Aluminum alloy part surface anti-corrosion treatment method
Through thermoelectrochemical oxidation treatment and polishing technology, a dense oxide layer is formed, which solves the corrosion resistance of aluminum alloys in harsh environments, and achieves higher corrosion resistance and hardness. It is suitable for railway transportation, aerospace and other fields.
Patent Information
- Application Number
- CN202411112363.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
AI Technical Summary
The existing aluminum alloy surface anti-corrosion technology is difficult to meet the long-term corrosion resistance needs in harsh environments. Commonly used materials such as 7050 and other 7 series alloys are expensive and are not suitable for casting and processing. The coating is easy to fall off and has a short service life.
Using thermoelectrochemical oxidation treatment, aluminum alloy parts are immersed in an electrolyte containing silicate, polysilicate and hydroxide ions for pulse power-driven thermoelectric oxidation to form a dense oxide layer, and are polished by vibration or hand-held grinding. Disk polishing is used to improve surface finish.
The corrosion resistance of aluminum alloy parts in copper ion accelerated salt spray test for 240 hours and neutral salt spray test for more than 2000 hours is achieved, while improving hardness and surface finish, providing higher corrosion resistance and wear resistance.
Smart Images

Figure CN119061449A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment, in particular to a surface anti-corrosion treatment method for aluminum alloy parts (cast aluminum alloy parts or deformed aluminum alloy parts). Background Art
[0002] Aluminum alloy is an alloy with aluminum as the base material and a certain amount of other alloying elements added. It is one of the light metal materials and is widely used in aerospace, aviation, railway transportation, construction, electromechanical and other fields. The anti-corrosion performance of aluminum alloy is one of the key performances concerned in the above application fields. Under the conditions of most good service environments, aluminum alloy does not need additional anti-corrosion treatment. However, for some areas with particularly harsh service environments, such as areas around chemical enterprises, areas with corrosive substances such as salt, alkali and acid in the air, marine salt spray and dry-wet alternating environment, aerospace high-temperature thermal corrosion environment, etc., additional anti-corrosion treatment is required to meet the anti-corrosion performance requirements. Since aluminum alloy will form a natural oxide film in the air, the anti-corrosion technologies such as plasma spraying, paint coating, hot-dip galvanizing, etc. applicable to steel have problems such as weak bonding, easy detachment of coating, and short service life on aluminum alloy. Therefore, aluminum alloy parts are mainly formed through passivation, anodizing, micro-arc oxidation, thermo-electrochemical oxidation and other processes to form a dense oxide layer, thereby improving the anti-corrosion performance.
[0003] Invention patent application CN 113913893 A discloses a method for preparing a micro-arc oxidation ceramic film layer on the surface of 7050 aluminum alloy, wherein a DC pulse micro-arc oxidation device is used to perform micro-arc oxidation on the surface of 7050 aluminum alloy, cerium oxide and carbon nanotubes are added to the electrolyte, and the corrosion resistance of the prepared ceramic film layer is improved as characterized by the self-corrosion potential and the self-corrosion current. However, 7050 and other 7 series alloys are expensive and not suitable for casting and processing, and are not commonly used materials for aluminum alloy castings and forgings. Invention patent application CN 107345309 A discloses a method for preparing a high silicon aluminum alloy plasma electrolytic oxidation ceramic coating, including the steps of pretreatment, determining the negative cut-off voltage, preparing the coating, etc., and the current density is 5 to 20A / dm 2 , the positive and negative duty ratio is 10-50%, the frequency is 50-2500Hz, the processing time is 60-120min, and the oxide coating with a thickness of 40-90 microns is obtained, achieving the preparation of a coating with high hardness (1000Hv), low friction coefficient (0.05) for high-speed oil lubrication, and good corrosion resistance (neutral salt spray over 1400h). In this patent application, the application object is the die-cast aluminum material of the automobile engine cylinder block, but the claims and implementation methods do not give an accurate definition of "high silicon aluminum alloy", and the neutral salt spray 1400h is still insufficient for the use demand in the aforementioned harsh environment areas. Summary of the invention
[0004] In view of the above problems existing in the prior art, the present invention provides a method for anti-corrosion treatment of the surface of aluminum alloy parts. The aluminum alloy parts treated by the method of the present invention have higher corrosion protection effect and at the same time have better hardness and surface finish.
