Aluminum alloy coated steel plate and preparation method thereof
By optimizing chemical composition and alloying heating treatment in aluminum alloy plated steel plates, combined with pulling and light finishing processes, the problem of insufficient heat absorption performance of aluminum alloy plated is solved, and more efficient heat absorption performance and surface characteristics are achieved.
Patent Information
- Application Number
- CN202411229613.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The heat absorption performance of existing aluminum alloy coatings still needs to be improved, which is difficult to meet the construction industry's demand for improving solar energy utilization and reducing fossil energy consumption.
By rationally designing chemical components, including Si, Fe, Ti and Al in aluminum alloy-coated steel plates, performing alloying heating treatment, and combining pulling and light finishing processes, the thickness and surface characteristics of the plating layer are optimized to improve the heat absorption performance of the plating layer. .
显著提高了铝合金镀层的吸热性能和表面均匀性,降低了热反射率,增强了镀层的耐蚀性和耐热性,满足了在0-800℃温度范围内的吸热需求。
Smart Images

Figure CN119061343A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steel material preparation, and in particular to an aluminum alloy coated steel plate and a preparation method thereof. Background Art
[0002] In the construction industry, improving the utilization rate of solar energy and improving the heat absorption performance of materials can better reduce the consumption of fossil energy and electricity, and play a role in energy conservation and emission reduction. Hot dip plating technology is mature, complete, and has a wide range of applications. Using hot dip plating technology instead of electroplating and other coating processes can achieve mass production of low-cost heat-absorbing coatings.
[0003] At present, among the commonly used metal hot-dip coatings, aluminum alloy coatings have the best corrosion resistance and heat resistance and are suitable for heat-absorbing coatings. However, the heat absorption performance of aluminum alloy coatings needs to be further improved. Summary of the invention
[0004] The present application provides an aluminum alloy coated steel plate and a preparation method thereof to solve the following technical problem: how to improve the heat absorption performance of the aluminum alloy coating.
[0005] In a first aspect, the present application provides a method for preparing an aluminum alloy coated steel plate, the method comprising:
[0006] A first aluminum alloy coated steel plate is obtained, wherein the first aluminum alloy coated steel plate comprises a steel substrate and an aluminum alloy coating attached to at least a portion of the surface of the steel substrate, wherein the chemical composition of the aluminum alloy coating comprises: Si, Fe, Ti and Al; wherein, by mass fraction, the content of Si is 5% to 11%, the content of Fe is 2% to 10%, and the content of Ti is 0.1% to 2%;
[0007] The first aluminum alloy coated steel plate is subjected to alloying heating, and the process parameters of the alloying heating are set according to the thickness of the first aluminum alloy coated steel plate to obtain a second aluminum alloy coated steel plate.
[0008] Optionally, the chemical composition of the aluminum alloy coating further includes: Mg, and the content of Mg is 0.1% to 2%.
[0009] Optionally, the Fe content on the coating surface is 35% to 70%; the Fe content within 0 to 1 μm on the coating surface is 3 O 4 The content is ≤30%.
[0010] Optionally, the chemical composition of the steel matrix includes: C, Si, Mn, Nb, Ti, P, S and Fe; wherein,
[0011] In terms of mass fraction,
[0012] The content of C is 0.001% to 0.1%, the content of Si is 0.001% to 0.5%, the content of Mn is 0.1% to 0.6%, the content of mixed elements of Nb and Ti is 0.1% to 0.4%, the content of P is ≤0.035%, and the content of S is ≤0.035%.
[0013] Optionally, setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate includes:
[0014] When 0.2 mm ≤ the thickness of the first aluminum alloy coated steel plate ≤ 0.8 mm, the process parameters of the alloying heating include: temperature 650° C. to 750° C., time 3 min to 8 min.
