Ruthenium modified bismuth tungstate photo-anode and preparation method thereof
By loading ruthenium on the bismuth tungstate photoanode, the Ru/BWO photoanode is formed, and the close contact between ruthenium and BWO and the band bending of energy bands is solved, the lack of performance of bismuth tungstate photoanode in photoelectric catalytic decomposition of water is significantly improved Photocurrent density and catalytic properties.
Patent Information
- Application Number
- CN202411218770.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
AI Technical Summary
The existing bismuth tungstate photoanode application in photoelectrocatalytic decomposition of water is limited by the narrow visible light absorption range, slow reaction kinetics and low photogenerated carrier separation efficiency, which cannot meet the current material performance requirements.
By mixing RuCl3·3H2O and PVP with aqueous bismuth tungstate solution, adjusting the pH value and carrying out hydrothermal reaction. Ru/BWO photoanode is formed by loading ruthenium on bismuth tungstate, and electron transfer and energy are promoted by using the close contact between ruthenium and BWO. Bending to improve photoelectric catalytic performance.
The photoelectrochemical performance was significantly improved, and the photocurrent density of Ru/BWO-15 reached 0.84mA/cm2 at 1.23V vs. RHE, exceeding 10 times that of unmodified BWO, improving the photoelectrocatalytic performance.
Smart Images

Figure CN119061431A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of photoelectric catalytic materials, and in particular to a ruthenium-modified bismuth tungstate photoanode and a preparation method thereof. Background Art
[0002] Exploring sustainable green energy is crucial to improving environmental pollution and energy crisis caused by excessive burning of fossil fuels. Hydrogen, as a promising pollution-free energy carrier, may significantly reduce pollutant and greenhouse gas emissions while improving energy efficiency. Photoelectrocatalytic technology relies on semiconductor electrodes to decompose water and is a promising technology for converting solar energy into chemical energy, especially for the production of hydrogen. In an ideal PEC reaction system, redox reactions occur at the photoanode to produce oxygen, while the photocathode promotes the production of hydrogen. Therefore, the development of efficient photoanodes is particularly important and necessary.
[0003] The core of photoelectrocatalytic technology lies in the development of efficient photocatalysts. Among many photocatalytic materials, BWO has become one of the photoelectrode materials with great development potential due to its moderate conduction band position and band gap width. However, the further application of BWO in photoelectrocatalytic water splitting is limited by its narrow visible light absorption range, slow reaction kinetics, and low efficiency of photogenerated carrier separation. Therefore, it is necessary to improve its photoelectrocatalytic performance through modification.
[0004] The existing bismuth tungstate photoanode modification has improved the photocurrent density at 1.23V vs. RHE, but the separation efficiency of photogenerated electrons and holes is still insufficient and cannot meet the current requirements for material performance. Summary of the invention
[0005] The purpose of the present invention is to provide a ruthenium-modified bismuth tungstate photoanode and a preparation method thereof. The method of the present invention has the characteristics of simple preparation process, simple operation, no pollution and low cost. The prepared ruthenium-modified bismuth tungstate photoanode has uniform particle size and controllable synthetic particle size. By loading ruthenium, it effectively promotes interfacial charge transfer and provides more active sites, thereby showing significantly improved photoelectrochemical performance.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a ruthenium-modified bismuth tungstate photoanode comprises the following steps:
[0008] Step (1): dissolving BWO in 50 ml of deionized water to form a bismuth tungstate aqueous solution, dissolving RuCl3·3H2O and PVP in 20 ml of deionized water and mixing thoroughly, and then adding the bismuth tungstate aqueous solution, wherein the mass ratio of PVP to RuCl3·3H2O is 1:2, and the mass ratio of RuCl3·3H2O to BWO is 0.05-0.2:1; adjusting the pH to 11-12 to obtain a reaction precursor solution;
[0009] Step (2): the reaction precursor solution is transferred into a polytetrafluoroethylene reactor, and the reaction temperature is set to 180-210° C. and the reaction time is set to 16-20 h for hydrothermal reaction;
[0010] Step (3): The product is taken out and washed by centrifugation with deionized water and anhydrous ethanol respectively, and then dried and ground to obtain a Ru / BWO photoanode.
