of lithium magnesium, and is suitable for solutions with different lithium concentrations and magnesium-lithium ratios, reducing the cost of lithium extraction, and reducing the swelling and corrosion of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a method for extracting and separating lithium, a solution containing lithium and magnesium and an organic phase containing a mixed extractant are mixed for extraction reaction, then phase separation is performed to obtain a lithium-loaded organic phase and raffinate, and the organic phase containing the mixed extractant comprises a neutral phosphorus extractant, a synergistic extractant and a diluent; and carrying out reverse extraction on the lithium-loaded organic phase through an acid solution or water to obtain a lithium-enriched liquid product. A synergistic extraction agent (a carbonyl compound containing an alkoxy group) is introduced into a neutral phosphorus extraction agent, the alkoxy group connected with the carbonyl group in the synergistic extraction agent can effectively improve the electron cloud density of the carbonyl group, the selective coordination capacity of the mixed extraction agent and lithium ions is enhanced, and then the extraction rate of lithium in a lithium-containing solution and the lithium-magnesium separation coefficient are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium extraction, and in particular to a method for extracting and separating lithium. Background Art

[0002] Lithium and its compounds can be used in batteries, ceramics and glass, lubricants, air treatment, continuous casting mold flux powder, polymer production and other fields. In recent years, with the rapid development of new energy vehicles, especially electric vehicles, the demand for lithium, the core material of secondary batteries, has surged, and the development and utilization of lithium resources has become a focus of common concern in all countries. my country's lithium resources mainly exist in the form of ores and salt lake brines, of which salt lake lithium resources account for about 85%. Although my country's salt lake lithium resources are rich, the production of salt lake lithium salts only accounts for 22%, and the comprehensive productivity is not advantageous. The main reason is that the magnesium-lithium ratio in most of my country's salt lake brines is high. Due to the similar chemical properties of lithium and magnesium, lithium and magnesium separation is difficult, and the existing process is difficult to extract and separate lithium economically and efficiently.

[0003] The extraction method has the advantages of low energy consumption, continuous operation, simple equipment, and large production volume. It is considered to be one of the most promising methods for separating and extracting lithium from salt lake brine with a high magnesium-lithium ratio. At present, the most commonly used extractant is a neutral phosphorus extractant (tributyl phosphate, TBP) as an extractant and ferric chloride as an additive. Li is co-extracted into the organic phase in the form of LiFeCl4 to achieve its separation from Mg and other impurities in the salt lake brine.

[0004] With the application and development of TBP extraction system, the disadvantage of single TBP extraction system for lithium-magnesium separation in high magnesium-lithium ratio salt lake has gradually emerged. Researchers have carried out a large number of studies on mixed extraction systems based on TBP. For example, TBP-methyl isobutyl ketone (MIBK) mixed extraction system was used to extract lithium from brine with a magnesium-lithium ratio of 68 and a lithium concentration of 1.67 g / L. Under the condition of an iron-lithium molar ratio of 1.5, the lithium extraction rate reached 91.2% and the lithium-magnesium separation coefficient reached 483.05; TBP-N,N-di(2-ethyl)-1,4-diol was used to extract lithium from brine with a magnesium-lithium ratio of 68 and a lithium concentration of 1.67 g / L. The mixed extraction system of TBP-2-ethylhexyl phosphate mono-2-ethylhexyl ester (P507) was used to extract lithium from a solution with a magnesium-lithium ratio of 140 and a lithium concentration of 0.69 g / L. The lithium extraction rate was 63%, and the lithium-magnesium separation factor was 87.