[0015] Optionally, setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate includes:
[0016] When the thickness of the first aluminum alloy coated steel plate is 0.8 mm<≤1.5 mm, the process parameters of the alloying heating include: temperature 690° C. to 800° C., time 5 min to 10 min.
[0017] Optionally, setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate includes:
[0018] When 1.5 mm<the thickness of the first aluminum alloy coated steel plate≤3.0 mm, the process parameters of the alloying heating include: a temperature of 750° C. to 850° C. and a time of 8 min to 15 min.
[0019] Optionally, the single-sided coating weight of the first aluminum alloy coated steel plate is 5 g / m 2 ~75g / m 2 The coating thickness of the second aluminum alloy coated steel plate is 8 μm to 50 μm.
[0020] Optionally, the method further comprises: performing tension straightening and skin-passing on the second aluminum alloy coated steel plate to obtain a target aluminum alloy coated steel plate; wherein,
[0021] The finishing process parameters include: finishing roller roughness Ra≥3.5μm, finishing elongation 0.2%-1.0%.
[0022] In a second aspect, the present application provides an aluminum alloy coated steel plate prepared by the method according to the first aspect, wherein the coating of the aluminum alloy coated steel plate satisfies the following characteristics:
[0023] The coating color Lab value L≤30; within the operating temperature range of 0-800℃, the coating thermal reflectivity ε≤20%; the coating surface roughness Ra≥1.5μm; the coating surface Rpc value≥80.
[0024] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0025] The preparation method of the aluminum alloy-coated steel plate provided in the embodiment of the present application includes: obtaining a first aluminum alloy-coated steel plate, wherein the first aluminum alloy-coated steel plate includes a steel substrate and an aluminum alloy coating attached to at least a portion of the surface of the steel substrate, and the chemical composition of the aluminum alloy coating includes: Si, Fe, Ti and Al; wherein, in terms of mass fraction, the content of Si is 5% to 11%, the content of Fe is 2% to 10%, and the content of Ti is 0.1% to 2%; alloying and heating the first aluminum alloy-coated steel plate, and setting the process parameters of the alloying and heating according to the thickness of the first aluminum alloy-coated steel plate to obtain a second aluminum alloy-coated steel plate; and straightening and finishing the second aluminum alloy-coated steel plate to obtain a target aluminum alloy-coated steel plate. Si can make the thickness of the aluminum alloy coating uniform, so that the ΔL value of the coating after subsequent alloying is small, thereby improving the uniformity of the heat absorption performance of the coating surface; Fe can increase the melting point of the coating to prevent the coating from melting during the subsequent alloying process, thereby affecting the completion of the coating, and improving the heat absorption of the coating after alloying; Ti can refine the surface grains of the coating, and due to the high oxygen affinity of Ti, Ti will be enriched on the surface of the coating during the hot-dip and alloying heating process, thereby refining the grains, improving the anisotropy of the coating surface, and reducing the thermal reflectivity of the coating; by alloying the first aluminum alloy-coated steel plate and setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy-coated steel plate, the Fe element in the steel substrate can be diffused into the coating during the alloying process, reducing the brightness (L value) of the coating, and increasing the surface roughness of the coating, thereby further reducing the heat reflectivity and improving the heat absorption performance. In summary, the heat absorption performance of the aluminum alloy coating is improved by rationally designing the chemical composition of the aluminum alloy coating and the alloying heating treatment of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 The present invention is a schematic flow chart of a method for preparing an aluminum alloy coated steel plate according to some embodiments of the present application. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0030] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0031] In this application, the terms "include", "comprising", etc. mean "including but not limited to". In this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations.