[0011] Furthermore, the preparation of BWO in step (1) comprises the following steps:
[0012] S1: Weigh Bi(NO3)3·5H2O, Na2WO4·2H2O and EDTA in a molar ratio of 2:1:2 respectively, dissolve Bi(NO3)3·5H2O in 20 ml of ethylene glycol, mix thoroughly, add EDTA and stir until completely dissolved to form a bismuth nitrate solution; dissolve Na2WO4·2H2O in 50 ml of deionized water to form a sodium tungstate solution;
[0013] S2: Mix the bismuth nitrate solution and the sodium tungstate solution, add 2 mol / L NaOH solution to adjust the pH to 9-10, and then move it into a polytetrafluoroethylene reactor, set the reaction temperature to 180-210°C, and the time to 16-20h for hydrothermal reaction. The hydrothermal reaction temperature is increased to the reaction temperature at a rate of 4-8°C / min, and after the reaction, the temperature is reduced to 25-50°C at a cooling rate of 3-6°C / min, and then naturally cooled to room temperature. After taking out the product, it is centrifugally washed with deionized water and anhydrous ethanol for 3-5 times, vacuum dried at 60-80°C for 12h, and ground to obtain BWO.
[0014] Furthermore, in step (1), the pH is adjusted using a 2 mol / L NaOH solution.
[0015] Furthermore, the hydrothermal reaction process of step (2) is to increase the temperature to the reaction temperature at a rate of 4 to 8°C / min, and after the reaction, cool the temperature to 25 to 50°C at a cooling rate of 3 to 6°C / min, and then naturally cool to room temperature.
[0016] Furthermore, the number of centrifugal washing in step (3) is 3 to 5 times.
[0017] Furthermore, the drying in step (3) is vacuum drying at 60-80° C. for 12 h.
[0018] The present invention provides a tungsten-ruthenium-modified bismuth tungstate photoanode prepared by the preparation method as described above. The structure of the ruthenium-modified bismuth tungstate photoanode is a stacked two-dimensional layered structure of BWO nanosheets, and some small particles of Ru are attached to the BWO nanosheets.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention first disperses the bismuth tungstate solution uniformly, then adds ruthenium trichloride hydrate and an aqueous solution of PVP and stirs until the mixture is uniformly mixed, and then adjusts the pH value and performs hydrothermal synthesis, so that ruthenium is loaded on the bismuth tungstate to obtain a ruthenium-modified bismuth tungstate photoanode material. BWO has a higher work function and a lower Fermi energy, while Ru has a lower work function and a higher Fermi energy. When BWO and Ru are in close contact, electron transfer from Ru to BWO occurs until equilibrium is reached in the Fermi level, resulting in a downward bending of the energy band and the formation of an ohmic contact, so that there is no barrier for electrons to enter the metal from the semiconductor, which is conducive to promoting the migration of photogenerated charge carriers. This charge redistribution at the interface establishes an internal electric field (IEF) between the negatively charged surface of BWO and the positively charged surface of Ru. When light is irradiated, the IEF can guide the photogenerated electrons to transfer from the conduction band of BWO to Ru, and the energy band bending formed due to the ohmic contact can prevent the migration of charge carriers from Ru to BWO, thereby effectively improving the photoelectrocatalytic performance. The photocurrent density of Ru / BWO-15 can reach a maximum of 0.84 mA / cm2 at 1.23 V vs. RHE, which is 10 times that of BWO (0.08 mA / cm2) at the same potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The XRD patterns of the samples prepared in Examples 1 to 4 and Comparative Example 1 of the present invention are shown in FIG.
[0022] Figure 2 This is a SEM image of the BWO sample of Comparative Example 1 of the present invention at 10 μm.
[0023] Figure 3 This is a SEM image of the sample prepared in Example 3 of the present invention at 10 μm.
[0024] Figure 4a The LSV graphs of the samples prepared in Examples 1 to 4 of the present invention and Comparative Example 1 under visible light irradiation.
