Sample taking and preparing method for rapidly and accurately measuring nitrogen content in steel billet
The problem of measuring the nitrogen content hysteresis in the prior art was solved by taking samples from the crystallizer through a vacuum sampler and quickly analyzing it with an oxygen and nitrogen analyzer, and the problem of measuring the nitrogen content in the existing technology was solved, which achieved rapid and accurate measurement of the nitrogen content, ensuring timely guidance of the steelmaking production process .
Patent Information
- Application Number
- CN202410879632.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, when determining the nitrogen content in steel billets, steel blocks need to be cut and sampled through machining lathes, resulting in lagging results, and the steelmaking production process cannot be guided in time, affecting the quality control of steel billets.
Use a vacuum sampler to take samples from the crystallizer, and use the immersion water outlet and the protective slag-covered crystallizer water level to ensure that the sample does not come into contact with the air. Use an oxygen and nitrogen analyzer to quickly analyze the nitrogen content to provide accurate billet nitrogen content data.
It realizes rapid and accurate determination of the nitrogen content in the steel billet, ensures that the nitrogen content of the sample is consistent with the nitrogen content in the steel billet, and promptly guides the steelmaking production process, solving the problem of lag in the measurement results.
Smart Images

Figure CN119064055A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of steel production detection, in particular to a sampling method for quickly and accurately determining the nitrogen content in a steel billet. Background Art
[0002] The nitrogen content in steel has a complex relationship with the performance of steel. On the one hand, with the increase of nitrogen content, the strength of steel can be significantly improved, but the plasticity, especially toughness, is significantly reduced, weldability is deteriorated, cold brittleness is aggravated, and aging tendency, cold brittleness and hot brittleness are increased, which damages the welding performance and cold bending performance of steel. Therefore, the nitrogen content in steel should be reduced and limited as much as possible. It is generally stipulated that the nitrogen content should not be higher than 180PPm; on the other hand, nitrogen can reduce its adverse effects and improve the performance of steel in combination with elements such as niobium, vanadium, and titanium. It can be used as an alloying element of low-alloy steel. Properly increasing the content of N can reduce the use of other alloys and effectively reduce costs. Accurately controlling the nitrogen content in steel is an important issue in metallurgical production.
[0003] In the existing method of measuring the nitrogen content in a steel billet, a steel block is usually cut from the steel billet and then processed into a smooth steel column by a machining lathe. The sampling cycle is long and the measurement result of the nitrogen content in the steel billet is obtained with a lag, which cannot guide the steelmaking production process to control the nitrogen content of the steel billet in time, and is not conducive to the quality control of the steel billet. Summary of the invention
[0004] The object of the present invention is to provide a sampling method for quickly and accurately determining the nitrogen content in a steel billet, so as to solve the problem that in the existing method of determining the nitrogen content in a steel billet, a steel block is usually cut from the steel billet and a sample is processed by a machining lathe, and the measurement result is delayed, so that the steelmaking production process cannot be guided in time to control the nitrogen content of the steel billet.
[0005] To achieve the above object, the present invention provides a method for sampling and preparing a steel billet for rapid and accurate determination of nitrogen content, which is implemented by the following steps: S1. Use an immersed nozzle to pour the molten steel in the tundish into the crystallizer, and keep the nozzle at the center of the steel liquid level in the crystallizer; S2. The molten steel surface of the crystallizer is covered by protective slag; S3. Use a vacuum sampler to take samples. The vacuum sampler has a round bubble at one end. During the sampling operation, use a clamping tool to clamp and fix the vacuum sampler, so that the vacuum sampler is deflected 30° in the vertical direction and extends about 10-20mm below the steel liquid level of the crystallizer, so that the round bubble of the vacuum sampler is immersed in the molten steel of the crystallizer. During sampling, the round bubble end of the vacuum sampler contacts the molten steel, and the high-temperature molten steel melts the round bubble end. The negative pressure in the vacuum sampler sucks the molten steel into the vacuum sampler, and then the vacuum sampler is quickly taken out; S4. Place the vacuum sampler in a cold water tank and wait for it to cool down, then remove the vacuum sampler to obtain a steel sample that can be used to detect nitrogen content; S5. The sample is quickly analyzed by an oxygen and nitrogen analyzer to obtain the nitrogen content value in the steel sample. The steel bar sample does not contact the air in the vacuum sampler. The nitrogen content value in the steel bar sample is the nitrogen content of the steel billet.