[0005] The above shows that when the TBP mixed extraction system treats brine with higher lithium concentration and higher magnesium-lithium ratio, its lithium extraction rate is higher than that of the single TBP extraction system, and the lithium-magnesium separation coefficient also increases to a certain extent. However, as the magnesium-lithium ratio increases and the lithium concentration decreases, the lithium extraction rate and lithium-magnesium separation coefficient both drop significantly. However, there are few reports on the use of mixed extraction systems based on neutral phosphorus extractants to treat salt lake brines with low lithium concentration and high magnesium-lithium ratio. Most of my country's salt lakes are high magnesium-lithium ratio salt lakes, and there is an urgent need to develop new mixed extraction systems and extraction technologies for extracting and separating lithium from solutions with low lithium concentration and high magnesium-lithium ratio. Summary of the invention

[0006] The purpose of the present invention is to provide a method for extracting and separating lithium, by introducing a synergist (a carbonyl compound containing an alkoxy group) into a neutral phosphorus extractant, the alkoxy group connected to the carbonyl group in the synergist can effectively increase the electron cloud density of the carbonyl group, enhance the selective coordination ability of the mixed extractant with lithium ions, and thus improve the extraction rate of lithium in a lithium-containing solution and the lithium-magnesium separation coefficient.

[0007] In order to solve the above technical problems, the present invention provides a method for extracting and separating lithium, comprising the following steps:

[0008] A solution containing lithium and magnesium and an organic phase containing a mixed extractant are mixed for extraction reaction and then phase separated to obtain an organic phase loaded with lithium and a raffinate containing magnesium, thereby achieving lithium-magnesium separation. The organic phase containing the mixed extractant includes: a neutral phosphorus extractant, a co-extractant and a diluent.

[0009] Further, the neutral phosphorus extractant includes: tributyl phosphate and / or dimethylheptyl methyl phosphate (P350);

[0010] The co-extractant includes: a carbonyl compound containing an alkoxy group;

[0011] The volume ratio of the neutral phosphorus extractant to the co-extractant is 1:3 to 10:1;

[0012] Preferably, the volume ratio of the neutral phosphorus extractant to the co-extractant is 1:1 to 5:1.

[0013] Further, the carbonyl compound containing an alkoxy group includes: monoalkoxy esters and / or dialkoxy carbonates;

[0014] The monoalkoxy ester comprises at least one of ethyl acetate, butyl acetate, ethyl butyrate, butyl butyrate and dioctyl phthalate;

[0015] The bis-alkoxy carbonate comprises at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, dibutyl carbonate, chloromethyl isopropyl carbonate, tert-butylphenyl carbonate and allyl methyl carbonate;

[0016] Preferably, the bis-alkoxy carbonate includes: diethyl carbonate and / or dipropyl carbonate.

[0017] Further, the diluent includes: at least one of sulfonated kerosene, 260# solvent oil, 2-octanol, 4-methyl-2-pentanone and diisobutyl ketone;

[0018] The volume percentage of the diluent in the organic phase is 20% to 70%;

[0019] Preferably, the diluent includes: sulfonated kerosene and / or 260# solvent oil, and the volume percentage of the diluent to the organic phase is 30% to 50%.

[0020] Furthermore, an additive is added during the mixing process of the lithium- and magnesium-containing solution and the organic phase containing the mixed extractant;

[0021] The additive comprises: at least one of chloride, sulfate and nitrate of transition metal;

[0022] Preferably, the additive includes at least one of ferric chloride, cupric chloride, zinc chloride, manganese sulfate and nickel chloride.

[0023] Furthermore, the molar ratio of the additive to the lithium metal ions in the lithium-magnesium containing solution is 1:1 to 2:1.

[0024] Furthermore, the lithium concentration in the lithium-magnesium solution is 0.01 g / L to 10 g / L, and the magnesium-lithium concentration ratio is 1:1 to 1500:1;

[0025] Preferably, the lithium concentration of the lithium-magnesium solution is 0.05 g / L to 5 g / L, and the magnesium-lithium concentration ratio is 30:1 to 400:1.

[0026] Furthermore, the volume ratio of the organic phase containing the mixed extractant to the lithium- and magnesium-containing solution is 1:30 to 10:1, preferably 1:20 to 5:1.

[0027] Furthermore, the extraction method includes at least one of countercurrent extraction, parallel current extraction, cross current extraction and fractional extraction;

[0028] Preferably, the extraction method includes: countercurrent extraction and / or fractional extraction.

