Dynamic isomerism reinforced transformation induced plasticity alloy and preparation method thereof

By regulating the layer error energy and grain size of the austenite phase, and optimizing the coordinated strengthening of TRIP and DHDI, the problems of cracking and insufficient performance during the molding of traditional TRIP alloys are solved, and high-strength, elongation and strong plasticization alloys are obtained. , suitable for automotive body and other structural parts.

CN119061329APending Publication Date: 2024-12-03CENT OF EXCELLENCE FOR ADVANCED MATERIALS +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411188022.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional phase transition-induced plasticity (TRIP) alloys are prone to cracking problems during molding, and their plasticity and toughness are insufficient, making it difficult to meet the requirements of impact resistance of structural parts such as automobile bodies. The high content and complexity of existing stainless steel TRIP alloys The process limits its wide application.

Method used

Through the coordinated regulation of alloy raw materials, composition ratio, processing technology and parameters, the layer error energy and grain size of the austenite phase are adjusted, and alloys with austenite and martensite biphasic structures are prepared to optimize dynamic heterogeneity (DHDI) and TRIP synergistic strengthening to obtain high strength, elongation and large-strength plasticization alloys.

Benefits of technology

It has achieved the improvement of the high strength, elongation and strong plasticization performance of the alloy, simplified production processes and equipment, reduced costs, broadened the alloy processing technology window, and met the performance requirements of structural parts such as automobile bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061329A_ABST
    Figure CN119061329A_ABST
Patent Text Reader

Abstract

The invention relates to a dynamic isomerism strengthened transformation induced plasticity alloy. The alloy comprises the following components in percentage by mass: 68-73% of Fe, 19-24% of Cr, 8-13% of Ni and the balance of Fe. A metallographic structure is a double-phase structure containing austenite and martensite, the austenite is used as a main part before stretching, the volume fraction of the austenite is 90-100%, and the volume fraction of the martensite is 0-10%; after stretching, the volume fraction of austenite is 50-60%, and the volume fraction of martensite is 40-50%; according to the mechanical properties, the tensile strength ranges from 560 MPa to 670 MPa, the ductility ranges from 41% to 43%, and the product of strength and elongation ranges from 24 GPa.% to 28 GPa.%; the thickness of the alloy plate ranges from 0.6 mm to 2 mm. The alloy provided by the invention has higher strength and elongation and larger product of strength and elongation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy materials, and in particular to a dynamic isomerization-strengthened phase-change-induced plasticity alloy and a preparation method thereof. Background Art

[0002] In recent years, the automobile industry has developed rapidly, and the number of cars in use has been on the rise. However, the problems that followed, such as fuel shortages and automobile environmental pollution, have become increasingly serious. Energy saving, environmental protection, safety, and comfort have become the new direction of the development of the automobile industry, and the requirements for corrosion resistance and collision resistance of the car body are becoming higher and higher. Transformation induced plasticity (TRIP) alloy is a high-strength material with good plasticity and toughness, which can be used in automobile body equipment manufacturing, etc. to ensure safety. The structure of traditional TRIP alloy is a highly plastic soft ferrite matrix and a hard second phase bainite and a small amount of residual austenite. This transformation induced plastic steel will crack during the forming process such as hole expansion, which reduces the yield rate and limits its wide application.

[0003] For TRIP alloys with good formability and austenite as the matrix, the soft austenite is transformed into hard martensite through phase transformation during deformation. At this time, austenite and martensite are adjacent and have significant mechanical response differences, including strength, plasticity, work hardening, etc. During deformation, a strain gradient will be formed at the interface between adjacent regions. The resulting back stress causes work hardening, which makes up for the lack of forest dislocation hardening. Especially at high strength levels, a good coordination of strength and toughness / plasticity can be obtained, showing a typical dynamic isomerization (DHDI) strengthening effect. Traditional TRIP alloys with austenite as the matrix quickly transform austenite into martensite at the beginning of deformation, and the material shows strong work hardening ability; however, when austenite is completely transformed into martensite, the material loses its deformation ability and breaks quickly, and its elongation and strength-ductility product are insufficient.

