Carbon fiber, preparation method thereof and composite material
By employing controlled carbonization treatments with temperature gradients and tensions, the method addresses the issue of fiber entanglement in low-gram-weight carbon fibers, enhancing yarn spreading and mechanical properties for aerospace applications.
Patent Information
- Application Number
- CN202411329557.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
Low-gram-weight carbon fiber composite materials face challenges in achieving uniform yarn spreading and maintaining mechanical properties due to high entanglement during the carbonization process, which affects their performance in aerospace applications.
A method involving sequential low-temperature and high-temperature carbonization treatments with controlled temperature gradients and tensions to reduce fiber entanglement, combined with pre-oxidation and post-treatments, ensures uniform yarn spreading and improved tensile strength.
The method results in carbon fibers with reduced entanglement and enhanced yarn spreading performance, leading to improved mechanical properties and reduced weight in composite materials.
Smart Images

Figure BDA0005056428270000071 
Figure BDA0005056428270000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of carbon fiber manufacturing, and in particular to a carbon fiber and a preparation method thereof, and a composite material. Background Art
[0002] Low-gram-weight carbon fiber composite materials refer to composite materials containing low-gram-weight carbon fibers (less than 100g / m). Compared with conventional gram-weight composite materials, low-gram-weight carbon fiber composite materials have obvious weight advantages and can meet the application fields with higher requirements for lightweight. They can achieve the purpose of reducing weight while maintaining strength and stiffness. Therefore, they are widely used in the aerospace field. They can be used to manufacture aircraft structural parts, spacecraft components and drones, etc., to improve the performance and fuel efficiency of aircraft. They have broad application prospects and market demand.
[0003] Compared with conventional gram-weight composite materials, low gram-weight carbon fiber composite materials have higher requirements on the yarn spreading performance of carbon fiber during the preparation process. The carbon fiber is required to be evenly dispersed in the resin matrix to avoid agglomeration or aggregation. Ensuring the uniform yarn spreading of carbon fiber is the key difficulty in the preparation process. Summary of the invention
[0004] To solve the above problems, the purpose of the embodiments of the present application includes providing a carbon fiber and a preparation method thereof, as well as a low-weight carbon fiber composite material, which can optimize the fiber yarn spreading performance by reducing the fiber entanglement degree and ensure the uniform yarn spreading of the carbon fiber.
[0005] In a first aspect, the present application provides a method for preparing carbon fiber, comprising the following steps:
[0006] The pre-oxidized fiber is subjected to low-temperature carbonization treatment and high-temperature carbonization treatment in sequence to obtain carbonized fiber; the carbonized fiber is subjected to post-treatment to obtain carbon fiber;
[0007] The low-temperature carbonization treatment includes heating the pre-oxidized fiber at a gradient temperature from 400°C to 900°C, and providing a plurality of carbonization temperature zones within the range of 500-700°C, so that there are a plurality of temperature gradients within the range of 500-700°C; the tension applied during the low-temperature carbonization treatment is 4-12N;
[0008] The high temperature carbonization treatment includes subjecting the low carbon fiber that has undergone the low temperature carbonization treatment to a gradient heating from 1000° C. to 1600° C.
[0009] During the low-temperature carbonization treatment (400℃-900℃), the carbon fiber undergoes a violent reaction inside, and the fiber orientation degree is significantly reduced. At around 600℃, the degree of entanglement inside the fiber increases sharply. The increase in entanglement indicates that the entanglement of the carbon fiber tows increases, which will cause the yarn spreading performance and tensile strength of the carbon fiber to decrease. Low-gram-weight carbon fiber composite materials mainly refer to carbon fibers with small gram-weight per unit area (i.e., a small number of corresponding roots) that can be evenly and comprehensively covered after yarn spreading. Therefore, the increase in entanglement will result in the need to use more carbon fibers when preparing low-gram-weight carbon fibers, so that their gram-weight and mechanical properties do not meet the requirements. The present application can effectively reduce the degree of entanglement inside the carbon fiber tows by setting multiple temperature gradients in the range of 500-700℃, and combining the tension in the low-temperature carbonization treatment process, so as to achieve the improvement of carbon fiber yarn spreading performance and tensile strength, thereby reducing the weight of the prepreg to improve the performance of low-gram-weight carbon fiber composite materials.