[0029] Furthermore, the extraction stages are 3 to 30, preferably 5 to 15; the mixing time of the extraction process is 10 sec to 30 min, preferably 30 sec to 10 min;

[0030] Furthermore, the method for extracting and separating lithium also includes the following steps:

[0031] The lithium-loaded organic phase is stripped with an acid solution or water to obtain a lithium-enriched liquid product.

[0032] Further, the acid solution includes: at least one of nitric acid, phosphoric acid, hydrochloric acid and sulfuric acid;

[0033] The H + The molar concentration is 1 mol / L to 10 mol / L;

[0034] Preferably, the acid solution comprises: hydrochloric acid;

[0035] Preferably, the H of the acid solution + The molar concentration is 3mol / L~6mol / L.

[0036] Furthermore, the stripping stage number is 3 to 30, preferably 5 to 15; the mixing time of the stripping process is 10 sec to 30 min, preferably 30 sec to 10 min.

[0037] The above technical solution of the embodiment of the present invention has the following beneficial technical effects:

[0038] By introducing a synergist (a carbonyl compound containing an alkoxy group) into a neutral phosphorus extractant, the alkoxy group connected to the carbonyl group in the synergist can effectively increase the electron cloud density of the carbonyl group, enhance the selective coordination ability of the mixed extractant with lithium ions, and thereby improve the lithium extraction rate and lithium-magnesium separation coefficient in the lithium-containing solution. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0040] Solvent extraction has the advantages of high efficiency, strong continuity, simple operation, and small fixed asset investment. It has been rapidly developed in the application of lithium extraction from salt lake brine with a high magnesium-to-lithium ratio. At present, the industry mainly uses tributyl phosphate extraction system to extract lithium from salt lake brine with a high magnesium-to-lithium ratio. At the same time, in order to reduce the swelling corrosion of high-concentration tributyl phosphate on the equipment and reduce the stripping acidity, methyl isobutyl ketone, N, N-di(2-ethylhexyl)-3-butanone acetamide, ethyl butyrate, dioctyl phthalate and other co-extractants are generally added to tributyl phosphate to reduce the concentration of tributyl phosphate and stripping acid. By adding the above-mentioned co-extractants, the scope of application of salt lake brine treatment has been expanded to a certain extent (higher lithium concentration, higher magnesium-to-lithium ratio), and the lithium extraction rate and lithium-magnesium separation coefficient have been improved. However, it is still difficult to meet the application needs of lithium extraction from salt lakes (low lithium concentration, high magnesium-to-lithium ratio) in my country, resulting in the obstruction of large-scale promotion and application.

[0041] Therefore, in order to solve the above-mentioned problem of extracting lithium from lithium-containing salt lake brine, in a typical embodiment of the present application, a method for extracting and separating lithium from a lithium-containing and magnesium-containing solution is provided, comprising the following steps:

[0042] A solution containing lithium and magnesium and an organic phase containing a mixed extractant are mixed for extraction reaction and then phase separated to obtain an organic phase loaded with lithium and a raffinate containing magnesium, thereby achieving lithium-magnesium separation. The polar phase composition includes: a neutral phosphorus extractant, a co-extractant and a diluent.

[0043] In the above method, the neutral phosphorus extractant includes: tributyl phosphate and / or dimethylheptyl methyl phosphate; the synergist includes: a carbonyl compound containing an alkoxy group. Among them, the volume ratio of the neutral phosphorus extractant to the synergist is 1:3 to 10:1. Preferably, the volume ratio of the neutral phosphorus extractant to the synergist is 1:1 to 5:1. By adding a carbonyl compound containing an alkoxy group, the electron cloud density of the carbonyl group can be effectively increased, and the selective coordination ability of the mixed extractant with lithium ions can be enhanced, thereby increasing the extraction rate of lithium in lithium- and magnesium-containing solutions, and at the same time, the lithium-magnesium separation coefficient can be effectively increased. In addition, the added synergist can also reduce the concentration of the neutral phosphorus extractant and reduce its swelling corrosion to the equipment.