[0004] The patent application with application number CN202310061738.8 discloses a method for manufacturing layered heterogeneous high-strength steel, the composition of the steel plate is: C: 0.35-0.45%, Mn: 9.5-10.5%, Al: 1.5-2.5%, V: 0.45-0.55%, Si: 0.5-1.5%, Mo: 0-0.5%; although the steel plate provided has excellent mechanical properties, the high content of Mn and Al makes the continuous casting process more difficult, and the deformation resistance and poor weldability in the rolling process are also more prominent, and the corrosion resistance of the steel plate is low, which is not suitable for large-scale promotion and application. The patent with application number CN202011485343.3 discloses an austenitic stainless steel for nuclear power valves and its preparation method. The composition of the stainless steel is C≤0.08%, Si≤0.8%, Mn≤2.00%, S≤0.02%, P≤0.03%, Cr: 17.0~19.0%, Ni: 9.0~12.0%, Co≤0.08%, Ti≥5×C%; the material provided has a large elongation and high impact absorption work, but its strength is low, and the cyclic forging process is complex and difficult to operate, and the production efficiency is low. In summary, the existing stainless steel TRIP alloy has high strength and high work hardening ability, but the plasticity and toughness are insufficient, and it is difficult to meet the requirements of the impact resistance of structural parts such as car bodies; in addition, traditional TRIP alloys are prone to cracking and other problems during the forming process such as hole expansion, which reduces the yield rate, and the processing technology of some materials is complex and difficult to operate, which limits its wide application. Therefore, how to obtain alloys with high strength and plasticity and large strength-plasticity product through "moderate" alloy composition and organizational structure design is the key to achieving widespread application of TRIP alloys. Summary of the invention

[0005] Based on this, the purpose of the present invention is to provide a method for preparing a phase transformation induced plasticity alloy with dynamic isomerization strengthening, through the coordinated regulation of alloy raw materials, component ratios, processing technology and parameters, the stacking fault energy and grain size of the austenite phase are effectively adjusted, an austenite matrix with moderate stability is obtained to slow down the rate of martensitic phase transformation during deformation, and the action mode of synergistic strengthening of TRIP and DHDI is optimized, thereby preparing an alloy with excellent comprehensive performance, and the prepared alloy has higher strength, elongation and greater strength-ductility product.

[0006] The present invention is realized by the following technical scheme: a method for preparing a phase change induced plastic alloy with dynamic isomerization strengthening, comprising the following steps: batching, smelting, hot rolling, pickling, cold rolling, annealing and leveling treatment.

[0007] Furthermore, the batching step is specifically as follows: batching is performed according to the following components and their mass percentages: Fe: 68-73%, Cr: 19-24%, Ni: 8-13%, wherein the raw material purity of Fe, Cr and Ni is ≥99.9%.

[0008] Furthermore, the smelting step is specifically as follows: the Fe, Cr, and Ni raw materials obtained according to the batching step are mixed and put into an induction melting furnace, vacuum smelting is performed under argon protection, and then the molten steel is cast into an ingot; the ingot is homogenized at a temperature of 1200±10°C, a heating rate of 8-12°C / s, a homogenization time of 180-240min, and a cooling rate of 2-4°C / s after the homogenization to room temperature to obtain an ingot at room temperature.

[0009] Furthermore, the hot rolling step is specifically as follows: heating the ingot at room temperature obtained in the smelting step to a hot rolling temperature of 1150±30°C, with a heating rate of 8-12°C / s, and keeping warm for 100-120 minutes; performing multiple rolling passes using a hot rolling mill, with a start rolling temperature of 1150±10°C, a rolling amount of 3-5% per pass, a total rolling amount of 30-40%, a final rolling temperature of 950±30°C, and obtaining a hot-rolled plate with a thickness of 9-11 mm; and air cooling to room temperature after hot rolling to obtain a hot-rolled plate at room temperature.

[0010] Furthermore, the pickling step is specifically as follows: using a 1:3 hydrochloric acid solution to pickle the hot-rolled plate at room temperature for 20 minutes to remove the oxide layer; after pickling, grinding and removing impurities from the surface of the hot-rolled plate, and then cleaning and drying with anhydrous ethanol.

[0011] Furthermore, the cold rolling step is specifically as follows: the hot rolled plate treated by the pickling step is cold rolled by a cold rolling mill, with each rolling amount being 3-5% and the total rolling amount being 70-80%, to obtain a cold rolled plate with a thickness of 0.8-2.2 mm.