[0005] The technical solution of the present invention is as follows:
[0006] The purpose of the present invention is to provide a method for surface anticorrosion treatment of aluminum alloy parts, comprising the following steps:
[0007] (1) Check cast or forged aluminum alloy parts to ensure that there is no obvious damage, oil stains, or oxide scale on the surface;
[0008] (2) immersing the aluminum alloy parts in an electrolyte for thermal electrochemical oxidation treatment;
[0009] (3) Polishing the aluminum alloy parts processed in step (2).
[0010] In one embodiment of the present invention, in step (1), the material of the aluminum alloy part is ZL101A, 2024 or 6082.
[0011] In one embodiment of the present invention, in step (2), the electrolyte includes silicate ions, polysilicate ions, and hydroxide ions; wherein the silicate ion concentration is 4-20 mol / L, and the SiO3 2- Calculate; the hydroxide ion concentration is 2-8mol / L.
[0012] In one embodiment of the present invention, in step (2), the electrolyte contains potassium ions and sodium ions to keep the solution in electrical balance.
[0013] In one embodiment of the present invention, in step (2), during the thermoelectric oxidation treatment: the aluminum alloy part is connected to the anode of the pulse power supply, and the metal electrode is connected to the cathode of the pulse power supply.
[0014] In one embodiment of the present invention, in step (2), the thermoelectric oxidation treatment conditions are: the positive current of the pulse power supply is 8-14A / dm 2 , negative current is 6-16A / dm 2 , the duty cycle is 70-100%, and the reaction time is 40 to 90 minutes.
[0015] In one embodiment of the present invention, in step (3), the polishing method is vibration polishing or handheld grinding disc polishing; and the polishing time is 1-6 minutes.
[0016] In one embodiment of the present invention, the polishing abrasive or grinding disk is a resin abrasive or a silicon carbide abrasive.
[0017] In one embodiment of the present invention, the abrasive is in the shape of a sphere, a quadrangular pyramid, a pyramid or a cylinder.
[0018] In one embodiment of the present invention, the thickness of the surface oxide layer of the aluminum alloy part after polishing is 90-110 μm, and the surface roughness Ra is 1.5-2.5 μm.
[0019] In one embodiment of the present invention, after the surface anti-corrosion treatment of aluminum alloy parts, the protection level of the copper ion accelerated salt spray test for 240 hours is Rp7 or above, and the protection level of the neutral salt spray test for 2000 hours is Rp7 or above, and the appearance is kept intact; the Vickers hardness of the ZL101A aluminum alloy surface is ≥600HV, and the Vickers hardness of the 2024 aluminum alloy surface is ≥1000HV.
[0020] The beneficial technical effects of the present invention are:
[0021] The present invention develops a new method for surface anti-corrosion treatment of aluminum alloy parts. The method can be generally applied to aluminum alloy castings and forgings, such as ZL101A, 2024, 6082 and other materials. After treatment, the method has higher corrosion protection effect, and at the same time has better hardness and surface finish. The method is suitable for applications with higher anti-corrosion performance requirements in the fields of railway transportation, aerospace, construction electromechanical, etc.
[0022] The method of the present invention can be applied to common cast or forged aluminum alloy grades such as ZL101A, 2024, 6082, etc. The sample coating thickness obtained in a relatively short processing time exceeds 90 μm, and can reach up to 110 μm at most. The corrosion resistance effect reaches 240 hours of copper ion accelerated salt spray test and more than 2000 hours of neutral salt spray test. The protection capability exceeds the existing technology, and it can also have high hardness and smooth surface, providing wear resistance and hydrophobicity. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a photo of the double-ear sample of the cast aluminum alloy ZL101A sleeve after treatment in Example 1;
[0024] Figure 2 This is a photo of the treated cast aluminum alloy ZL101A sleeve double-ear sample after 240 hours of copper ion accelerated salt spray test in Example 1;
[0025] Figure 3 This is a SEM photo of the treated cast aluminum alloy ZL101A sleeve double-ear sample in Example 1 after 2000 hours of neutral salt spray test;
[0026] Figure 4 This is a photo of the cast aluminum alloy 2024 round cake sample after treatment in Example 2;
[0027] Figure 5These are photos of forged aluminum alloy 6082 round cake samples after treatment in Example 3 (4 samples are shown in the figure). DETAILED DESCRIPTION
[0028] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0029] The copper ion accelerated salt spray test and neutral salt spray test performed in the embodiments are carried out in accordance with GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test".