[0044] Furthermore, the carbonyl compound containing an alkoxy group includes: monoalkoxy esters and / or dialkoxy carbonates. The monoalkoxy esters include: at least one of ethyl acetate, butyl acetate, ethyl butyrate, butyl butyrate and dioctyl phthalate; the dialkoxy carbonates include: at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, dibutyl carbonate, chloromethyl isopropyl carbonate, tert-butylphenyl carbonate and allyl methyl carbonate, preferably diethyl carbonate and / or dipropyl carbonate. When the alkoxy group is connected to the carbonyl compound, the oxygen atom and the carbonyl compound can form a p-π conjugation, so that the electron cloud density on the carbonyl group increases. By introducing an electron-donating carbonyl co-extractant, the selective coordination ability of the neutral phosphorus extractant for lithium ions can be effectively improved.

[0045] In the above method, the diluent includes at least one of sulfonated kerosene, 260# solvent oil, 2-octanol, 4-methyl-2-pentanone and diisobutyl ketone; the volume percentage of the diluent in the organic phase is 20% to 70%. Preferably, the diluent includes sulfonated kerosene and / or 260# solvent oil, and the volume percentage of the diluent in the organic phase is 30% to 50%. By adding the diluent to the mixed extractant, within the concentration range, the organic phase containing the mixed extractant has a relatively high fluidity, and is more fully in contact with the lithium and magnesium solution, which can effectively improve the mass transfer efficiency of the extraction process. In addition, the concentration and density of the neutral phosphorus extractant can also be further reduced, which can not only reduce the swelling corrosion of the equipment, but also facilitate the oil-water two-phase separation.

[0046] In the above method, additives are added during the mixing process of the lithium-containing and magnesium-containing solutions and the mixed extractants. Specifically, the additives include at least one of chlorides, sulfates and nitrates of transition metals; preferably, the additives include at least one of ferric chloride, copper chloride, zinc chloride, manganese sulfate and nickel chloride. When a neutral phosphorus extractant is used alone to extract and separate lithium, the extraction rate of lithium is low. However, when an appropriate amount of transition metal is added to the lithium-containing and magnesium-containing solution, the transition metal (Me n+ ) can react with Cl in lithium and magnesium solutions - Complexation to form [MeCl n+1 ] - ions, which can react with Li + They are extracted at the same time, thereby effectively improving the extraction rate of lithium.

[0047] Specifically, the molar ratio of the transition metal to the lithium in the lithium- and magnesium-containing solution is 1:1 to 2:1. Within this molar ratio range, the lithium and transition metal are in the form of LiMeCl n+1 can be extracted simultaneously in the form of , which can effectively improve the extraction rate of lithium.

[0048] Specifically, the lithium concentration in the lithium-containing and magnesium-containing solution is 0.01 g / L to 10 g / L, and the magnesium-lithium ratio is 1:1 to 1500:1; preferably, the lithium concentration is 0.05 g / L to 5 g / L, and the magnesium-lithium ratio is 30:1 to 400:1. The mixed extractant in the present application is suitable for extracting and separating lithium from lithium-containing and magnesium-containing solutions with different lithium concentrations and magnesium-lithium ratios, and is particularly suitable for treating lithium-containing and magnesium-containing solutions with low lithium concentrations and high magnesium-lithium ratios, and the lithium extraction rate and lithium-magnesium separation coefficient are significantly improved compared with the existing TBP mixed extraction system, thereby effectively improving the lithium recovery rate and reducing the cost of lithium extraction.

[0049] In the above method, the volume ratio of the mixed extractant to the lithium- and magnesium-containing solution is 1:30 to 10:1, preferably 1:20 to 5:1.

[0050] The above-mentioned extraction method includes: at least one of countercurrent extraction, parallel current extraction, cross current extraction and fractional extraction. Specifically, the number of extraction stages is 3 to 30, and the mixing time of the extraction process is 10 seconds to 30 minutes. The extraction equipment includes: at least one of a mixing and settling tank, a centrifugal extractor and an extraction tower.