[0032] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0033] In a first aspect, the present application provides a method for preparing an aluminum alloy coated steel plate. Figure 1 A schematic diagram of a process for preparing an aluminum alloy coated steel plate according to some embodiments of the present application; see Figure 1 , the method comprising:
[0034] S1. Obtain a first aluminum alloy coated steel plate, wherein the first aluminum alloy coated steel plate comprises a steel substrate and an aluminum alloy coating attached to at least a portion of the surface of the steel substrate, wherein the chemical composition of the aluminum alloy coating comprises: Si, Fe, Ti and Al; wherein, by mass fraction, the content of Si is 5% to 11%, the content of Fe is 2% to 10%, and the content of Ti is 0.1% to 2%;
[0035] In the embodiment of the present application, by adding Si element, the coating thickness can be made more uniform, so that the ΔL value of the coating after subsequent alloying can be small, thereby improving the uniformity of the heat absorption performance of the coating surface. The Si element can also improve the fluidity of the plating solution, and has good oxidation resistance, which can reduce the oxidation of the plating solution and make it easier to control the coating thickness. If the Si content is too high, the plasticity of the coating will be reduced, and the coating will easily crack during subsequent processing, affecting the integrity of the coating and reducing the heat absorption performance of the coating; if the Si content is too low, it is difficult to effectively control the uniformity of the coating, thereby reducing the heat absorption effect of the coating. Exemplarily, the above-mentioned Si content can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, etc.
[0036] The Fe element is added to the plating solution to increase the melting point of the coating, prevent the coating from melting and polluting the equipment during the subsequent alloying process, and the Fe element can be added to the coating to increase the melting point of the coating to prevent the coating from melting during the subsequent alloying process, thereby affecting the completeness of the coating and improving the heat absorption of the coating after alloying. In addition, the selection of the Fe element also takes into account the low cost advantage of the element and is easy to add to the plating solution pot during the production process. If the Fe content in the plating solution is too high, a large amount of iron slag will be generated in the plating solution, causing the surface quality of the material to deteriorate after hot plating and causing the coating to fall off during the stamping process, and iron slag will be generated in the plating solution, resulting in the presence of iron slag in the material coating, which will cause the coating to fall off during the subsequent processing process and affect the heat absorption performance of the material; if the Fe content is too low, it is difficult to effectively increase the melting point of the coating, so that the coating melts during the alloying process and affects the heat absorption performance of the coating. Exemplarily, the above-mentioned Fe content can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.
[0037] The main purpose of adding Ti element to the plating solution is to refine the surface grains of the coating. Due to the high oxygen affinity of Ti element, Ti element will be enriched on the surface of the coating during hot-dip and alloying heating, thereby refining the grains, increasing the anisotropy of the coating surface, and reducing the thermal reflectivity of the coating. If the Ti content in the plating solution is too high, the hardness of the coating will be greatly increased, which will easily cause the coating to crack in the subsequent stamping process, thereby affecting the heat absorption performance of the material; if the Ti content in the plating solution is too low, it is difficult to effectively refine the surface grains of the coating, and the thermal reflectivity of the material surface cannot be effectively reduced. Exemplarily, the above-mentioned Ti content can be 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, 1%, 1.3%, 1.5%, 1.7%, 2%, etc.
[0038] In some embodiments, the chemical composition of the aluminum alloy coating further includes: Mg, and the content of Mg is 0.1% to 2%.
[0039] In the present embodiment, the addition of Mg element in the plating solution is mainly to improve the corrosion resistance of the coating. When the Mg content is too high, excessive Mg will be generated in the coating. 2 Si reduces the plasticity of the coating and affects its performance; when the Mg content is too low, the corrosion resistance of the coating cannot be effectively improved. For example, the Mg content can be 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, 1%, 1.3%, 1.5%, 1.7%, 2%, etc.
[0040] In some embodiments, the Fe content on the surface of the coating is 35% to 70%; the Fe content within 0 to 1 μm on the surface of the coating is 3 O 4 The content is ≤30%.
