Color-fixing ink-carrying type ironing film and preparation method thereof
By designing inorganic cations and organic cations on the PET film to achieve color-fixing ink-carrying layer for pigment color fixation, the problem of peeling of ink absorbing layer and release layer during pattern color fixation in the prior art is solved, and the simple pattern is achieved Printing and thermal transfer improve color purity and fold resistance, while simplifying production processes and reducing costs.
Patent Information
- Application Number
- CN202411270807.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-11
AI Technical Summary
In the existing thermal transfer film technology, the ink absorbing layer and the release layer are peeled off together during the pattern fixing process, which affects the original color, pattern accuracy and fold resistance of the ink, and the production process is complex and the cost is high.
Using a color-fixed ink-loading type hot film, the inorganic cations and organic cations on the surface jointly realize direct color fixation of pigments or dye molecules. A PET thermal transfer hot film method with few coating structures and simple production is designed to realize the pattern. simple printing and thermal transfer.
It solves the problem of insufficient pure color of the pattern, achieves the effect of small coatings, simple process, low cost, and purer pattern, and improves the original color and fold resistance of the ink.
Smart Images

Figure CN119078389A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal sublimation transfer, and in particular to a color-fixing ink-carrying hot stamping film and a preparation method thereof. Background Art
[0002] Digitally printed heat transfer heat transfer film is suitable for making personalized and customized products, as well as printing full-color images or photos. The principle is to print the pattern on the PET heat transfer film, sprinkle hot melt powder on the pattern, and transfer the pattern to fabrics and other products through heat pressing. It has the advantages of bright colors, rich layers, low production costs, simple and convenient process, etc. It can be used for textile fabrics, leather, organic glass, metal, plastic, crystal, wood products and other materials; as people's love for DIY is gradually accepted by ordinary families, the product has broad market prospects.
[0003] In the existing thermal transfer hot stamping film technology, patent application number CN202010315595.5 discloses a method for producing a hot stamping film and its production process, wherein the hot stamping film comprises an anti-sticking layer, a base layer, a release layer, a polyurethane layer, an ink layer and an adhesive layer connected in sequence, and the prepared hot stamping film has a novel six-layer structure, which is very complex and cumbersome to produce; patent ZL200380107048.2 (authorization announcement number CN100431848C) discloses an inkjet receiving layer, comprising: a base comprising an ink receiving layer, the ink receiving layer comprising a raw polymer, the raw polymer being selected from: 1) a urethane acrylic copolymer, 2) a blend of at least one polyurethane polymer having a Mw greater than 400,000 g / mol and at least one acrylic polymer, 3) a blend of at least two polyurethane polymers, and a mixture thereof, wherein the ink receiving layer does not contain a filler; and a non-aqueous inkjet image located on the ink receiving layer. This type of patented structure has 4 to 6 layers, and the pattern is displayed by fixing the color through the ink-absorbing layer.
[0004] Patent application number 202010470186.2 discloses an environmentally friendly heat transfer ink, a PET film heat transfer method and its application. The PET film is preferably coated with a coating composition, which includes the following weight ratio components based on 100 parts by total weight: 10 to 30 parts of polyvinyl butyral, 5 to 10 parts of aqueous polyurethane, 5 to 10 parts of polyvinyl alcohol and 0.5 to 1 part of coupling agent, and the balance is water. The patent particularly emphasizes that the ink absorption effect of polyvinyl butyral is achieved, indicating that this patented coating composition is achieved through the structural characteristics of the ink absorption layer.
[0005] The current heat transfer film technology is to pass the ink through the inkjet printer PET heat transfer film ink absorption layer, through the PET heat transfer film for heat transfer, the ink absorption layer is completely printed on the fabric. During the heat transfer, the ink absorption layer containing pigment or dye molecules and the release layer are peeled off together, and the original color of the ink, the accuracy of the pattern, the folding resistance, the changeability and other properties are affected.