[0051] In order to improve the extraction rate of lithium and the separation coefficient of lithium and magnesium, in another preferred embodiment of the present application, the extraction method includes countercurrent extraction and / or fractional extraction, the extraction level is 5 to 15, and the mixing time is 30 sec to 10 min. By adopting countercurrent extraction and / or fractional extraction methods, by increasing the extraction level and extending the mixing time, the oil-water two-phase contact mass transfer can be strengthened, so that the extraction and separation of lithium can be fully carried out, thereby improving the extraction rate of lithium and the separation coefficient of lithium and magnesium, but increasing the extraction level will increase the equipment investment, so the extraction level is preferably 5 to 15. At the same time, according to the different volume ratios of the mixed extractant and the lithium- and magnesium-containing solutions, in order to achieve efficient extraction and separation of lithium, the mixing time is preferably 30 sec to 10 min.

[0052] The above method further comprises the following step: using an acid solution or water to strip the organic phase loaded with lithium to obtain a lithium-enriched solution.

[0053] Specifically, the acid solution includes at least one of nitric acid, phosphoric acid, hydrochloric acid and sulfuric acid; + The molar concentration is 1 to 8 mol / L. Preferably, the acid solution comprises: hydrochloric acid; + The molar concentration is 3~6mol / L.

[0054] Specifically, the number of stripping stages is 3 to 30, preferably 5 to 15; the mixing time of the stripping process is 10 sec to 30 min, preferably 30 sec to 10 min.

[0055] Due to H + With [MeCl n+1] - The stability of the extractant formed by combining with neutral phosphorus extractants is better than that of Li + , H + Stripping of Li from mixed extractants loaded with lithium + In order to completely strip the Li in the lithium-loaded mixed extractant as much as possible + It is preferred to use hydrochloric acid solution for stripping, with stripping stages of 5 to 15 and stripping time of 30 sec to 10 min.

[0056] The method for extracting and separating lithium of the present invention is described in detail with reference to several embodiments below:

[0057] Example 1 (Comparative Example)

[0058] The lithium-containing and magnesium-containing solution (Li concentration of 278 mg / L, magnesium-lithium ratio of 370) and the organic phase containing the mixed extractant (40% TBP + 20% methyl isobutyl ketone + 40% 260# solvent oil) were mixed, and the FeCl3 additive was added at the same time, and the iron-lithium molar ratio was controlled to be 1.5:1, and the O / A ratio was 1:3. After mixing for 300 seconds, the phases were separated to obtain the organic phase loaded with lithium and the raffinate containing magnesium. At this time, the single-stage extraction rate of lithium was 53.6%, and the lithium-magnesium separation factor was 172.

[0059] Examples 2 to 4 (comparative examples) are shown in Table 1, and the operating steps are the same as above.

[0060] Example 5

[0061] The lithium-containing and magnesium-containing solution (Li concentration of 278 mg / L, magnesium-lithium ratio of 370) and the organic phase containing the mixed extractant (40% TBP + 20% DEC + 40% 260# solvent oil) were mixed, and the FeCl3 additive was added at the same time, and the iron-lithium molar ratio was controlled to be 1.5:1, and the O / A ratio was 1:3. After mixing for 300 seconds, the phases were separated to obtain the organic phase loaded with lithium and the raffinate containing magnesium. At this time, the single-stage extraction rate of lithium was 66.0%, and the lithium-magnesium separation factor was 318.

[0062] Examples 6 to 67 are shown in Tables 2 and 3, and the operating steps are the same as above.

[0063] Embodiment 68

[0064] The lithium-containing and magnesium-containing solution (Li concentration of 800 mg / L, magnesium-lithium ratio of 370) and the organic phase containing the mixed extractant (40% TBP + 20% DEC + 40% 260# solvent oil) were mixed, and FeCl3 additive was added at the same time, and the iron-lithium molar ratio was controlled to be 1.5:1, and the O / A ratio was 1:2. Four-stage countercurrent extraction was adopted, and phase separation was performed after single-stage mixing for 300 seconds to obtain the organic phase loaded with lithium and the raffinate containing magnesium. At this time, the extraction rate of lithium was 98.1%.

[0065] Examples 69 to 73 are shown in Table 4, and the operating steps are the same as above.