[0012] Furthermore, the annealing step is specifically as follows: annealing the cold-rolled sheet obtained by the cold rolling step, the annealing temperature is 600-800°C, the heating rate is 8-12°C / s, the temperature is kept for 10-60 minutes, and then cooled to room temperature.

[0013] Furthermore, the flattening step is specifically as follows: flattening the plate treated in the annealing step, with a flattening elongation of 0.5-1.2%; and obtaining a plate with a thickness of 0.6-2 mm after flattening.

[0014] Furthermore, the hot rolling mill in the hot rolling step is a double-roll hot rolling mill, and the cold rolling mill in the cold rolling step is a four-roll cold rolling mill.

[0015] At the same time, the present invention also provides a dynamic isomerization strengthened phase transformation induced plasticity alloy, which includes the following components according to mass percentage: Fe: 68-73%, Cr: 19-24%, Ni: 8-13%;

[0016] Metallographic structure: a dual-phase structure containing austenite and martensite. Before stretching, austenite is dominant, with a volume fraction of austenite of 90-100% and a volume fraction of martensite of 0-10%. After stretching, the volume fraction of austenite is 50-60% and the volume fraction of martensite is 40-50%.

[0017] Mechanical properties: tensile strength is 560-670MPa, elongation is 41-43%, and strength-ductility product is 24-28GPa·%;

[0018] The alloy plate has a thickness of 0.6 to 2 mm.

[0019] The beneficial effects of the present invention are: through the coordinated regulation of alloy raw materials, component ratios, processing technology and parameters, the stacking fault energy and grain size of the austenite phase are effectively adjusted, an austenite matrix with moderate stability is obtained to slow down the rate of martensitic phase transformation during deformation, and the synergistic strengthening mode of TRIP and DHDI is optimized, which has higher strength, elongation and greater strength-ductility product, thereby preparing an alloy with excellent comprehensive performance. On the one hand, the martensitic phase transformation during deformation can significantly improve the strength of the material, and a series of stainless steel TRIP alloys with different yield strengths can be obtained in combination with pre-deformation treatment; on the other hand, the mechanical properties of the martensite formed by phase transformation and the austenitic matrix are significantly different, and the DHDI stimulated thereby further improves the work hardening ability and elongation of the alloy. The yield strength of the obtained alloy is ≥500MPa, the elongation is ≥43%, and the strength-ductility product is better than 28GPa·%; the production process and equipment used for the alloy are simple and low-cost, providing a new direction for industrial production.

[0020] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 1 is a uniaxial tensile engineering stress-strain curve diagram of the alloys prepared in Example 1 and Comparative Example 2 provided by the present invention;

[0022] Figure 2 is an EBSD morphology image of the alloy after annealing treatment in Example 1 provided by the present invention;

[0023] Figure 3 This is an EBSD morphology image of the alloy prepared in Example 1 provided by the present invention after tensile fracture. DETAILED DESCRIPTION

[0024] In order to achieve the synergistic improvement of the comprehensive mechanical properties of stainless steel TRIP alloys, it is crucial to regulate the coupled strengthening process of TRIP and DHDI. Liu Haitao et al. reported in the paper "Enhanced strength-ductility synergy in brittle high borated steel bytailoring strain hardening behavior" published in the journal "Scripta Materialia" on page 115398, volume 230, that the stability of austenite in FeCrNiB alloy increases with the increase of tensile temperature, and the alloy exhibits a discontinuous TRIP strengthening effect and has the best strength-ductility match. In addition, Hodgson et al. published a paper "Dependence of deformation behavior on grain size and strain rate in an ultrahigh strength-ductile Mn-based TRIP alloy" on pages 35-42, volume 653, in the journal "Materials Science & Engineering A", which proposed that the grain size significantly affects the stability of austenite, and reasonable regulation of the alloy's microstructure is expected to optimize its mechanical properties. It can be seen that too high or too low austenite stability is not conducive to fully exerting the advantages of the synergistic strengthening effect of TRIP and DHDI. How to achieve a "moderate" microstructure design is the key to obtaining alloys with high strength and plasticity and large strength-plasticity product.

[0025] Based on this, the present application proposes a method for preparing a phase transformation induced plasticity alloy with dynamic isomerization strengthening, which includes the following steps: batching, smelting, hot rolling, pickling, cold rolling, annealing, and leveling.