[0006] In order to solve the above problems, the applicant has studied and improved the existing technology. The first purpose is to propose a new method for the structure of the color-fixing ink-carrying layer, in which the inorganic cations and organic cations on the surface jointly realize the color-fixing ink-carrying of pigment or dye molecules instead of absorbing ink; the second purpose is to provide a method for digital printing PET thermal transfer heat transfer film with fewer structural layers and simpler production; the third purpose is to solve the problem that the thermal transfer of the pattern does not contain the color-fixing ink-carrying layer component, ensuring the original color of the ink and other properties. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention provides a color-fixing ink-carrying hot transfer film and a method for manufacturing the same. Compared with the existing PET-based hot transfer film technology, the present invention designs a new method in which inorganic cations and organic cations on the surface of the color-fixing ink-carrying film jointly realize direct color fixation of pigment or dye molecules to form a patterned color-fixing ink-carrying layer, thereby overcoming the problem that the existing PET hot transfer film forms a pattern by fixing the color through an ink-absorbing layer, and can realize thermal transfer of a simple printed pattern without containing a surface color-fixing ink-carrying layer, thereby solving the problem that the color of the printed pattern in the prior art is not pure enough when the ink-absorbing layer is transferred together. The method of the present invention has the characteristics of less number of coating layers, good comprehensive coating performance, simple production process, lower cost, and purer transferred patterns.
[0008] In order to solve the above technical problems, the present invention is solved by the following technical solutions:
[0009] A color-fixing ink-carrying hot stamping film comprises a substrate film and a surface color-fixing ink-carrying layer, wherein the substrate film is a PET substrate, the surface color-fixing ink-carrying layer is on the substrate film, and the surface of the surface color-fixing ink-carrying layer directly fixes the pigment or dye molecules in the coating ink to form a printing pattern.
[0010] Preferably, the surface of the PET film of the hot-burning film is formed into a concave-convex structure by heat pressing, and the concave-convex structure includes a plurality of concave portions distributed at equal intervals, and the concave portions are all square structures.
[0011] Preferably, the surface color fixing ink-carrying layer comprises a grid-shaped polymer cross-linking layer, one end of which is connected to the substrate film and the other end is covered with an inorganic ion layer to fix the pigment or dye molecules directly to form a pattern.
[0012] Specifically, the surface color fixing ink-carrying layer includes cationic polyacrylamide, waterborne polyurethane, carboxymethyl cellulose, silicone resin and inorganic salt. The grid-shaped polymer cross-linking layer is composed of waterborne polyurethane, cationic polyacrylamide, carboxymethyl cellulose and silicone resin, and the inorganic ion layer is composed of inorganic salt.
[0013] Preferably, the surface color fixing ink-carrying layer comprises, by weight, 15-8 parts of waterborne polyurethane, 5-7 parts of cationic polyacrylamide, 3-8 parts of carboxymethyl cellulose, 47-30 parts of organic dimethyl silicone resin and 30-47 parts of inorganic salt.
[0014] Preferably, the waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, which contains a self-crosslinking group; or the end group of the waterborne aliphatic polyether polyurethane is one of a hydroxyl group, a carboxyl group, a carboxymethyl group or an aldehyde group, and the silicone resin is an organic dimethyl silicone resin.
[0015] Preferably, the inorganic salt comprises a solid salt and an inorganic salt liquid solution, the solid salt is one or a combination of BaSO4, CaSO4, BaCO3, and CaCO3; the inorganic salt liquid solution is one or a combination of BaCl2, ZnCl2, CaCl2, MgCl2, and ALCl3, with a liquid concentration of 10%-20%; the ratio of the two is 100:22 to 100:13.
[0016] Preferably, the method for preparing the surface color-fixing ink-carrying layer comprises the following steps:
[0017] (1) According to the ratio, add a certain amount of water to the high-speed dispersion tank, then add water-based polyurethane to form a dispersion liquid with a dispersing effect, and disperse it at a speed of 200-500r / min for 5-10min;
[0018] (2) then adding cationic polyacrylamide and dispersing at a rotation speed of 1500-2000 r / min for 30-40 min to obtain a dispersion of the composition;
[0019] (3) adding solid inorganic salt and inorganic salt liquid solution in sequence under stirring at a speed of 200-500 r / min. After each raw material is added, stirring is performed at the same speed for 5-10 minutes before adding another raw material;
[0020] (4) Continue to add the silicone resin while stirring at a speed of 200-500 r / min. After the addition is completed, continue to add carboxymethyl cellulose at the same speed and stir for 5-10 minutes. Measure the solid content and viscosity and set aside.
[0021] A method for preparing a color-fixing ink-carrying hot stamping film comprises the following steps: coating a surface color-fixing ink-carrying material on one side of a substrate film, and drying to form a surface color-fixing ink-carrying layer.