[0025] Figure 4b The LSV graphs of the samples prepared in Examples 1 to 4 of the present invention and Comparative Example 1 under dark conditions are shown. DETAILED DESCRIPTION
[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0027] Example 1: A method for preparing a ruthenium-modified bismuth tungstate photoanode is as follows:
[0028] (1) Weigh 2 mmol of Bi(NO3)3·5H2O, 1 mmol of Na2WO4·2H2O and 2 mmol of EDTA, all of which are analytical grade (AR);
[0029] (2) Add 2mmol Bi(NO3)3·5H2O to 20ml ethylene glycol, stir magnetically at room temperature, add 2mmol EDTA after stirring evenly, and stir until completely dissolved; add 1mmol Na2WO4·2H2O into deionized water, and in order to strictly control the filling ratio of the subsequent reaction, use 50ml of deionized water as the aqueous solution system, stir magnetically at room temperature, and add the sodium tungstate aqueous solution to the bismuth nitrate solution to obtain a reaction precursor solution;
[0030] (3) adjusting the pH value of the reaction precursor solution to 9 with 2 mol / L NaOH solution;
[0031] (4) transferring the reaction precursor solution with adjusted pH value into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h;
[0032] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0033] (5) After the hydrothermal reaction is completed, the product is taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in a vacuum at 70° C. for 12 h, and then ground to obtain a BWO photoanode.
[0034] (6) Weigh 0.5 g of BWO material and dissolve it in 50 ml of deionized water and perform ultrasonic dispersion. Dissolve 0.025 g of RuCl3·3H2O and 0.0125 g of PVP in 20 ml of deionized water, mix thoroughly, and then add them to the bismuth tungstate aqueous solution to obtain a reaction precursor solution. At this time, the Ru loading amount is 5%;
[0035] (7) adjusting the pH value of the reaction precursor solution to 11 with 2 mol / L NaOH solution;
[0036] (8) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h.
[0037] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0038] After the hydrothermal reaction was completed, the product was taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in vacuum at 70°C for 12h, and then ground to obtain the Ru / BWO-5 photoanode.
[0039] Example 2: A method for preparing a ruthenium-modified bismuth tungstate photoanode is as follows:
[0040] (1) Weigh 2 mmol of Bi(NO3)3·5H2O, 1 mmol of Na2WO4·2H2O and 2 mmol of EDTA, all of which are analytical grade (AR);
[0041] (2) Add 2mmol Bi(NO3)3·5H2O to 20ml ethylene glycol, stir magnetically at room temperature, add 2mmol EDTA after stirring evenly, and stir until completely dissolved; add 1mmol Na2WO4·2H2O into deionized water, and in order to strictly control the filling ratio of the subsequent reaction, use 50ml of deionized water as the aqueous solution system, stir magnetically at room temperature, and add the sodium tungstate aqueous solution to the bismuth nitrate solution to obtain a reaction precursor solution;
[0042] (3) adjusting the pH value of the reaction precursor solution to 9 with 2 mol / L NaOH solution;
[0043] (4) transferring the reaction precursor solution with adjusted pH value into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h;
[0044] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0045] (5) After the hydrothermal reaction is completed, the product is taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in a vacuum at 70° C. for 12 h, and then ground to obtain a BWO photoanode.
[0046] (6) Weigh 0.5 g of BWO material and dissolve it in 50 ml of deionized water and perform ultrasonic dispersion. Dissolve 0.05 g of RuCl3·3H2O and 0.025 g of PVP in 20 ml of deionized water, mix thoroughly, and then add them to the bismuth tungstate aqueous solution to obtain a reaction precursor solution. At this time, the Ru loading amount is 10%;
[0047] (7) adjusting the pH value of the reaction precursor solution to 11 with 2 mol / L NaOH solution;
[0048] (8) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h.
[0049] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0050] After the hydrothermal reaction, the product was taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in vacuum at 70°C for 12h, and then ground to obtain the Ru / BWO-10 photoanode.