[0026] The specific steps of batching are: batching according to the following components and their mass percentages: Fe: 68-73%, Cr: 19-24%, Ni: 8-13%, wherein the raw material purity of Fe, Cr and Ni is ≥ 99.9%. High-purity raw materials are used to avoid the influence of impurities on the alloy phase transformation process.

[0027] The smelting step is specifically as follows: the Fe, Cr and Ni raw materials obtained according to the batching step are mixed and put into an induction melting furnace, vacuum smelting is performed under argon protection, and then the molten steel is cast into an ingot; the ingot is homogenized at a temperature of 1200±10°C, a heating rate of 8-12°C / s, a homogenization time of 180-240min, and a cooling rate of 2-4°C / s after the homogenization to room temperature to obtain an ingot at room temperature.

[0028] The hot rolling step is specifically as follows: using a hot charging method, heating the ingot at room temperature obtained in the smelting step to a hot rolling temperature of 1150±30°C, a heating rate of 8-12°C / s, and keeping warm for 100-120min; using a hot rolling mill to perform multiple passes of rolling, the start rolling temperature is 1150±10°C, the rolling amount of each pass is 3-5%, the total rolling amount is 30-40%, the final rolling temperature is 950±30°C, and a hot-rolled plate with a thickness of 9-11mm is obtained; after hot rolling, air cooling is performed to room temperature to obtain a hot-rolled plate at room temperature.

[0029] The pickling step is specifically as follows: the hot-rolled plate at room temperature obtained by the hot pressing step is pickled for 20 minutes using a 1:3 hydrochloric acid solution to remove the oxide layer; after pickling, the surface of the hot-rolled plate is polished and decontaminated, and then cleaned and dried using anhydrous ethanol.

[0030] The cold rolling step is specifically as follows: the hot rolled sheet after the pickling step is cold rolled by a cold rolling mill, with each rolling amount being 3-5% and the total rolling amount being 70-80%, to obtain a cold rolled sheet with a thickness of 0.8-2.2 mm.

[0031] The annealing step is specifically as follows: annealing the cold-rolled sheet obtained in the cold-rolling step, with an annealing temperature of 600-800° C., a heating rate of 8-12° C. / s, keeping the temperature for 10-60 minutes, and then cooling to room temperature.

[0032] The leveling step is specifically as follows: leveling the plate after the annealing step, with a leveling elongation of 0.5-1.2%; and obtaining a plate with a thickness of 0.6-2 mm after leveling.

[0033] Furthermore, the hot rolling mill in the hot rolling step is a double-roll hot rolling mill, and the cold rolling mill in the cold rolling step is a four-roll cold rolling mill.

[0034] According to the above steps, a dynamic isomerization strengthened phase transformation induced plasticity alloy is obtained, and the metallographic structure of the alloy is: a dual-phase structure containing austenite and martensite, with austenite as the main phase before stretching, the volume fraction of austenite is 90-100%, and the volume fraction of martensite is 0-10%; the volume fraction of austenite after stretching is 50-60%, and the volume fraction of martensite is 40-50%; mechanical properties: tensile strength is 560-670MPa, elongation is 41-43%, and strength-ductility product is 24-28GPa·%; the thickness of the alloy plate is 0.6-2mm. Among them, the strength-ductility product is a comprehensive performance index that characterizes the strength and toughness level of metal materials. It is the product of the tensile strength of steel or alloy and the elongation after fracture (i.e., elongation). Its value is approximately equal to the area surrounded by the tensile curve of steel, which represents the energy absorbed by steel during the tensile test or the work done when the external force breaks the specimen. The larger the strength-ductility product, the better the comprehensive strength and toughness performance of the metal material.