[0010] In some embodiments of the present application, 3-4 carbonization temperature zones are provided in the range of 500-700°C, and the temperature difference between each carbonization temperature zone is 50-150°C.
[0011] In the above technical solution, by adjusting the carbonization temperature quantity and temperature difference, the intensity of the reaction of the internal structure of the carbon fiber can be further mitigated, and the fiber entanglement degree can be effectively reduced.
[0012] In some embodiments of the present application, the total time of the low-temperature carbonization treatment is 115-150 seconds. Optionally, the low-temperature carbonization treatment is carried out in nitrogen, and the oxygen content in the nitrogen is less than 2 ppm. Optionally, the pre-oxidized fiber is treated for the same time in each carbonization temperature zone.
[0013] In the above technical scheme, by regulating the time of low-temperature carbonization treatment, the degree of thermal cracking and recombination reaction of the low carbon fibers can be correspondingly regulated, and then the carbon structure and mechanical properties can be regulated. By making the pre-oxidized fibers move at a uniform speed and making the treatment time in each carbonization temperature zone equal, the consistency and stability of the low carbon fiber structure can be ensured.
[0014] In some embodiments of the present application, the tension applied by the high temperature carbonization treatment is 40-60N.
[0015] In the above technical solution, controlling the tension within a suitable range during the high-temperature carbonization treatment can slow down the reaction rate and increase the density of the carbon fibers.
[0016] In some embodiments of the present application, the total time of the high temperature carbonization treatment is 90-110 seconds. Optionally, the high temperature carbonization treatment is performed in nitrogen, and the oxygen content in the nitrogen is less than 1 ppm.
[0017] In the above technical solution, by controlling the time and atmosphere of the low-temperature carbonization treatment and the high-temperature carbonization treatment, the internal structure of the fiber can be optimized to the greatest extent, and the density and performance of the carbon fiber can be improved.
[0018] In some embodiments of the present application, the line speed of the pre-oxidized fiber is 420-520 m / h.
[0019] In the above technical solution, the pre-oxidized fiber is kept running stably at a constant line speed during the carbonization process, so as to ensure the stability and consistency of the carbon fiber.
[0020] In some embodiments of the present application, the method for preparing pre-oxidized fibers comprises the following steps:
[0021] The polyacrylonitrile fiber is subjected to a pre-oxidation reaction to obtain a pre-oxidized fiber;
[0022] The pre-oxidation step includes heating the polyacrylonitrile fiber from 215° C. to 255° C., with a temperature increase gradient of 15-25° C., a pre-oxidation time of 60-90 minutes, and an applied tension of 16-21N.
[0023] In the above technical scheme, by controlling the pre-oxidation reaction conditions within the above range, the oxidation reaction of the fiber can be promoted, the fiber structure can be improved, the thermal stability and crystallinity of the fiber can be enhanced, and an excellent foundation can be provided for subsequent carbonization treatment, thereby obtaining high-quality carbon fiber.
[0024] In some embodiments of the present application, the post-processing includes: sequentially performing surface treatment, water washing, sizing, drying and winding on the carbonized fiber to obtain the carbon fiber;
[0025] Optionally, the surface treatment comprises: electrochemically treating the carbonized fiber body in an alkaline electrolyte.
[0026] In a second aspect, an embodiment of the present application provides a carbon fiber prepared by the above-mentioned preparation method.
[0027] In a third aspect, an embodiment of the present application also provides a composite material, comprising a matrix resin and the above-mentioned carbon fiber.
[0028] Since the carbon fiber has excellent yarn spreading performance and tensile strength, a composite material with low grammage and excellent mechanical properties can be prepared. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below.
[0030] The present invention provides a carbon fiber, and a preparation method thereof comprises the following steps:
[0031] S110: performing a pre-oxidation reaction on the polyacrylonitrile fiber to obtain a pre-oxidized fiber. The pre-oxidation reaction step includes heating the polyacrylonitrile fiber at a temperature from 215° C. to 255° C., with a temperature increase gradient of 15-25° C., a pre-oxidation reaction time of 60-90 minutes, and an applied tension of 16-21N.