[0051] Example 3: A method for preparing a ruthenium-modified bismuth tungstate photoanode is as follows:
[0052] (1) Weigh 2 mmol of Bi(NO3)3·5H2O, 1 mmol of Na2WO4·2H2O and 2 mmol of EDTA, all of which are analytical grade (AR);
[0053] (2) Add 2mmol Bi(NO3)3·5H2O to 20ml ethylene glycol, stir magnetically at room temperature, add 2mmol EDTA after stirring evenly, and stir until completely dissolved; add 1mmol Na2WO4·2H2O into deionized water, and in order to strictly control the filling ratio of the subsequent reaction, use 50ml of deionized water as the aqueous solution system, stir magnetically at room temperature, and add the sodium tungstate aqueous solution to the bismuth nitrate solution to obtain a reaction precursor solution;
[0054] (3) adjusting the pH value of the reaction precursor solution to 9 with 2 mol / L NaOH solution;
[0055] (4) transferring the reaction precursor solution with adjusted pH value into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h;
[0056] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0057] (5) After the hydrothermal reaction is completed, the product is taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in a vacuum at 70° C. for 12 h, and then ground to obtain a BWO photoanode.
[0058] (6) Weigh 0.5 g of BWO material and dissolve it in 50 ml of deionized water and perform ultrasonic dispersion. Dissolve 0.075 g of RuCl3·3H2O and 0.0375 g of PVP in 20 ml of deionized water, mix thoroughly, and then add them to the bismuth tungstate aqueous solution to obtain a reaction precursor solution. At this time, the Ru loading amount is 15%;
[0059] (7) adjusting the pH value of the reaction precursor solution to 11 with 2 mol / L NaOH solution;
[0060] (8) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h.
[0061] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0062] After the hydrothermal reaction, the product was taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in vacuum at 70°C for 12h, and then ground to obtain the Ru / BWO-15 photoanode.
[0063] Example 4: A method for preparing a ruthenium-modified bismuth tungstate photoanode is as follows:
[0064] (1) Weigh 2 mmol of Bi(NO3)3·5H2O, 1 mmol of Na2WO4·2H2O and 2 mmol of EDTA, all of which are analytical grade (AR);
[0065] (2) Add 2mmol Bi(NO3)3·5H2O to 20ml ethylene glycol, stir magnetically at room temperature, add 2mmol EDTA after stirring evenly, and stir until completely dissolved; add 1mmol Na2WO4·2H2O into deionized water, and in order to strictly control the filling ratio of the subsequent reaction, use 50ml of deionized water as the aqueous solution system, stir magnetically at room temperature, and add the sodium tungstate aqueous solution to the bismuth nitrate solution to obtain a reaction precursor solution;
[0066] (3) adjusting the pH value of the reaction precursor solution to 9 with 2 mol / L NaOH solution;
[0067] (4) transferring the reaction precursor solution with adjusted pH value into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h;
[0068] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0069] (5) After the hydrothermal reaction is completed, the product is taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in a vacuum at 70° C. for 12 h, and then ground to obtain a BWO photoanode.
[0070] (6) Weigh 0.5 g of BWO material and dissolve it in 50 ml of deionized water and perform ultrasonic dispersion. Dissolve 0.1 g of RuCl3·3H2O and 0.05 g of PVP in 20 ml of deionized water, mix thoroughly, and then add them to the bismuth tungstate aqueous solution to obtain a reaction precursor solution. At this time, the Ru loading amount is 20%;
[0071] (7) adjusting the pH value of the reaction precursor solution to 11 with 2 mol / L NaOH solution;
[0072] (8) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h.
[0073] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0074] After the hydrothermal reaction was completed, the product was taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in vacuum at 70°C for 12h, and then ground to obtain the Ru / BWO-20 photoanode.