[0035] Through the coordinated regulation of alloy raw materials, component ratios, processing technology and parameters, the stacking fault energy and grain size of the austenite phase are effectively adjusted, and an austenite matrix with moderate stability is obtained to slow down the rate of martensitic phase transformation during deformation, and the synergistic strengthening mode of TRIP and DHDI is optimized, which has higher strength, elongation and greater strength-ductility product, thereby preparing an alloy with excellent comprehensive performance. On the one hand, the martensitic phase transformation during deformation can significantly improve the strength of the material, and combined with pre-deformation treatment, a series of stainless steel TRIP alloys with different yield strengths can be obtained; on the other hand, the mechanical properties of the martensite formed by phase transformation and the austenitic matrix are significantly different, and the DHDI stimulated thereby further improves the alloy's work hardening ability and elongation. Compared with the existing stainless steel TRIP alloy, the present invention improves the strength, plasticity, toughness and formability of the alloy simultaneously by regulating the stacking fault energy, grain size, quantity, distribution and other aspects of the austenite phase, broadens the processing window of the alloy and improves the processing efficiency of the alloy; the obtained alloy has a yield strength of ≥500MPa, an elongation of ≥43%, and a strength-plasticity product better than 28GPa·%; the production process and equipment used for the alloy are simple and low-cost, providing a new direction for industrial production.

[0036] Furthermore, the mechanical properties and strength-ductility product of the alloys obtained under different component ratios, processing techniques and parameters will be compared and analyzed through 3 examples and 7 comparative examples, so as to prepare an alloy with excellent comprehensive performance through the coordinated regulation of alloy raw materials, component ratios, processing techniques and parameters.

[0037] Examples 1 to 3 and Comparative Examples 1 to 8

[0038] First, the Thermal-Cal software and TCFE7 database are used to calculate the transformation temperatures of ferrite, austenite and martensite of alloys with different components under the equilibrium phase diagram, determine the element ratio, homogenization treatment, hot rolling, and annealing temperature parameters, and determine the mass percentage of the main elements of the alloy. The element ratios of Examples 1 to 3 and Comparative Examples 1 to 6 are shown in Table 1, wherein the element ratios of Examples 1 to 3 are the same, and only the annealing temperatures are different, the element ratios of Comparative Examples 1 to 3 are the same, and only the annealing temperatures are different, and the element ratios of Comparative Examples 4 to 6 are the same, and only the annealing temperatures are different. The specific annealing temperatures are shown in Table 2. Table 1 Mass percentage of alloy components of Examples 1 to 3 and Comparative Examples 1 to 6 of the phase transformation induced plasticity alloy with dynamic isomerization strengthening in the present invention

[0039] Element content / wt.% Fe Cr Ni Example 1, 2, 3 68 24 8 Comparative Examples 1, 2, 3 73 19 8 Comparative Examples 4, 5, and 6 68 19 13

[0040] Example 1 According to the ratio in Table 1, the corresponding alloy was prepared according to the following method steps:

[0041] (1) Ingredients: Fe, Cr and Ni alloy raw materials with a purity of ≥99.9% were weighed according to the chemical composition mass percentage of the alloy described in Table 1, mixed evenly and transferred to a melting crucible for later use.

[0042] (2) Melting: placing a crucible in an induction melting furnace, performing vacuum melting under argon protection, and then casting the molten steel into an ingot; homogenizing the ingot, the homogenization temperature is 1200°C, the heating rate is 10°C / s, the homogenization time is 240min, and the cooling rate after the homogenization is 2°C / s.

[0043] (3) Hot rolling: The ingot at room temperature was heated to a hot rolling temperature of 1150°C by hot charging method, with a heating rate of 10°C / s and a heat preservation time of 120 min; multiple passes of rolling were performed on a hot rolling mill, with a starting rolling temperature of 1150°C, a rolling amount of 5% per pass, a total rolling amount of 30%, and a final rolling temperature of 950°C to obtain a hot-rolled plate with a thickness of 10 mm; after hot rolling, the ingot was air-cooled to room temperature.

[0044] (4) Pickling: The hot-rolled plate was pickled for 20 min using a 1:3 hydrochloric acid solution to remove the oxide layer. After pickling, the surface of the plate was polished and decontaminated, and then cleaned with anhydrous ethanol and dried.

[0045] (5) Cold rolling: The hot-rolled plate is cold-rolled, with each pass having a rolling amount of 5% and a total rolling amount of 80%, to obtain a plate with a thickness of 1.6 mm.

[0046] (6) Annealing: The cold rolled sheet was annealed at 600°C, a heating rate of 10°C / s, and a holding time of 60 min. After annealing, the sheet was air-cooled to room temperature.