[0032] Among them, the density of polyacrylonitrile fiber can be 1.18g / cm 3 The diameter of the single fiber is 8.6 μm, and the density of the corresponding pre-oxidized fiber can be 1.341.42 g / cm 3 As an example, the density of the pre-oxidized fiber may be 1.37 g / cm 3 .
[0033] Preferably, the temperature gradient is 20° C., the pre-oxidation reaction time is 60 min, the applied tension is 19 N, and the linear speed of the polyacrylonitrile fiber tow is 420-520 m / h.
[0034] S120: The pre-oxidized fiber is subjected to low-temperature carbonization treatment and high-temperature carbonization treatment in sequence to obtain carbonized fiber. The low-temperature carbonization treatment includes gradient heating of the pre-oxidized fiber from 400°C to 900°C, and multiple carbonization temperature zones are provided in the range of 500-700°C, so that there are multiple temperature gradients in the range of 500-700°C, and the tension of the low-temperature carbonization treatment is 4-12N; the high-temperature carbonization treatment includes gradient heating of the low carbon fiber subjected to the low-temperature carbonization treatment from 1000°C to 1600°C.
[0035] During the low temperature carbonization process, 3 or 4 carbonization temperature zones are set within the range of 500-700° C., and the temperature difference between each carbonization temperature zone can be 50-150° C. The total time of the low temperature carbonization process is 115-150 seconds, and the low temperature carbonization process is carried out in nitrogen, and the oxygen content in the nitrogen is less than 2ppm.
[0036] During the high temperature carbonization process, the applied tension is 40-60 N. The total time of the high temperature carbonization process is 90-110 seconds, and the high temperature carbonization process is carried out in nitrogen, and the oxygen content in the nitrogen is less than 1 ppm.
[0037] It should be noted that during the low-temperature carbonization treatment and the high-temperature carbonization treatment, the linear speed of the pre-oxidized fiber is constant at 420-520 m / h. The length of each carbonization temperature zone is the same, so the time the pre-oxidized fiber stays in each carbonization temperature zone is also the same, which can ensure the stability and consistency of the carbon fiber.
[0038] S130: performing surface treatment, water washing, sizing, drying and winding on the carbonized fiber in sequence to obtain carbon fiber.
[0039] The surface treatment may include: performing electrochemical treatment on the carbonized fiber body in an alkaline electrolyte.
[0040] In addition, the present application also provides a composite material, including a composite matrix resin and carbon fibers, wherein the matrix resin may be an epoxy resin.
[0041] The features and properties of the present application are further described in detail below in conjunction with specific examples. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0042] Example 1
[0043] This embodiment provides a carbon fiber, and the preparation method thereof comprises the following steps:
[0044] (1) Density is 1.18 g / cm 3 , polyacrylonitrile fiber with a single fiber diameter of 8.6 μm was subjected to a preoxidation reaction to obtain a preoxidized fiber body; wherein the starting temperature of the preoxidation reaction was 215°C, the ending temperature was 255°C, the temperature gradient was 20°C, the running speed of the polyacrylonitrile fiber bundle was 520 m / h, the preoxidation residence time was 60 min, and during the preoxidation reaction, the tension applied to the bundle was 19 N, and the density of the obtained preoxidized fiber was 1.370 g / cm 3 .
[0045] (2) The pre-oxidized fiber body in step (1) is subjected to low-temperature carbonization treatment in a low-temperature furnace (low-temperature carbonization temperature zone). In the low-temperature carbonization treatment, four temperature zones are set within a temperature range of 500-700°C, namely 500°C, 560°C, 630°C, and 700°C. The total residence time of the fiber is 115 seconds, and the tension applied to the pre-oxidized fiber body is 9N. Nitrogen is introduced into the low-temperature furnace, and the oxygen content of the nitrogen in the low-temperature furnace is less than 2ppm.
[0046] The low carbon fiber obtained by low temperature carbonization treatment is then subjected to high temperature carbonization treatment in a high temperature furnace (high temperature carbonization temperature zone). In the high temperature carbonization treatment, the residence time of the fiber is 90 seconds, and the tension applied to the pre-oxidized fiber body is 50 N. Nitrogen is introduced into the high temperature furnace, and the oxygen content of the nitrogen in the high temperature furnace is less than 1 ppm.