[0006] As a further solution of the present invention, the submerged water nozzle is inserted into the crystallizer to a depth of not less than 100-130 mm.
[0007] As a further solution of the present invention, the thickness of the protective slag is maintained at about 20 mm.
[0008] As a further solution of the present invention, the vacuum sampler is made of quartz glass, the interior of the vacuum sampler is completely sealed and in a vacuum state, and the wall thickness of the vacuum sampler is about 1.5 mm.
[0009] As a further solution of the present invention, the clamping tool is a clamping pliers.
[0010] Compared with the prior art, the present invention selects a preferred vacuum sampler to take out a steel sample from the molten steel in the crystallizer. During the sampling operation, the molten steel does not come into contact with the air throughout the entire process. The nitrogen content of the steel sample is the same as the nitrogen content in the steel billet, thereby ensuring that the sample preparation for the nitrogen content inspection in the steel is completed quickly. This solves the problem that when determining the nitrogen content in the steel billet in the prior art, usually a steel block is cut from the steel billet and the sample needs to be processed by a machining lathe, resulting in a delayed measurement result and failure to timely guide the steelmaking production process to control the nitrogen content of the steel billet. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 The present invention is a schematic structural diagram of a sampling method for quickly and accurately determining the nitrogen content in a steel billet.
[0012] In the attached figure: 1. crystallizer; 2. molten steel; 3. protective slag; 4. submerged nozzle; 5. tundish; 6. vacuum sampler; 601. round bubble. DETAILED DESCRIPTION
[0013] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.
[0014] like Figure 1 As shown, in an embodiment of the present invention, a sampling method for quickly and accurately determining the nitrogen content in a steel billet is implemented by the following steps: S1. The molten steel 2 in the tundish 5 is poured into the crystallizer 1 by using an immersion nozzle 4, and the nozzle is kept at the center of the steel liquid level in the crystallizer 1; S2. The surface of the molten steel 2 in the crystallizer 1 is covered by the protective slag 3; S3. The vacuum sampler 6 is used for sampling. The vacuum sampler 6 has a round bubble 601 at one end. During the sampling operation, the vacuum sampler 6 is clamped and fixed by a clamping tool, so that the vacuum sampler 6 is deflected 30° in the vertical direction and extends into the crystallizer 1 about 10-20 mm below the steel liquid surface, so that the round bubble 601 of the vacuum sampler 6 is immersed in the molten steel 2 of the crystallizer 1. During sampling, the round bubble 601 end of the vacuum sampler 6 contacts the molten steel 2, and the high-temperature molten steel 2 melts the round bubble 601 end. The negative pressure in the vacuum sampler 6 sucks the molten steel 2 into the vacuum sampler 6, and then the vacuum sampler 6 is quickly taken out; S4. The vacuum sampler 6 is placed in a cold water tank and cooled, and then the vacuum sampler 6 is removed to obtain a steel sample that can be used to detect the nitrogen content; S5. The sample is quickly analyzed by an oxygen-nitrogen analyzer to obtain the nitrogen content value in the steel sample. The steel bar sample does not contact the air in the vacuum sampler 6. The nitrogen content value in the steel bar sample is the nitrogen content of the steel billet.
[0015] Specifically, in the present invention, the surface of the molten steel in the crystallizer 1 is covered with protective slag 3, which can isolate the molten steel 2 from contact with the air, prevent the molten steel 2 from absorbing nitrogen in the air, and ensure that the nitrogen content in the molten steel 2 is stable. At the same time, during the sampling operation, the molten steel 2 is not in contact with the air throughout the whole process. The nitrogen content of the steel sample is the same as the nitrogen content in the steel billet, providing a basis for accurately controlling the nitrogen content in the steel.
[0016] Furthermore, in the embodiment of the present invention, the immersion nozzle 4 is inserted into the crystallizer 1 to a liquid level of not less than 100-130 mm to locate the depth of the molten steel 2 for sampling.