[0047] (7) Flattening: The annealed sheet is flattened, and the flattening elongation is 1.2%. After flattening, the surface is polished to obtain a sheet with a thickness of 1.2 mm.

[0048] Similarly, Examples 2 to 3 and Comparative Examples 1 to 6 obtained alloys according to the ratios in Table 1 and the process parameters in Table 2 according to the same steps as above; in addition, conventional dual-phase steel and conventional TRIP steel were used as Comparative Examples 7 and 8 for mechanical property comparison with Examples 1 to 3 and Comparative Examples 1 to 6.

[0049] The mechanical properties of Examples 1 to 3 and Comparative Examples 1 to 8 are shown in Table 2. The uniaxial tensile engineering stress-strain curves of Example 1 and Comparative Example 2 are shown in Table 2. Figure 1 ,from Figure 1It can be seen that the strength-ductility product of Example 1 is greater than that of Comparative Example 2, indicating that its comprehensive performance is better. In terms of alloy composition, compared with Comparative Examples 1 to 3, Examples 1 to 3 have the same Ni content, which is about 8%, but the Cr content of Examples 1 to 3 is higher, about 24%. The higher Cr content can ensure the excellent corrosion resistance of the alloy. Compared with Comparative Examples 4 to 6, the Fe content of Examples 1 to 3 is about 68%, but the Ni content of Examples 1 to 3 is reduced to about 8%, which can effectively adjust the stacking fault energy of the austenite matrix while reducing the manufacturing cost of the alloy and facilitating industrial production.

[0050] For Examples 1 to 3 having the same alloy composition, the main difference is the heat treatment temperature, which is 600, 700 and 800° C. respectively. Different heat treatment temperatures significantly affect the grain size, proportion, distribution state, etc. of the austenite matrix. Figure 2 This is the EBSD morphology of Example 1 after annealing. In the figure, gray and white represent austenite and martensite, respectively; the volume fractions of austenite and martensite are 91% and 9%, respectively. After annealing at a relatively low temperature, some grains in the cold-rolled plate are recrystallized, and the average grain size is about 1 μm; this is consistent with the grain size range proposed in the paper "A TRIP-assisted dual-phase high-entropy alloy: Grain size and phase fraction effects on deformation behavior" published by Li Zhiming et al. in the journal Acta Materialia, Volume 131, Pages 323-335, that is, the phase transformation process of the TRIP alloy is closely related to the grain size. When the grain size drops to about 1 μm, the phase transformation process is significantly inhibited, and the TRIP effect becomes discontinuous. The microstructure of Example 1 after tensile fracture is shown in the figure. Figure 3As shown, at this time, the volume fraction of austenite drops to 55%, and the volume fraction of martensite rises to 45%, indicating that only part of the austenite matrix undergoes phase transformation during the stretching process, and the coupling effect of the residual austenite and the phase transformation martensite can well stimulate the DHDI strengthening effect. Under the interaction of the DHDI and TRIP effects, the yield strength of Example 1 is 500MPa, the tensile strength is 668MPa, the elongation is 41.9%, and the strength-plasticity product is 28GPa·%. The comprehensive performance is significantly better than that of Example 2, Example 3 and Comparative Examples 1 to 8. In summary, compared with the prior art, the present invention proposes to adjust the stability of stainless steel TRIP alloys with austenite as the matrix through alloy composition and organizational structure design, and obtain a material with good strength, plasticity and formability by stimulating the DHDI and TRIP coupling strengthening effects. Table 2 Heat treatment process parameters and mechanical properties of Examples 1 to 3 and Comparative Examples 1 to 7 of the multi-stage heterogeneous strengthening phase transformation induced plastic alloys in the present invention

[0051]

[0052] Compared with the prior art, the phase transformation induced plastic alloy method of dynamic isomerization strengthening described in the present invention effectively adjusts the stacking fault energy and grain size of the austenite phase through the coordinated regulation of alloy raw materials, component ratios, processing technology and parameters, obtains an austenite matrix with moderate stability to slow down the rate of martensitic phase transformation during deformation, optimizes the synergistic strengthening mode of TRIP and DHDI, and has higher strength, elongation and greater strength-plasticity product, thereby preparing an alloy with excellent comprehensive performance. On the one hand, the martensitic phase transformation during deformation can significantly improve the strength of the material, and a series of stainless steel TRIP alloys with different yield strengths can be obtained in combination with pre-deformation treatment; on the other hand, the mechanical properties of the martensite formed by phase transformation and the austenitic matrix are significantly different, and the DHDI stimulated thereby further improves the work hardening ability and elongation of the alloy. The yield strength of the obtained alloy is ≥500MPa, the elongation is ≥43%, and the strength-plasticity product is better than 28GPa·%; the production process and equipment used for the alloy are simple and low-cost, providing a new direction for industrial production.