[0066] Embodiment 74

[0067] The lithium-containing and magnesium-containing solution (Li concentration of 278 mg / L, magnesium-lithium ratio of 370) and the organic phase containing the mixed extractant (40% TBP+20% DEC+40% 260# solvent oil) were mixed, and FeCl3 additive was added at the same time, the iron-lithium molar ratio was controlled to be 1.4:1, and the O / A ratio was 1:5. A three-stage countercurrent extraction was adopted, and the phase separation was performed after single-stage mixing for 300 sec to obtain the organic phase loaded with lithium and the raffinate containing magnesium. The organic phase loaded with lithium was stripped with 6 mol / L hydrochloric acid, and the stripping ratio was O / A=10:1, and the single-stage stripping rate of lithium was 68.2%.

[0068] Examples 75 to 95 are shown in Tables 5 and 6, and the operating steps are the same as above.

[0069] Embodiment 96

[0070] The lithium-containing and magnesium-containing solution (Li concentration of 278 mg / L, magnesium-lithium ratio of 370) and the organic phase containing the mixed extractant (40% TBP+20% DEC+40% 260# solvent oil) were mixed, and FeCl3 additives were added at the same time, the iron-lithium molar ratio was controlled to be 1.5:1, and the O / A ratio was 1:4. Six-stage countercurrent extraction and three-stage countercurrent washing were adopted, and the washing liquid was a lithium chloride-containing aqueous solution to obtain an organic phase loaded with lithium and a raffinate containing magnesium. The lithium concentration in the organic phase was 1.09 g / L, and the lithium extraction rate was more than 98%. The organic phase loaded with lithium was stripped with 6 mol / L hydrochloric acid, the stripping ratio was O / A=10:1, and five-stage countercurrent stripping was adopted, and the stripping rate of lithium was 97.3%.

[0071] Examples 97 to 105 are shown in Table 7, and the operating steps are the same as above.

[0072] Table 1 (single-stage extraction, mixing time 300 sec)

[0073]

[0074] Table 2 (single-stage extraction, mixing time 300 sec)

[0075]

[0076]

[0077]

[0078]

[0079]

[0080] Table 3 (single-stage extraction, mixing time variation)

[0081]

[0082]

[0083] Table 4 (multi-stage countercurrent extraction, mixing time 300 sec)

[0084]

[0085] Table 5 (3-stage countercurrent extraction, mixing time 300 sec; single-stage stripping, stripping mixing time 500 sec)

[0086]

[0087]

[0088]

[0089] Table 6 (3-stage countercurrent extraction, mixing time 300 sec; single-stage stripping)

[0090]

[0091] Table 7 (6-stage countercurrent extraction, 3-stage countercurrent washing, 8-stage countercurrent stripping, mixing time 300 sec)

[0092]

[0093]

[0094] The embodiment of the present invention aims to protect a method for extracting and separating lithium, wherein a lithium-containing solution and an active phase containing a mixed extractant are mixed for extraction reaction and then phase separated to obtain an organic phase loaded with lithium and a raffinate, wherein the organic phase composition includes: a neutral phosphorus extractant, a synergist and a diluent. The above technical solution has the following effects:

[0095] By introducing a synergist (a carbonyl compound containing an alkoxy group) into a neutral phosphorus extractant, the alkoxy group connected to the carbonyl group in the synergist can effectively increase the electron cloud density of the carbonyl group, enhance the selective coordination ability of the extractant with lithium ions, and thereby improve the lithium extraction rate and lithium-magnesium separation coefficient in the lithium-containing solution.

[0096] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. A method for extracting and separating lithium, characterized in that: The steps include: The lithium- and magnesium-containing solutions and the organic phase containing the mixed extractant are mixed for extraction reaction and then phase separated to obtain the lithium-loaded organic phase and the magnesium-containing raffinate, thereby achieving lithium-magnesium separation. The organic phase containing the mixed extractant comprises: a neutral phosphorus extractant, a co-extractant and a diluent.