[0075] Example 5: A method for preparing a ruthenium-modified bismuth tungstate photoanode is as follows:
[0076] (1) Weigh 2 mmol of Bi(NO3)3·5H2O, 1 mmol of Na2WO4·2H2O and 2 mmol of EDTA, all of which are analytical grade (AR);
[0077] (2) Add 2mmol Bi(NO3)3·5H2O to 20ml ethylene glycol, stir magnetically at room temperature, add 2mmol EDTA after stirring evenly, and stir until completely dissolved; add 1mmol Na2WO4·2H2O into deionized water, and in order to strictly control the filling ratio of the subsequent reaction, use 50ml of deionized water as the aqueous solution system, stir magnetically at room temperature, and add the sodium tungstate aqueous solution to the bismuth nitrate solution to obtain a reaction precursor solution;
[0078] (3) adjusting the pH value of the reaction precursor solution to 10 with 2 mol / L NaOH solution;
[0079] (4) transferring the reaction precursor solution with adjusted pH value into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 180° C. for 20 h;
[0080] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 4°C / min, and after the reaction, it was cooled to 25°C at a rate of 3°C / min, and then naturally cooled to room temperature;
[0081] (5) After the hydrothermal reaction is completed, the product is taken out and washed with deionized water and anhydrous ethanol for 5 times by centrifugation, dried in vacuum at 60° C. for 12 h, and then ground to obtain a BWO photoanode.
[0082] (6) Weigh 0.5 g of BWO material and dissolve it in 50 ml of deionized water and perform ultrasonic dispersion. Dissolve 0.025 g of RuCl3·3H2O and 0.0125 g of PVP in 20 ml of deionized water, mix thoroughly, and then add them to the bismuth tungstate aqueous solution to obtain a reaction precursor solution. At this time, the Ru loading amount is 5%;
[0083] (7) adjusting the pH value of the reaction precursor solution to 12 with 2 mol / L NaOH solution;
[0084] (8) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 210° C. for 16 h.
[0085] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 8°C / min, and after the reaction, it was cooled to 50°C at a rate of 6°C / min, and then naturally cooled to room temperature;
[0086] After the hydrothermal reaction was completed, the product was taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in vacuum at 80°C for 12h, and then ground to obtain the Ru / BWO-5 photoanode.
[0087] Example 6: A method for preparing a ruthenium-modified bismuth tungstate photoanode is as follows:
[0088] (1) Weigh 2 mmol of Bi(NO3)3·5H2O, 1 mmol of Na2WO4·2H2O and 2 mmol of EDTA, all of which are analytical grade (AR);
[0089] (2) Add 2mmol Bi(NO3)3·5H2O to 20ml ethylene glycol, stir magnetically at room temperature, add 2mmol EDTA after stirring evenly, and stir until completely dissolved; add 1mmol Na2WO4·2H2O into deionized water, and in order to strictly control the filling ratio of the subsequent reaction, use 50ml of deionized water as the aqueous solution system, stir magnetically at room temperature, and add the sodium tungstate aqueous solution to the bismuth nitrate solution to obtain a reaction precursor solution;
[0090] (3) adjusting the pH value of the reaction precursor solution to 9 with 2 mol / L NaOH solution;
[0091] (4) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 210° C. for 16 h;
[0092] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 8°C / min, and after the reaction, it was cooled to 50°C at a rate of 6°C / min, and then naturally cooled to room temperature;
[0093] (5) After the hydrothermal reaction is completed, the product is taken out and washed with deionized water and anhydrous ethanol for four times by centrifugation, dried in a vacuum at 80° C. for 12 h, and then ground to obtain a BWO photoanode.
[0094] (6) Weigh 0.5 g of BWO material and dissolve it in 50 ml of deionized water and perform ultrasonic dispersion. Dissolve 0.025 g of RuCl3·3H2O and 0.0125 g of PVP in 20 ml of deionized water, mix thoroughly, and then add them to the bismuth tungstate aqueous solution to obtain a reaction precursor solution. At this time, the Ru loading amount is 5%;
[0095] (7) adjusting the pH value of the reaction precursor solution to 11 with 2 mol / L NaOH solution;
[0096] (8) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 180° C. for 20 h.
[0097] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 4°C / min, and after the reaction, it was cooled to 25°C at a rate of 3°C / min, and then naturally cooled to room temperature;
[0098] After the hydrothermal reaction was completed, the product was taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in vacuum at 80°C for 12h, and then ground to obtain the Ru / BWO-5 photoanode.