[0030] Embodiment 1:
[0031] A method for anti-corrosion treatment of the surface of aluminum alloy parts, the specific steps are:
[0032] (1) Check the ZL101A aluminum alloy sleeve double-ear sample to ensure that there is no obvious damage, oil stain, or oxide scale on the surface;
[0033] (2) preparing an electrolyte, the electrolyte comprising: silicate and polysilicate ions, hydroxide ions, wherein the silicate ions (in the form of SiO3 2- The concentration of ions is 4 mol / L, the concentration of hydroxide ions is 8 mol / L, and the concentration of sodium ions is 16 mol / L;
[0034] (3) Connecting the ZL101A aluminum alloy sleeve binaural sample to the anode of a pulse power supply, and connecting the metal electrode to the cathode of a pulse power supply, immersing the ZL101A aluminum alloy sleeve binaural sample in the electrolyte prepared in step (2) for thermoelectrochemical oxidation treatment; the conditions of the thermoelectrochemical oxidation treatment are: the positive current of the pulse power supply is 8A / dm 2 , negative current is 16A / dm 2 , the duty cycle is 70% and the reaction time is 50 minutes;
[0035] (4) The ZL101A aluminum alloy sleeve double-ear sample obtained after the treatment in step (3) is subjected to vibration polishing. The polishing time is 2 minutes, and the polishing abrasive is a tetrahedral resin abrasive.
[0036] After the treatment in this embodiment, the surface of the ZL101A aluminum alloy sleeve double-ear sample is formed with a relatively smooth gray-white coating (such as Figure 1 ); Copper ion accelerated salt spray test 240 hours protection level is Rp7 or above (such as Figure 2 ), neutral salt spray test for 2000 hours to keep the coating intact (such as Figure 3 ), all keep their appearance intact; the average Vickers hardness of the aluminum alloy surface is 650HV.
[0037] Embodiment 2:
[0038] A method for anti-corrosion treatment of the surface of aluminum alloy parts, the specific steps are:
[0039] (1) Check the aluminum alloy 2024 round cake sample (diameter 60mm, thickness 8mm) to ensure that there is no obvious damage, oil stain, or oxide scale on the surface;
[0040] (2): Prepare an electrolyte, which includes silicate and polysilicate ions and hydroxide ions, wherein the silicate ions (in the form of SiO3 2- The concentration of hydrogen ion is 8mol / L, the concentration of hydroxide ion is 5mol / L, the concentration of sodium ion is 16mol / L, and the concentration of potassium ion is 5mol / L;
[0041] (3) Connecting the aluminum alloy 2024 round cake sample to the anode of the pulse power supply, connecting the metal electrode to the cathode of the pulse power supply, and immersing the aluminum alloy 2024 round cake sample in the electrolyte prepared in step (2) for thermoelectrochemical oxidation treatment; the conditions of the thermoelectrochemical oxidation treatment are: the positive current of the pulse power supply is 8A / dm 2 , negative current is 8A / dm 2 , the duty cycle is 100%, and the reaction time is 90 minutes;
[0042] (4) The aluminum alloy 2024 round cake sample obtained after the treatment in step (3) was polished with a handheld grinding wheel for 6 minutes, and the polishing abrasive was a silicon carbide grinding wheel.
[0043] After the treatment in this embodiment, the surface of the aluminum alloy 2024 round cake sample is formed with a smooth black coating with an average thickness of 70 μm and a surface roughness Ra of 1.5 μm (such as Figure 4 ), the protection level of the copper ion accelerated salt spray test for 240 hours is Rp7 or above; the average Vickers hardness of the aluminum alloy surface is 1000HV.