[0041] In the embodiment of the present application, the content of the coating surface is limited to ensure that the L value of the coating is ≤30. During the heating process, the Fe element will diffuse into the coating, thereby reducing the L value of the coating. When the Fe content on the coating surface is too high, the plasticity of the coating will be greatly reduced to a certain extent. Microcracks are likely to exist in the coating during the stamping process, thereby affecting the corrosion resistance of the coating. In addition, as the heating temperature and time change, the composition of the iron oxide on the coating surface will change. Within 0 to 1 μm on the coating surface, when the Fe content on the coating surface is too high, the coating surface will be more resistant to corrosion. 3 O 4 When the content is too high, the L value of the coating will be greatly increased, thereby deteriorating the heat absorption performance of the coating. For example, the Fe content on the surface of the coating can be 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, etc.; within 0-1 μm of the coating surface, Fe 3 O 4 The content can be 30%, 28%, 26%, 24%, etc.
[0042] In some embodiments, the chemical composition of the steel matrix includes: C, Si, Mn, Nb, Ti, P, S and Fe; wherein, in terms of mass fraction,
[0043] The content of C is 0.001% to 0.1%, the content of Si is 0.001% to 0.5%, the content of Mn is 0.1% to 0.6%, the content of mixed elements of Nb and Ti is 0.1% to 0.4%, the content of P is ≤0.035%, and the content of S is ≤0.035%.
[0044] In the embodiment of the present application, the chemical composition of the steel matrix is reasonably regulated to ensure the performance of the aluminum alloy coated steel plate. For example, the content of C can be 0.001%, 0.005%, 0.01%, 0.05%, 0.1%, etc., the content of Si can be 0.001%, 0.005%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, etc., the content of Mn can be 0.1%, 0.2%, 0.3%, 0.5%, 0.6%, etc., the content of Nb and Ti mixed elements can be 0.1%, 0.2%, 0.3%, 0.4%, etc., the content of P can be 0.035%, 0.03%, 0.027%, 0.025%, etc., and the content of S can be 0.035%, 0.03%, 0.027%, 0.025%, etc.
[0045] S2. Performing alloying heating on the first aluminum alloy coated steel plate, and setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate, to obtain a second aluminum alloy coated steel plate.
[0046] In some embodiments, setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate includes:
[0047] When 0.2 mm ≤ the thickness of the first aluminum alloy coated steel plate ≤ 0.8 mm, the process parameters of the alloying heating include: temperature 650° C. to 750° C., time 3 min to 8 min.
[0048] In some embodiments, setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate includes:
[0049] When the thickness of the first aluminum alloy coated steel plate is 0.8 mm<≤1.5 mm, the process parameters of the alloying heating include: temperature 690° C. to 800° C., time 5 min to 10 min.
[0050] In some embodiments, setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate includes:
[0051] When 1.5 mm<the thickness of the first aluminum alloy coated steel plate≤3.0 mm, the process parameters of the alloying heating include: a temperature of 750° C. to 850° C. and a time of 8 min to 15 min.
[0052] In the present application embodiment, the Lab value of the coating can be reduced by alloying heating of the coating, thereby reducing the thermal reflectivity of the coating. The coating alloying process can be used to replace the traditional painting or electroplating process to better play the role of energy conservation and emission reduction and improve environmental protection, and the production efficiency of alloying heating is higher and the production cost is lower. The coating is alloyed so that the Fe element in the substrate can be diffused into the coating during the alloying process, so that the coating brightness (L value) is reduced, and the coating surface roughness is increased to reduce the thermal reflectivity and improve the heat absorption performance. The process parameters of alloying heating are set according to the thickness of the first aluminum alloy coated steel plate, and the content and roughness of the Fe element on the coating surface can be controlled by controlling the time and temperature of the coating alloying. It is found through research that with the extension of the heating time, the coating surface roughness first increases and then decreases, so in order to ensure that the coating surface roughness after alloying reaches the target requirement range, the process parameters of alloying heating are reasonably regulated. Exemplarily, when 0.2 mm ≤ the thickness of the first aluminum alloy coated steel plate ≤ 0.8 mm, the process parameters of the alloying heating include: the temperature can be 650 ° C, 670 ° C, 690 ° C, 710 ° C, 730 ° C, 750 ° C, etc., and the time can be 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, etc.; when 0.8 mm < the thickness of the first aluminum alloy coated steel plate ≤ 1.5 mm, the process parameters of the alloying heating include: the temperature can be 690 ° C, 700 ° C, 720 ° C, 740 ° C , 760℃, 780℃, 800℃, etc., and the time can be 5min, 6min, 7min, 8min, 9min, 10min, etc.; when 1.5mm<thickness of the first aluminum alloy coated steel plate≤3.0mm, the process parameters of the alloying heating include: the temperature can be 750℃, 770℃, 790℃, 810℃, 830℃, 850℃, etc., and the time can be 8min, 9min, 10min, 11min, 12min, 13min, 14min, 15min, etc. The above alloying heating can be carried out by three heating methods: salt bath furnace, roller bottom furnace, or radiation tube heating furnace to alloy the material, and the atmosphere in the furnace is air during heating.