[0053] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.

Claims

1. A dynamic isomerization strengthened phase transformation induced plasticity alloy, characterized in that: According to the mass percentage, it includes the following components: Fe: 68-73%, Cr: 19-24%, Ni: 8-13%; Metallographic structure: a dual-phase structure containing austenite and martensite. Before stretching, austenite is dominant, with a volume fraction of austenite of 90-100% and a volume fraction of martensite of 0-10%. After stretching, the volume fraction of austenite is 50-60% and the volume fraction of martensite is 40-50%. Mechanical properties: tensile strength is 560-670MPa, elongation is 41-43%, and strength-ductility product is 24-28GPa·%; The alloy plate has a thickness of 0.6 to 2 mm.

2. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 1, characterized in that: The following steps are involved: Batching, smelting, hot rolling, pickling, cold rolling, annealing and leveling.

3. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 2, characterized in that: The step of mixing ingredients specifically comprises: mixing ingredients according to the following components and their mass percentages: Fe: 68-73%, Cr: 19-24%, Ni: 8-13%, wherein the raw material purity of Fe, Cr and Ni is ≥99.9%.

4. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 3, characterized in that: The smelting step is specifically as follows: the Fe, Cr and Ni raw materials obtained according to the batching step are mixed and put into an induction melting furnace, vacuum smelting is performed under argon protection, and then the molten steel is cast into an ingot; the ingot is homogenized at a temperature of 1200±10°C, a heating rate of 8-12°C / s, a homogenization time of 180-240min, and a cooling rate of 2-4°C / s after the homogenization to room temperature to obtain an ingot at room temperature.

5. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 4, characterized in that: The hot rolling step is specifically as follows: heating the ingot at room temperature obtained in the smelting step to a hot rolling temperature of 1150±30°C, with a heating rate of 8-12°C / s, and keeping the temperature for 100-120 minutes; performing multiple rolling passes using a hot rolling mill, with a start rolling temperature of 1150±10°C, a rolling amount of 3-5% in each pass, a total rolling amount of 30-40%, a final rolling temperature of 950±30°C, and obtaining a hot-rolled plate with a thickness of 9-11 mm; and air cooling to room temperature after hot rolling to obtain a hot-rolled plate at room temperature.

6. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 5, characterized in that: The pickling step is specifically as follows: using a 1:3 hydrochloric acid solution to pickle the hot-rolled plate at room temperature for 20 minutes to remove the oxide layer; after pickling, grinding and removing impurities from the surface of the hot-rolled plate, and then cleaning and drying with anhydrous ethanol.

7. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 6, characterized in that: The cold rolling step is specifically: the hot rolled plate treated in the pickling step is cold rolled by a cold rolling mill, with each rolling amount being 3-5% and the total rolling amount being 70-80%, to obtain a cold rolled plate with a thickness of 0.8-2.2 mm.

8. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 7, characterized in that: The annealing step is specifically: annealing the cold-rolled sheet obtained by the cold rolling step, the annealing temperature is 600-800°C, the heating rate is 8-12°C / s, the temperature is kept for 10-60 minutes, and then cooled to room temperature.

9. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 8, characterized in that: The leveling step is specifically as follows: leveling the plate after the annealing step, with a leveling elongation of 0.5-1.2%; and obtaining a plate with a thickness of 0.6-2 mm after leveling.

10. The method for preparing a dynamic isomerization strengthened phase transformation induced plasticity alloy according to claim 9, characterized in that: The hot rolling mill in the hot rolling step is a double-roll hot rolling mill, and the cold rolling mill in the cold rolling step is a four-roll cold rolling mill.

Citation Information

Cited By

  • Light-weight high-strength transformation induced plasticity alloy with ideal elastoplasticity and preparation method of light-weight high-strength transformation induced plasticity alloy

    CN121183250A