2. The method for extracting and separating lithium according to claim 1, characterized in that: The neutral phosphorus extractant includes: tributyl phosphate and / or dimethylheptyl methyl phosphate; The co-extractant includes: a carbonyl compound containing an alkoxy group; The volume ratio of the neutral phosphorus extractant to the co-extractant is 1:3 to 10:1; Preferably, the volume ratio of the neutral phosphorus extractant to the co-extractant is 1:1 to 5:

1.

3. The method for extracting and separating lithium according to claim 2, characterized in that: The carbonyl compound containing an alkoxy group includes: monoalkoxy esters and / or dialkoxy carbonates; The monoalkoxy ester comprises at least one of ethyl acetate, butyl acetate, ethyl butyrate, butyl butyrate and dioctyl phthalate; The bis-alkoxy carbonate comprises at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, dibutyl carbonate, chloromethyl isopropyl carbonate, tert-butylphenyl carbonate and allyl methyl carbonate; Preferably, the bis-alkoxy carbonate includes: diethyl carbonate and / or dipropyl carbonate.

4. The method for extracting and separating lithium according to claim 1, characterized in that: The diluent comprises: at least one of sulfonated kerosene, 260# solvent oil, 2-octanol, 4-methyl-2-pentanone and diisobutyl ketone; The volume percentage of the diluent in the organic phase is 20% to 70%; Preferably, the diluent includes: sulfonated kerosene and / or 260# solvent oil, and the volume percentage of the diluent in the organic phase is 30% to 50%.

5. The method for extracting and separating lithium according to claim 1, characterized in that: Adding additives during the mixing process of the lithium- and magnesium-containing solution and the organic phase containing the mixed extractant; The additive comprises: at least one of chloride, sulfate and nitrate of transition metal; Preferably, the additive includes at least one of ferric chloride, cupric chloride, zinc chloride, manganese sulfate and nickel chloride.

6. The method for extracting and separating lithium according to claim 5, characterized in that: The molar ratio of the additive to the lithium metal ions in the lithium-magnesium containing solution is 1:1 to 2:

1.

7. The method for extracting and separating lithium according to claim 1, characterized in that: The lithium concentration of the lithium-magnesium solution is 0.01 g / L to 10 g / L, and the magnesium-lithium concentration ratio is 1:1 to 1500:1; Preferably, the lithium concentration of the lithium-magnesium solution is 0.05 g / L to 5 g / L, and the magnesium-lithium concentration ratio is 30:1 to 400:

1.

8. The method for extracting and separating lithium according to claim 1, characterized in that: The volume ratio of the organic phase containing the mixed extractant to the lithium- and magnesium-containing solution is 1:30 to 10:1, preferably 1:20 to 5:

1.

9. The method for extracting and separating lithium according to any one of claims 1 to 8, characterized in that: The extraction method includes at least one of countercurrent extraction, parallel current extraction, cross current extraction and fractional extraction; Preferably, the extraction method includes: countercurrent extraction and / or fractional extraction.

10. The method for extracting and separating lithium according to claim 9, characterized in that: The extraction stages are 3 to 30, preferably 5 to 15; The mixing time of the extraction process is 10 sec to 30 min, preferably 30 sec to 10 min.

11. The method for extracting and separating lithium according to any one of claims 1 to 8, characterized in that: The following steps are also included: The lithium-loaded organic phase is stripped with an acid solution or water to obtain a lithium-enriched liquid product.

12. The method for extracting and separating lithium according to claim 11, characterized in that: The acid solution comprises: at least one of nitric acid, phosphoric acid, hydrochloric acid and sulfuric acid; The H + The molar concentration is 1 mol / L to 10 mol / L; Preferably, the acid solution comprises: hydrochloric acid; Preferably, the H of the acid solution + The molar concentration is 3mol / L~6mol / L.

13. The method for extracting and separating lithium according to claim 11, characterized in that: The stripping stage number is 3 to 30, preferably 5 to 15; The mixing time of the stripping process is 10 sec to 30 min, preferably 30 sec to 10 min.

Citation Information

Cited By

  • Method for comprehensively recovering lithium, sodium, potassium, magnesium and boron resources in original halogen

    CN121496198A