[0053] In some embodiments, the single-sided coating weight of the first aluminum alloy coated steel plate is 5 g / m 2 ~75g / m 2 The coating thickness of the second aluminum alloy coated steel plate is 8 μm to 50 μm.
[0054] In the embodiment of the present application, the single-side coating weight of the first aluminum alloy coated steel plate can be 5g / m 2 , 10g / m 2 , 15g / m 2 , 20g / m 2 , 25g / m 2 , 30g / m 2 , 35g / m 2 , 40g / m 2 , 45g / m 2 , 50g / m 2 , 55g / m 2 , 60g / m 2 , 65g / m 2 , 70g / m 2 , 75g / m 2 etc.; the coating thickness of the above-mentioned second aluminum alloy coated steel plate can be 8μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, etc.
[0055] In some embodiments, the method further comprises: S3, performing tension straightening and skin-passing on the second aluminum alloy coated steel sheet to obtain a target aluminum alloy coated steel sheet; wherein,
[0056] The finishing process parameters include: finishing roller roughness Ra≥3.5μm, finishing elongation 0.2%-1.0%.
[0057] In the embodiment of the present application, after alloying, the straightening and finishing processes should be used to improve the material shape and improve the surface profile of the steel plate, so that the surface roughness of the steel plate Ra ≥ 1.5 μm and the coating surface Rpc value ≥ 80 can be achieved. By increasing the volatility of the surface morphology of the steel plate, the surface thermal reflectivity can be further reduced to ensure that the coating thermal reflectivity ε ≤ 20%. Exemplarily, the roughness Ra of the above-mentioned finishing roller can be 3.5 μm, 3.7 μm, 4.0 μm, 4.5 μm, etc., and the finishing elongation can be 0.2%, 0.4%, 0.6%, 0.8%, 1.0%, etc. The finishing roller can be processed by electric spark roughening to improve the randomness of the peaks on the coating surface and reduce the processing cost of the grinding roller.
[0058] In a second aspect, the present application provides an aluminum alloy coated steel plate prepared by the method described in the first aspect, wherein the coating of the aluminum alloy coated steel plate satisfies the following excellent properties:
[0059] The coating color Lab value L≤30; within the operating temperature range of 0-800℃, the coating thermal reflectivity ε≤20%; the coating surface roughness Ra≥1.5μm; the coating surface Rpc value≥80.
[0060] The aluminum alloy coated steel plate is realized based on the preparation method of the aluminum alloy coated steel plate mentioned above. The specific steps of the preparation method of the aluminum alloy coated steel plate can refer to the above embodiment. Since the aluminum alloy coated steel plate adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.
[0061] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0062] The embodiment of the present application provides a method for preparing an aluminum alloy-coated steel plate. Please refer to Table 1 for the thickness and coating composition of the first aluminum alloy-coated steel plate, Table 2 for the process parameters of alloying heating and the surface parameters of the coating after heating, and Table 3 for the thickness and performance of the coating after alloying.