[0099] Example 7: A method for preparing a ruthenium-modified bismuth tungstate photoanode is as follows:
[0100] (1) Weigh 0.5 g of BWO material and dissolve it in 50 ml of deionized water and perform ultrasonic dispersion. Dissolve 0.025 g of RuCl3·3H2O and 0.0125 g of PVP in 20 ml of deionized water, mix thoroughly, and then add them to the bismuth tungstate aqueous solution to obtain a reaction precursor solution. At this time, the Ru loading amount is 5%;
[0101] (2) adjusting the pH value of the reaction precursor solution to 11 with 2 mol / L NaOH solution;
[0102] (3) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200° C. for 18 h.
[0103] The hydrothermal reaction temperature was raised to the reaction temperature at a rate of 5°C / min, and after the reaction, it was cooled to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0104] After the hydrothermal reaction was completed, the product was taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in vacuum at 70°C for 12h, and then ground to obtain the Ru / BWO-5 photoanode.
[0105] Comparative Example 1:
[0106] A method for preparing a bismuth tungstate photoanode comprises the following steps:
[0107] (1) Weigh 2 mmol of Bi(NO3)3·5H2O, 1 mmol of Na2WO4·2H2O and 2 mmol of EDTA, all of which are analytical grade (AR);
[0108] (2) Add 2 mmol Bi(NO3)3·5H2O to 20 ml ethylene glycol, stir magnetically at room temperature, add 2 mmol EDTA after stirring evenly, stir until completely dissolved, add 1 mmol Na2WO4·2H2O into deionized water, use 50 ml deionized water as the aqueous solution system to strictly control the filling ratio of the subsequent reaction, stir magnetically at room temperature, add the sodium tungstate aqueous solution to the bismuth nitrate solution, and obtain a reaction precursor solution;
[0109] (3) adjusting the pH value of the reaction precursor solution to 7 with 2 mol / L NaOH solution;
[0110] (4) The reaction precursor solution with adjusted pH value was transferred into a polytetrafluoroethylene reactor for hydrothermal reaction at a reaction temperature of 200°C for 18 hours; the hydrothermal reaction temperature was increased to the reaction temperature at a rate of 5°C / min, and after the reaction, the temperature was decreased to 40°C at a rate of 5°C / min, and then naturally cooled to room temperature;
[0111] After the hydrothermal reaction was completed, the product was taken out and washed three times with deionized water and anhydrous ethanol respectively by centrifugation, dried in vacuum at 70° C. for 12 h, and then ground to obtain a BWO photoanode.
[0112] Photoelectrocatalytic water splitting performance under simulated sunlight (AM 1.5G, 100mW·cm -2 ) was irradiated and tested with an electrochemical workstation (Chenhua CHI 660E). In this experiment, the photoelectrocatalytic properties of the prepared samples were measured in 0.1M Na2SO4 solution (pH = 7). During the test, the working electrode, reference electrode and counter electrode were photoanode, saturated calomel electrode (SCE) and platinum electrode, respectively, which were placed together in the electrolyte. The LSV curve was tested at -0.3~0.6V vs.RHE at a scan rate of 10mV / s. The measured potential and SCE reference electrode were transferred to the reversible hydrogen electrode (RHE) using the following formula:
[0113] E(vs.RHE)=E(vs.SCE)+0.2415+0.059pH
[0114] from Figure 1 It can be seen that the diffraction peaks of the prepared samples are completely consistent with the standard card of BWO (PDF#26-1044), indicating that Ru loading does not change the crystal structure of BWO.
[0115] from Figure 2 It can be seen that pure phase bismuth tungstate is stacked by two-dimensional nanosheets (Comparative Example 1). The sample loaded with 15% Ru was tested by SEM. Figure 3 It can be seen that compared with BWO, the morphology did not change significantly after loading 15% Ru, but some small particles were observed attached to the nanosheets, indicating that Ru was successfully loaded on BWO.