[0022] The present invention has significant technical effects due to the adoption of the above technical solution:
[0023] The present invention realizes a new method for coating a PET film substrate to form a surface color-fixing ink-carrying layer, and surface inorganic cations and organic cations jointly realize direct color fixation of pigment or dye molecules to form a pattern color-fixing ink-carrying layer. Compared with the existing PET-based heat transfer film technology, the new method of the present invention designs a surface direct color fixation to form a pattern color-fixing ink-carrying layer, overcomes the problem that the existing PET heat transfer film forms a pattern by fixing the color through the ink absorbing layer, realizes the thermal transfer of a simple printed pattern without a surface color-fixing ink-carrying layer, and solves the problem that the printed pattern in the prior art contains an ink absorbing layer and the color is not pure enough.
[0024] The existing PET heat transfer film preparation requires an anti-adhesive layer, a base layer, a release layer, a polyurethane layer, an ink-absorbing layer, etc., and the steps of gravure feeding and coating are repeated many times to form a 4-6-layer structure, and the production process is relatively complicated. The method of the present invention realizes one-time coating and molding, has the characteristics of fewer coating layers, good comprehensive coating performance, simple production process, lower cost, better water resistance and printability, and purer transferred patterns. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the structure of the color-fixing ink-carrying hot stamping film in this embodiment.
[0026] Figure 2 1 is a schematic diagram of the structure of the surface of the color-fixing ink-carrying hot stamping film after heat pressing in this embodiment.
[0027] The parts indicated by the numerical symbols in the accompanying drawings are as follows: 1-substrate film, 2-surface color fixing ink-carrying layer, 3-ink layer. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0029] Example 1
[0030] A color-fixing ink-carrying hot stamping film, comprising a substrate film and a surface color-fixing ink-carrying layer, wherein the substrate film is a PET film 1, the substrate film 1 is bonded to the surface color-fixing ink-carrying layer 2, and the surface of the surface color-fixing ink-carrying layer 2 directly fixes the pigment or dye molecules in the coating ink to form a printing pattern;
[0031] The surface color fixing ink-carrying layer 2 comprises a grid-shaped polymer cross-linking layer, one end of which is connected to the substrate film and the other end is covered with an inorganic ion layer to fix the pigment or dye molecules to directly fix the color to form a pattern, namely the ink layer 3.
[0032] Specifically, the grid-shaped polymer cross-linked layer in the surface color-fixing ink-carrying layer 2 is composed of water-based polyurethane, cationic polyacrylamide, carboxymethyl cellulose and silicone resin, and the inorganic ion layer is composed of inorganic salt.
[0033] The PET film on the surface of the hot-melt film is formed into a concave-convex structure by heat pressing, and the concave-convex structure includes a plurality of concave parts distributed at equal intervals, and the concave parts are all square structures.
[0034] Example 2
[0035] This embodiment provides a color-fixing ink-carrying hot stamping film, which differs from the above embodiment only in that: the surface color-fixing ink-carrying layer 2 comprises, by weight, 2 parts of cationic polyacrylamide, 8 parts of waterborne polyurethane, 3 parts of carboxymethyl cellulose, 47 parts of organic dimethyl silicone resin and 40 parts of inorganic salt;
[0036] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the modified waterborne aliphatic polyether polyurethane contains a self-crosslinking group;
[0037] The inorganic salt includes solid salt and inorganic salt liquid solution, the solid salt is BaSO4, the inorganic salt liquid solution is BaCl2, the liquid concentration is 10%-20%, and the ratio of the two is 100:32.
[0038] Example 3
[0039] This embodiment provides a color-fixing ink-carrying hot stamping film, which differs from the above embodiment only in that: the surface color-fixing ink-carrying layer comprises, by weight, 3 parts of cationic polyacrylamide, 8 parts of waterborne polyurethane, 3 parts of carboxymethyl cellulose, 40 parts of organic dimethyl silicone resin and 40 parts of inorganic salt;
[0040] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the terminal group of the waterborne aliphatic polyether polyurethane is a hydroxyl group;
[0041] The inorganic salt includes solid salt and inorganic salt liquid solution, the solid salt is BaSO4, the inorganic salt liquid solution is BaCl2, the liquid concentration is 10%-20%, and the ratio of the two is 100:30.
[0042] Example 4
[0043] This embodiment provides a color-fixing ink-carrying hot stamping film, which differs from the above embodiment only in that: the surface color-fixing ink-carrying layer comprises 5 parts of cationic polyacrylamide, 10 parts of waterborne polyurethane, 4 parts of carboxymethyl cellulose, 40 parts of organic dimethyl silicone resin and 45 parts of inorganic salt in terms of weight parts;
[0044] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the terminal group of the waterborne aliphatic polyether polyurethane is a hydroxyl group;
[0045] The inorganic salt includes solid salt and inorganic salt liquid solution. The solid salt is a combination of BaSO4 and BaCO3, and the inorganic salt liquid solution is BaCl2 with a liquid concentration of 10%-20%. The ratio of the two is 100:25.