[0063] Among them, the steel substrate composition (wt%) used in Examples 1-4 and Comparative Examples 1-4 is as follows: C: 0.005, Si: 0.025, Mn: 0.5, Nb: 0.05, Ti: 0.15, P: 0.02, S: 0.02, and the rest is Fe and inevitable impurities. The aluminum alloy coated steel sheet is processed according to the following steps: steelmaking → hot rolling → cold rolling → annealing → hot-dip aluminum alloy → coiling → uncoiling → surface cleaning → alloying heating → straightening, finishing → oiling → coiling. Examples 1-4 and Comparative Examples 1-3 use a finishing roller with a roughness of 4.0 μm for finishing, and the finishing elongation is 0.6%. Comparative Example 3 uses a finishing roller with a roughness of 2.0 μm for finishing, and the finishing elongation is 0.6%.
[0064] The L value of the coating after alloying was measured by a surface colorimeter, the measuring temperature was room temperature, and the average value of 10 points was taken as the result. The thermal reflectivity of the coating was measured by a reflectance spectrometer, the infrared incident angle was 60°, the test temperature was 800°C, and the average value of 10 times was taken as the result. The surface roughness and Rpc value were measured by a surface profiler, the measuring temperature was room temperature, and the average value of 10 times was taken as the result. The coating thickness and the Fe element content on the coating surface were measured by a scanning electron microscope, and the average value of 10 times was taken as the result. The number of cracks is the number of cracks at the bend of the coating within a length of 1μm, the bending angle is 90°, and the number of cracks is measured under a scanning electron microscope. The red rust time is obtained by a neutral salt spray test. The experiment is carried out in accordance with the national standard GB / T10125-2021 "Artificial Atmosphere Corrosion Test Salt Spray Test", and 3 parallel specimens are used in each group of experiments.
[0065] Table 1 Thickness and coating composition (wt%) of the first aluminum alloy coated steel sheet, the rest being Al and unavoidable impurities
[0066]
[0067] Table 2 Process parameters of alloying heating and surface parameters of the coating after heating
[0068]
[0069] Table 3 Thickness and properties of coating after alloying
[0070]
[0071] In summary, through a suitable alloying process, the coating surface heat reflectivity is ≤20% within the use temperature range of 0-800°C without losing plasticity, and the aluminum alloy coated steel plate is suitable for energy storage and heat absorption equipment or working environment. From Comparative Example 1, it can be obtained that when the Fe content in the plating solution is greater than 10wt%, the Fe content on the surface of the coating exceeds 70wt% under the same alloying process, resulting in a significant increase in the number of cracks in the coating and a decrease in the corrosion resistance of the coating; from Comparative Example 2, compared with Example 3, the coating fails to achieve complete alloying after shortening the heating time, resulting in the L value and Fe content of the coating exceeding the range, and the heat absorption rate of the coating does not meet the use standard; from Comparative Example 3, it can be obtained that when the Si content in the plating solution is less than 5wt%, the coating thickness is excessively thick during the hot-dip process, resulting in an excessively thick coating after alloying. In addition, due to the excessive thickness, the Fe content on the coating surface is reduced under the same alloying process conditions, resulting in a decrease in the thermal reflectivity of the coating, and the excessive thickness of the coating also leads to a decrease in plasticity, thereby increasing the number of cracks in the coating and reducing corrosion resistance. It can be seen from Comparative Example 4 that the roughness of the finishing roller and the finishing elongation in the finishing process are not within the scope of the embodiments of the present application. When the surface roughness and Rpc value of the alloyed coating are less than the specified range, the reflectivity of the coating will be affected, thereby affecting the heat absorption performance of the coating.