[0047] (3) The carbonized fibers are sequentially subjected to surface treatment, water washing, sizing, drying, and winding to obtain carbon fibers.
[0048] When the pre-oxidized fiber body passes through the low-temperature furnace and the high-temperature furnace in turn, the temperature of each temperature zone in each furnace is preset first, so that the temperature of each temperature zone reaches the preset value, and then the pre-oxidized fiber body starts to run at a constant linear speed (520m / h) and passes through the low-temperature furnace and the high-temperature furnace in turn.
[0049] Example 2
[0050] This embodiment provides a carbon fiber, and its preparation method is substantially the same as the preparation method in Embodiment 1, except that:
[0051] In step (2), three temperature zones are set within the temperature range of 500-700°C, namely 540°C, 610°C and 700°C.
[0052] Example 3
[0053] This embodiment provides a carbon fiber, and its preparation method is substantially the same as the preparation method in Embodiment 1, except that:
[0054] In step (2), the tension applied to the pre-oxidized fiber body during the low-temperature carbonization treatment is 7N.
[0055] Example 4
[0056] This embodiment provides a carbon fiber, and its preparation method is substantially the same as the preparation method in Embodiment 1, except that:
[0057] In step (2), the tension applied to the pre-oxidized fiber body during the low-temperature carbonization treatment is 11N.
[0058] Comparative Example 1
[0059] This comparative example provides a carbon fiber, and its preparation method is substantially the same as the preparation method in Example 1, except that:
[0060] In step (2), four carbonization temperature zones are set within the temperature range of 400-500°C, namely 420°C, 440°C, 460°C and 480°C, and no carbonization temperature zone is set within the temperature range of 500-700°C.
[0061] Comparative Example 2
[0062] This comparative example provides a carbon fiber, and its preparation method is substantially the same as the preparation method in Example 1, except that:
[0063] In step (2), the tension applied to the pre-oxidized fiber body during the low-temperature carbonization treatment is 13N.
[0064] Comparative Example 3
[0065] This comparative example provides a carbon fiber, and its preparation method is substantially the same as the preparation method in Example 1, except that:
[0066] In step (2), the tension applied to the pre-oxidized fiber body during the low-temperature carbonization treatment is 3N.
[0067] Test example
[0068] This test example tests the performance of the carbon fiber products provided in Examples 1-4 and Comparative Examples 1-3, and at the same time spreads the carbon fiber to observe its spreading properties. The specific test method is as follows:
[0069] (1) Tensile strength: Tested in accordance with GB / T 3362 test standard;
[0070] (2) Intertwining degree: Hang a hook with a weight of 10g inside the tow and let it slide freely. It will get stuck due to intertwining at a certain position. Record the sliding distance, take it out and hang it again at the same position, record the sliding distance of each 1 meter slide, and restart the test after reaching 1m. After 100 sliding distance data, remove the 20 data before and after, and take the average of the remaining 60 values. Divide 100 by the average of 60 values to get the intertwining degree.
[0071] (3) Yarn spreading width: The yarn is spread through a yarn spreading machine and the width is measured after the yarn is spread.
[0072] The above performance test results are shown in Table 1.
[0073] Table 1 Carbon fiber performance test results of the embodiments and comparative examples
[0074]
[0075]
[0076] It can be seen from Table 1 that in Examples 1-4, by setting multiple carbonization temperature zones during the low-temperature carbonization treatment and correspondingly controlling the tension within a specific range, the low-carbon fibers obtained after the low-temperature carbonization treatment have a lower degree of entanglement, and the final carbon fibers have a higher yarn width and tensile strength.
[0077] In Comparative Example 1, a temperature gradient of 4 is set within the temperature range of 400-500°C instead of 500-700°C, so that during the carbonization treatment in this range, in the temperature range of about 600°C, the internal reaction of the fiber is violent, the entanglement degree increases sharply, and at the same time, due to the violent reaction, a large amount of exhaust gas escapes, resulting in a large number of holes in the fiber microscopic interior. Ultimately, the mechanical properties of the carbon fiber are greatly reduced, and the yarn width is also significantly reduced.