[0046] Example 5
[0047] This embodiment provides a color-fixing ink-carrying hot stamping film, which is different from the above embodiment only in that: the surface color-fixing ink-carrying layer includes 5 parts of cationic polyacrylamide, 12 parts of waterborne polyurethane, 4 parts of carboxymethyl cellulose, 30 parts of organic dimethyl silicone resin and 45 parts of inorganic salt in terms of weight parts;
[0048] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the terminal group of the waterborne aliphatic polyether polyurethane is a carboxymethyl group;
[0049] The inorganic salt includes solid salt and inorganic salt liquid solution. The solid salt is a combination of BaSO4 and BaCO3, and the inorganic salt liquid solution is BaCl2 with a liquid concentration of 10%-20%. The ratio of the two is 100:13.
[0050] Example 6
[0051] This embodiment provides a color-fixing ink-carrying hot stamping film, which differs from the above embodiment only in that: the surface color-fixing ink-carrying layer comprises, by weight, 6 parts of cationic polyacrylamide, 12 parts of waterborne polyurethane, 6 parts of carboxymethyl cellulose, 20 parts of organic dimethyl silicone resin and 48 parts of inorganic salt;
[0052] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the terminal group of the waterborne aliphatic polyether polyurethane is a carboxyl group;
[0053] The inorganic salt includes solid salt and inorganic salt liquid solution. The solid salt is a composition of CaSO4 and CaCO3, and the inorganic salt liquid solution is CaCl2 with a liquid concentration of 10%-20%. The ratio of the two is 100:30.
[0054] Example 7
[0055] This embodiment provides a color-fixing ink-carrying hot stamping film, which is different from the above embodiment only in that: the surface color-fixing ink-carrying layer includes 7 parts of cationic polyacrylamide, 15 parts of waterborne polyurethane, 6 parts of carboxymethyl cellulose, 20 parts of organic dimethyl silicone resin and 52 parts of inorganic salt in terms of weight parts;
[0056] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the terminal group of the waterborne aliphatic polyether polyurethane is an aldehyde group;
[0057] The inorganic salt includes solid salt and inorganic salt liquid solution. The solid salt is a composition of CaSO4 and CaCO3, and the inorganic salt liquid solution is CaCl2 with a liquid concentration of 10%-20%. The ratio of the two is 100:20.
[0058] Example 8
[0059] This embodiment provides a color-fixing ink-carrying hot stamping film, which is different from the above embodiment only in that: the surface color-fixing ink-carrying layer includes 7 parts of cationic polyacrylamide, 12 parts of waterborne polyurethane, 6 parts of carboxymethyl cellulose, 30 parts of organic dimethyl silicone resin and 50 parts of inorganic salt in terms of weight parts;
[0060] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the terminal group of the waterborne aliphatic polyether polyurethane is a carboxyl group;
[0061] The inorganic salt includes solid salt and inorganic salt liquid solution, the solid salt is CaSO4; the inorganic salt liquid solution is CaCl2, the liquid concentration is 10%-20%; the ratio of the two is 100:25.
[0062] Example 9
[0063] This embodiment provides a color-fixing ink-carrying hot stamping film, which differs from the above embodiment only in that: the surface color-fixing ink-carrying layer comprises 6 parts of cationic polyacrylamide, 13 parts of waterborne polyurethane, 5 parts of carboxymethyl cellulose, 40 parts of organic dimethyl silicone resin and 50 parts of inorganic salt in terms of weight parts;
[0064] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the terminal group of the waterborne aliphatic polyether polyurethane is a hydroxyl group;
[0065] The inorganic salt includes solid salt and inorganic salt liquid solution, the solid salt is CaCO3, the inorganic salt liquid solution is ZnCl2, the liquid concentration is 10%-20%, and the ratio of the two is 100:30.