[0116] Figure 4a This is the LSV curve under visible light. It can be seen that the photoelectrocatalytic performance of Ru / BWO-15 photoanode is the best, and its current density is significantly better than that of pure phase bismuth tungstate. Figure 4b The LSV curve under dark conditions is significantly lower than that under visible light irradiation, but the performance of Ru / BWO-15 is still the best, which is mainly due to the synergy between a small amount of bulk Ru and the two-dimensional layered BWO in the sample prepared in Example 3, indicating that the ohmic contact between Ru and BWO can effectively improve the separation efficiency of carriers, so that the photocurrent density of the composite sample is improved, thereby greatly enhancing the performance of photoelectrocatalysis. As the ruthenium loading increases, the photocurrent density of the Ru / BWO-20 sample decreases instead, because the higher the Ru content, the higher the aggregation, which hinders the migration of photogenerated carriers.
Claims
1. A method for preparing a ruthenium-modified bismuth tungstate photoanode, characterized in that: The following steps are involved: Step (1): dissolving BWO in 50 ml of deionized water to form a bismuth tungstate aqueous solution, dissolving RuCl3·3H2O and PVP in 20 ml of deionized water and mixing thoroughly, and then adding the bismuth tungstate aqueous solution, wherein the mass ratio of PVP to RuCl3·3H2O is 1:2, and the mass ratio of RuCl3·3H2O to BWO is 0.05-0.2:1; adjusting the pH to 11-12 to obtain a reaction precursor solution; Step (2): the reaction precursor solution is transferred into a polytetrafluoroethylene reactor, and the reaction temperature is set to 180-210° C. and the reaction time is set to 16-20 h for hydrothermal reaction; Step (3): The product is taken out and washed by centrifugation with deionized water and anhydrous ethanol respectively, and then dried and ground to obtain a Ru / BWO photoanode.
2. The method for preparing a ruthenium-modified bismuth tungstate photoanode according to claim 1, characterized in that: The preparation of BWO in step (1) comprises the following steps: S1: Weigh Bi(NO3)3·5H2O, Na2WO4·2H2O and EDTA in a molar ratio of 2:1:2 respectively, dissolve Bi(NO3)3·5H2O in 20 ml of ethylene glycol, mix thoroughly, add EDTA and stir until completely dissolved to form a bismuth nitrate solution; dissolve Na2WO4·2H2O in 50 ml of deionized water to form a sodium tungstate solution; S2: Mix the bismuth nitrate solution and the sodium tungstate solution, add 2 mol / L NaOH solution to adjust the pH to 9-10, and then move it into a polytetrafluoroethylene reactor, set the reaction temperature to 180-210°C, and the time to 16-20h for hydrothermal reaction. The hydrothermal reaction temperature is increased to the reaction temperature at a rate of 4-8°C / min, and after the reaction, the temperature is reduced to 25-50°C at a cooling rate of 3-6°C / min, and then naturally cooled to room temperature. After taking out the product, it is centrifugally washed with deionized water and anhydrous ethanol for 3-5 times, vacuum dried at 60-80°C for 12h, and ground to obtain BWO.
3. The method for preparing a ruthenium-modified bismuth tungstate photoanode according to claim 1, characterized in that: The pH in step (1) is adjusted using a 2 mol / L NaOH solution.
4. The method for preparing a ruthenium-modified bismuth tungstate photoanode according to claim 1, characterized in that: The process of the hydrothermal reaction described in step (2) is to increase the temperature to the reaction temperature at a rate of 4 to 8°C / min, and after the reaction, cool the temperature to 25 to 50°C at a cooling rate of 3 to 6°C / min, and then naturally cool to room temperature.
5. The method for preparing a ruthenium-modified bismuth tungstate photoanode according to claim 1, characterized in that: The number of centrifugal washing in step (3) is 3 to 5 times.
6. The method for preparing a ruthenium-modified bismuth tungstate photoanode according to claim 1, characterized in that: The drying in step (3) is vacuum drying at 60-80°C for 12 hours.
7. A ruthenium-modified bismuth tungstate photoanode prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The structure of the ruthenium-modified bismuth tungstate photoanode is a stacked two-dimensional layered BWO nanosheet, and some small Ru particles are attached to the BWO nanosheet.