[0078] In Comparative Example 2, four temperature gradients were set within the temperature range of 500-700°C. However, due to the excessive tension, the internal single filaments of the whole bundle of low-carbon fibers were broken, resulting in a decrease in the tensile strength performance of the whole bundle of carbon fibers. The tensile strength performance of the carbon fibers was reduced, resulting in a decrease in the performance of the prepared composite.
[0079] In Comparative Example 3, the tension set during the low-temperature carbonization process is too small, only 3N. Due to the escape of a large amount of exhaust gas during the low-temperature carbonization process, a large number of defects and pores appear inside the fiber. The appropriate tension can suppress the generation of pores under the action of drafting, but too low tension is difficult to achieve. Therefore, although 4 temperature gradients are set within the temperature range of 500-700℃ to smooth the internal reaction of the fiber, the tensile strength of the carbon fiber still shows a significant decrease in the end, the entanglement degree of the low carbon fiber is also significantly increased, and the corresponding yarn width is reduced.
[0080] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
Claims
1. A method for preparing carbon fiber, characterized in that: The following steps are involved: The pre-oxidized fiber is subjected to low-temperature carbonization treatment and high-temperature carbonization treatment in sequence to obtain carbonized fiber; Post-processing the carbonized fiber to obtain carbon fiber; The low-temperature carbonization treatment includes heating the pre-oxidized fiber at a gradient temperature from 400°C to 900°C, and providing a plurality of carbonization temperature zones within the range of 500-700°C, so that there are a plurality of temperature gradients within the range of 500-700°C; the tension applied by the low-temperature carbonization treatment is 4-12N; The high temperature carbonization treatment includes performing gradient heating from 1000° C. to 1600° C. on the low carbon fiber that has undergone the low temperature carbonization treatment.
2. The preparation method according to claim 1, characterized in that: There are 3-4 carbonization temperature zones in the range of 500-700°C, and the temperature difference between each carbonization temperature zone is 50-150°C.
3. The preparation method according to claim 1 or 2, characterized in that: The total time of the low temperature carbonization treatment is 115-150 seconds; Optionally, the low-temperature carbonization treatment is carried out in nitrogen, and the oxygen content in the nitrogen is less than 2 ppm; Optionally, the pre-oxidized fiber is treated in each of the carbonization temperature zones for the same time.
4. The preparation method according to claim 1, characterized in that: The tension applied by the high temperature carbonization treatment is 40-60N.
5. The preparation method according to claim 1 or 4, characterized in that: The total time of the high temperature carbonization treatment is 90-110 seconds; Optionally, the high-temperature carbonization treatment is carried out in nitrogen, and the oxygen content in the nitrogen is less than 1 ppm.
6. The preparation method according to claim 1, characterized in that: The pre-oxidized fiber runs at a linear speed of 420-520 m / h.
7. The preparation method according to claim 1, characterized in that: The method for preparing the pre-oxidized fiber comprises the following steps: Performing a pre-oxidation reaction on polyacrylonitrile fiber to obtain the pre-oxidized fiber; The pre-oxidation step includes heating the polyacrylonitrile fiber from 215° C. to 255° C., with a temperature increase gradient of 15-25° C., the pre-oxidation time is 60-90 minutes, and the applied tension is 16-21N.
8. The preparation method according to claim 1, characterized in that: The post-treatment comprises: performing surface treatment, washing, sizing, drying and winding on the carbonized fiber in sequence to obtain the carbon fiber; Optionally, the surface treatment comprises: electrochemically treating the carbonized fiber body in an alkaline electrolyte.
9. A carbon fiber, characterized in that: The method is prepared according to any one of claims 1 to 8.
10. A composite material, characterized in that: The invention comprises a matrix resin and the carbon fiber as claimed in claim 9.
Citation Information
Patent Citations
High strength polyacrylonitrile-base carbon fibers having structured surface grooves, and preparation method thereof
CN102733009A
6k polyacrylonitrile-based carbon fibre manufacturing method
CN103233297A
Polyacrylonitrile-based carbon fiber and preparation method thereof
CN110106585A
Carbon fiber and preparation method thereof
CN117187989A
Cited By
Device and method for detecting interlacing degree of fiber bundles
CN119936368A
A device and method for detecting the interlacing degree of a fiber bundle
CN119936368B