[0066] Example 10
[0067] This embodiment provides a color-fixing ink-carrying hot stamping film, which is different from the above embodiment only in that: the surface color-fixing ink-carrying layer includes 7 parts of cationic polyacrylamide, 15 parts of waterborne polyurethane, 6 parts of carboxymethyl cellulose, 20 parts of organic dimethyl silicone resin and 52 parts of inorganic salt in terms of weight parts;
[0068] The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the terminal group of the waterborne aliphatic polyether polyurethane is a hydroxyl group;
[0069] The inorganic salt includes solid salt and inorganic salt liquid solution. The solid salt is a combination of BaSO4 and BaCO3, and the inorganic salt liquid solution is BaCl2 with a liquid concentration of 10%-20%. The ratio of the two is 100:32.
[0070] Embodiment 11
[0071] This embodiment provides a method for preparing a color-fixing ink-carrying hot stamping film, which comprises the following steps:
[0072] (1) Preparation of surface color fixing ink-carrying layer:
[0073] 1) According to the ratio, add a certain amount of water to the high-speed dispersion tank, and then add a corresponding amount of waterborne polyurethane to form a dispersion liquid with a dispersing effect, and disperse it at a speed of 200-500r / min for 5-10min;
[0074] 2) then adding cationic polyacrylamide and dispersing at a rotation speed of 1500-2000 r / min for 30-40 min to obtain a dispersion of the composition;
[0075] 3) Add solid inorganic salt and inorganic salt liquid solution in sequence under stirring at a speed of 200-500 r / min. After adding each raw material, stir at the same speed for 5-10 minutes before adding another raw material;
[0076] 4) Continue to add the silicone resin while stirring at a speed of 200-500 r / min. After the addition is completed, continue to add carboxymethyl cellulose at the same speed, stir for 5-10 minutes, measure the solid content and viscosity, and set aside;
[0077] (2) Preparation of hot stamping film: coating a surface color fixing ink carrying material on one side of the substrate film, and drying to form a surface color fixing ink carrying layer.
[0078] The hot stamping film of the present invention directly fixes color to form a pattern-fixing ink-carrying layer 3, which overcomes the problem that the existing PET hot stamping film forms a pattern by fixing color through the ink-absorbing layer 3, realizes thermal transfer of a simple printed pattern, and does not contain a surface color-fixing ink-carrying layer 2, thereby solving the problem that the printed pattern in the prior art contains the ink-absorbing layer 3 and the color is not pure enough when transferred together.
[0079] The technical solution of the present invention is further illustrated below through specific embodiments to provide a better understanding of the present invention.
[0080] Test example: a surface color-fixing ink-carrying material is prepared according to the weight ratios shown in Example 1, Example 2 and Example 6, and the surface color-fixing ink-carrying material is coated on one side of a PET substrate, and dried at 150-180° C. to form a hot film of a color-fixing ink-carrying layer;
[0081] Comparative Example: Without using inorganic salt, the surface color fixing ink carrying material was prepared according to the weight ratios shown in Example 1, Example 2 and Example 6, and the surface color fixing ink carrying material was coated on one side of the PET substrate, and dried at 150-180° C. to form a PET hot film;
[0082] The PET film thermal transfer method of each test example and the comparative example is the same. The specific method of the PET film thermal transfer is as follows: ink is printed on the PET film by inkjet printing, and hot-melt powder is sprinkled on the printed pattern. After the hot-melt powder is heated and melted into a viscous state, the transfer layer of the PET film is facing the printing fabric, and the PET film is pressed on a pressing machine at 170°C for 10 seconds to obtain a printed pattern on the fabric surface.
[0083] Specific performance test:
[0084] Test Item 1: Printing Fluency
[0085] The heat transfer films prepared in the above-mentioned Examples 1, 2, 6 and the comparative example were printed on a double-head offset heat transfer white ink machine-Q3-E602 inkjet printer, with a single color block printed according to the 100% inkjet setting. The printing process was observed and recorded, and the test results are shown in Table 1 below; then they were transferred to a white pure cotton fabric and hot pressed at 160° C. to 170° C. to obtain a finished fabric.
[0086] Test Item 2: Evaluation of Support Fixation Effect
[0087] Take the hot stamping films prepared in the above-mentioned Examples 1, 2, 6 and the comparative example, and print them on a double-head offset hot stamping white ink machine-Q3-E602 inkjet printer, and print a single color block according to the 100% inkjet setting. After printing, sprinkle hot melt powder on the pattern, heat and melt the hot melt powder to a viscous flow state, and then place the transfer layer of the PET film toward the substrate fabric. The PET film is pressed for 10 seconds under a 170°C pressing machine to obtain a printed pattern on the fabric surface. Check the surface of the PET film, the support layer is intact and not damaged, indicating that only the fixed color pigment is transferred, and the support layer is not transferred together.