[0044] Embodiment 3:
[0045] A method for anti-corrosion treatment of the surface of aluminum alloy parts, the specific steps are:
[0046] (1) Check the aluminum alloy 6082 round cake sample (diameter 30 mm, thickness 8 mm) to ensure that there is no obvious damage, oil stain, or oxide scale on the surface;
[0047] (2) preparing an electrolyte, the electrolyte comprising: silicate and polysilicate ions, hydroxide ions, wherein the silicate ions (in the form of SiO3 2- The concentration of hydrogen ion is 6mol / L, the concentration of hydroxide ion is 5mol / L, the concentration of sodium ion is 12mol / L, and the concentration of potassium ion is 5mol / L;
[0048] (3) The aluminum alloy 6082 round cake sample is connected to the anode of the pulse power supply, and the metal electrode is connected to the cathode of the pulse power supply, and the aluminum alloy 6082 round cake sample is immersed in the electrolyte prepared in step (2) for thermoelectrochemical oxidation treatment; the conditions of the thermoelectrochemical oxidation treatment are: the positive current of the pulse power supply is 8A / dm 2 , negative current is 8A / dm 2 , the duty cycle is 80% and the reaction time is 90 minutes;
[0049] (4) The aluminum alloy 6082 round cake sample obtained after the treatment in step (3) is polished with a handheld grinding wheel for 2 minutes, and the polishing abrasive is a silicon carbide grinding wheel.
[0050] After the treatment in this embodiment, the aluminum alloy 6082 round cake sample has a smooth gray-white coating with an average thickness of 100 μm and a surface roughness Ra of 1.5 μm (such as Figure 5 ); the protection level of the copper ion accelerated salt spray test for 240 hours is Rp7 or above; the average Vickers hardness of the aluminum alloy surface is 700HV.
[0051] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for anti-corrosion treatment of the surface of aluminum alloy parts, characterized in that: The steps include: (1) Check cast or forged aluminum alloy parts to ensure that there is no obvious damage, oil stains, or oxide scale on the surface; (2) immersing the aluminum alloy parts in an electrolyte for thermal electrochemical oxidation treatment; (3) Polishing the aluminum alloy parts processed in step (2).
2. The method for anticorrosion treatment of the surface of aluminum alloy parts according to claim 1, characterized in that: In step (1), the material of the aluminum alloy part is ZL101A, 2024 or 6082.
3. The method for anticorrosion treatment of the surface of aluminum alloy parts according to claim 1, characterized in that: In step (2), the electrolyte includes silicate ions, polysilicate ions, and hydroxide ions; wherein the concentration of silicate ions is 4-20 mol / L, and the concentration of SiO3 2- Calculate; the hydroxide ion concentration is 2-8mol / L.
4. The method for anticorrosion treatment of the surface of aluminum alloy parts according to claim 1, characterized in that: In step (2), the electrolyte contains potassium ions and sodium ions to keep the solution in electrical balance.
5. The method for anti-corrosion treatment of the surface of aluminum alloy parts according to claim 1, characterized in that: In step (2), during the thermoelectric oxidation treatment: the aluminum alloy part is connected to the anode of the pulse power supply, and the metal electrode is connected to the cathode of the pulse power supply.
6. The method for anticorrosion treatment of the surface of aluminum alloy parts according to claim 1, characterized in that: In step (2), the thermoelectric oxidation treatment conditions are: the positive current of the pulse power supply is 8-14A / dm 2 , negative current is 6-16A / dm 2 , the duty cycle is 70-100%, and the reaction time is 40-90min.
7. The method for anticorrosion treatment of the surface of aluminum alloy parts according to claim 1, characterized in that: In step (3), the polishing method is vibration polishing or handheld grinding disc polishing; the polishing time is 1-6 minutes.
8. The method for anticorrosion treatment of the surface of aluminum alloy parts according to claim 7, characterized in that: The polishing abrasive or grinding disc is resin abrasive or silicon carbide abrasive.
9. The method for anticorrosion treatment of the surface of aluminum alloy parts according to claim 7, characterized in that: The abrasive shape is spherical, quadrangular pyramidal, pyramidal or cylindrical.
10. The method for anti-corrosion treatment of the surface of aluminum alloy parts according to claim 1, characterized in that: After polishing, the surface oxide layer thickness of the aluminum alloy parts is 90-110μm, and the surface roughness Ra is 1.5-2.5μm.
Citation Information
Patent Citations
Preparation method of high-silicon aluminum alloy plasma electrolytic oxidation ceramic coating
CN107345309A
Preparation method of 7050 aluminum alloy surface micro-arc oxidation ceramic film layer
CN113913893A