[0017] Furthermore, in the embodiment of the present invention, the thickness of the protective slag 3 is maintained at about 20 mm, so as to prevent the molten steel 2 from being isolated from the air and to prevent the nitrogen element in the air from being contacted by the molten steel 2 .
[0018] Further, in the embodiment of the present invention, the vacuum sampler 6 is made of quartz glass, the vacuum sampler 6 is completely closed and in a vacuum state, the wall thickness of the vacuum sampler 6 is about 1.5 mm, wherein the vacuum sampler 6 stays in the molten steel of the crystallizer 1 for about 3 seconds, and during sampling, the round bubble 601 end of the vacuum sampler 6 contacts the molten steel 2, the high-temperature molten steel 2 melts the quartz glass round bubble 601, and the negative pressure in the vacuum sampler 6 sucks the molten steel 2 into the vacuum sampler 6 to realize automatic sampling, and after the sampling is completed, the vacuum sampler 6 is placed in a cold water tank to rapidly cool down the vacuum sampler 6; Furthermore, in an embodiment of the present invention, the clamping tool is a clamping pliers, which clamps the vacuum sampler 6 to keep the vacuum sampler 6 stable when extending into the steel liquid level of the crystallizer 1, and prevent the vacuum sampler 6 from falling during sampling.
[0019] In summary, the present invention selects a preferred vacuum sampler 6 to take out a steel sample from the molten steel 2 in the crystallizer 1. During the sampling operation, the molten steel 2 does not come into contact with the air throughout the entire process. The nitrogen content of the steel sample is the same as the nitrogen content in the steel billet, thereby ensuring that the sample preparation for the nitrogen content inspection in the steel is quickly completed. This solves the problem that when determining the nitrogen content in the steel billet, the existing method usually involves cutting a steel block on the steel billet and sampling it using a machining lathe, resulting in delayed measurement results and failure to timely guide the steelmaking production process to control the nitrogen content in the steel billet.
[0020] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for sampling and preparing a sample for rapid and accurate determination of nitrogen content in steel billets. It is characterized in that To do this, follow these steps: S1. Use an immersed nozzle to pour the molten steel in the tundish into the crystallizer, and keep the nozzle at the center of the steel liquid level in the crystallizer; S2. The molten steel surface of the crystallizer is covered by protective slag; S3. Use a vacuum sampler to take samples. The vacuum sampler has a round bubble at one end. During the sampling operation, use a clamping tool to clamp and fix the vacuum sampler, so that the vacuum sampler is deflected 30° in the vertical direction and extends about 10-20mm below the steel liquid level of the crystallizer, so that the round bubble of the vacuum sampler is immersed in the molten steel of the crystallizer. During sampling, the round bubble end of the vacuum sampler contacts the molten steel, and the high-temperature molten steel melts the round bubble end. The negative pressure in the vacuum sampler sucks the molten steel into the vacuum sampler, and then the vacuum sampler is quickly taken out; S4. Place the vacuum sampler in a cold water tank and wait for it to cool down, then remove the vacuum sampler to obtain a steel sample that can be used to detect nitrogen content; S5. The sample is quickly analyzed by an oxygen and nitrogen analyzer to obtain the nitrogen content value in the steel sample. The steel bar sample does not contact the air in the vacuum sampler. The nitrogen content value in the steel bar sample is the nitrogen content of the steel billet.
2. A method for quickly and accurately determining the nitrogen content in a steel billet according to claim 1, It is characterized in that The immersion nozzle is inserted into the crystallizer to a depth of not less than 100-130 mm.
3. A method for quickly and accurately determining the nitrogen content in a steel billet according to claim 1, It is characterized in that The thickness of the protective slag is maintained at about 20 mm.
4. A method for sampling and preparing a steel billet for rapid and accurate determination of nitrogen content according to claim 1, It is characterized in that The vacuum sampler is made of quartz glass. The inside of the vacuum sampler is completely sealed and in a vacuum state. The wall thickness of the vacuum sampler is about 1.5 mm.
5. A method for sampling and preparing a steel billet for rapid and accurate determination of nitrogen content according to claim 1, It is characterized in that The clamping tool is a clamping pliers.