[0072] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing an aluminum alloy coated steel plate, It is characterized in that The method comprises: A first aluminum alloy coated steel plate is obtained, wherein the first aluminum alloy coated steel plate comprises a steel substrate and an aluminum alloy coating attached to at least a portion of the surface of the steel substrate, wherein the chemical composition of the aluminum alloy coating comprises: Si, Fe, Ti and Al; wherein, by mass fraction, the content of Si is 5% to 11%, the content of Fe is 2% to 10%, and the content of Ti is 0.1% to 2%; The first aluminum alloy coated steel plate is subjected to alloying heating, and the process parameters of the alloying heating are set according to the thickness of the first aluminum alloy coated steel plate to obtain a second aluminum alloy coated steel plate.
2. The method according to claim 1, It is characterized in that The chemical composition of the aluminum alloy coating also includes: Mg, and the content of Mg is 0.1% to 2%.
3. The method according to claim 1, It is characterized in that The Fe content of the coating surface is 35% to 70%; the Fe content of the coating surface within 0 to 1 μm is 20%. 3 O 4 The content is ≤30%.
4. The method according to claim 1, It is characterized in that The chemical composition of the steel matrix includes: C, Si, Mn, Nb, Ti, P, S and Fe; wherein, in terms of mass fraction, The content of C is 0.001% to 0.1%, the content of Si is 0.001% to 0.5%, the content of Mn is 0.1% to 0.6%, the content of mixed elements of Nb and Ti is 0.1% to 0.4%, the content of P is ≤0.035%, and the content of S is ≤0.035%.
5. The method according to claim 1, It is characterized in that The step of setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate comprises: When 0.2 mm ≤ the thickness of the first aluminum alloy coated steel plate ≤ 0.8 mm, the process parameters of the alloying heating include: temperature 650° C. to 750° C., time 3 min to 8 min.
6. The method according to claim 1, It is characterized in that The step of setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate comprises: When the thickness of the first aluminum alloy coated steel plate is 0.8 mm<≤1.5 mm, the process parameters of the alloying heating include: temperature 690° C. to 800° C., time 5 min to 10 min.
7. The method according to claim 1, It is characterized in that The step of setting the process parameters of the alloying heating according to the thickness of the first aluminum alloy coated steel plate comprises: When 1.5 mm<the thickness of the first aluminum alloy coated steel plate≤3.0 mm, the process parameters of the alloying heating include: a temperature of 750° C. to 850° C. and a time of 8 min to 15 min.
8. The method according to claim 1, It is characterized in that The single-sided coating weight of the first aluminum alloy coated steel plate is 5g / m 2 ~75g / m 2 The coating thickness of the second aluminum alloy coated steel plate is 8 μm to 50 μm.
9. The method according to claim 1, It is characterized in that The method further comprises: performing tension straightening and skin-passing on the second aluminum alloy coated steel sheet to obtain a target aluminum alloy coated steel sheet; wherein, The finishing process parameters include: finishing roller roughness Ra≥3.5μm, finishing elongation 0.2%-1.0%.
10. An aluminum alloy coated steel plate prepared by the method according to any one of claims 1 to 9, It is characterized in that The coating of the aluminum alloy coated steel plate meets the following characteristics: The coating color Lab value L≤30; within the operating temperature range of 0-800℃, the coating thermal reflectivity ε≤20%; the coating surface roughness Ra≥1.5μm; the coating surface Rpc value≥80.
Citation Information
Patent Citations
High-surface-quality aluminum coating steel plate and production method thereof
CN108754312A
Preparation method of hot stamping component coated with aluminum-silicon alloy coating and product of hot stamping component
CN111647802A
1900MPa-grade high-strength and high-toughness aluminum-silicon coated steel plate for hot stamping and preparation method thereof
CN111893377A
Aluminum-silicon alloy plating layer hot forming steel and preparation method thereof
CN113528940A
Method for preparing hot forming part by using hot forming plate containing aluminum coating
CN113814654A