[0088] The test results are shown in Table 1 below.
[0089] Table 1
[0090] Test items Printing Fluency Support layer retention effect Example 1 Continuous printing of 500ml, smooth printing without white lines good Example 2 Continuous printing of 500ml, smooth printing without white lines good Example 6 Continuous printing of 500ml, smooth printing without white lines good
[0091] In addition, in Comparative Example 1-2, the water-based pigment ink was transferred to the ink-absorbing layer on the PET transfer film, and the PET surface was damaged in the shape of the pattern, which was then transferred to the cloth.
[0092] In conclusion, the above is only a preferred embodiment of the present invention, and all equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the patent of the present invention.
Claims
1. A color-fixing ink-carrying hot stamping film, characterized in that: The invention comprises a substrate film (1) and a surface color-fixing ink-carrying layer (2), wherein the substrate film (1) is a PET film, the surface color-fixing ink-carrying layer (2) is coated on the substrate film (1), and the surface of the surface color-fixing ink-carrying layer (2) directly fixes the pigment or dye molecules in the coating ink to form a printing pattern.
2. The color-fixing ink-carrying hot stamping film according to claim 1, characterized in that: The surface of the PET film is hot pressed to form a concave-convex structure, and the concave-convex structure includes a plurality of concave parts distributed at equal intervals, and the concave parts are all square.
3. The color-fixing ink-carrying hot stamping film according to claim 1, characterized in that: The surface color-fixing ink-carrying layer (2) comprises cationic polyacrylamide, water-based polyurethane, carboxymethyl cellulose, organic silicon resin and inorganic salt.
4. The color-fixing ink-carrying hot stamping film according to claim 3, characterized in that: The surface color-fixing ink-carrying layer (2) comprises, by weight, 2-7 parts of cationic polyacrylamide, 8-15 parts of waterborne polyurethane, 3-6 parts of carboxymethyl cellulose, 47-20 parts of silicone resin and 40-52 parts of inorganic salt.
5. The color-fixing ink-carrying hot stamping film according to claim 4, characterized in that: The waterborne polyurethane is a modified waterborne aliphatic polyether polyurethane, and the waterborne aliphatic polyether polyurethane contains a self-crosslinking group; or the end group of the waterborne aliphatic polyether polyurethane is one of a hydroxyl group, a carboxyl group, a carboxymethyl group or an aldehyde group, and the organic silicone resin is an organic dimethyl silicone resin.
6. The color-fixing ink-carrying hot stamping film according to claim 4, characterized in that: The inorganic salt includes solid salt and inorganic salt liquid solution, the solid salt is one or a combination of BaSO4, CaSO4, BaCO3, CaCO3; the inorganic salt liquid solution is one or a combination of BaCl2, ZnCl2, CaCl2, MgCl2, ALCl3, and the liquid concentration is 10%-20%; the ratio of the two is 100:32 to 100:
13.
7. A color-fixing ink-carrying hot stamping film according to any one of claims 2 to 6, characterized in that: The preparation method of the surface color-fixing ink-carrying layer comprises the following steps: (1) adding a certain amount of water to a high-speed dispersion tank according to the ratio, then adding water-based polyurethane to form a dispersion liquid with a dispersing effect, and dispersing at a speed of 200-500 r / min for 5-10 min; then adding cationic polyacrylamide and dispersing at a speed of 1500-2000 r / min for 30-40 min to obtain a dispersion liquid of the composition; (2) adding a liquid salt solution while stirring at a speed of 200-500 r / min, stirring at the speed for 5-10 min, and then adding a solid inorganic salt to obtain a mixed dispersion; (3) Continue to add the silicone resin while stirring at a speed of 200-500 r / min. After the addition is completed, continue to add carboxymethyl cellulose at the same speed and stir for 5-10 minutes. Measure the solid content and viscosity and set aside.
8. A method for preparing a color-fixing ink-carrying hot stamping film, characterized in that: The following steps are involved: A surface color-fixing ink-carrying material is coated on one side of a substrate film (1), and after drying, a surface color-fixing ink-carrying layer (2) is formed.
Citation Information
Patent Citations
Ink jet receptive coating
CN100431848C
Environmentally friendly heat transfer inks, PET film heat transfer methods and their applications
CN111607286B
A heat transfer film and its manufacturing process
CN111619257B
Ink receptive material, tinted optical lenses and method for manufacturing the same
CN101119852A
Prime coating liquid suitable for aqueous pigment ink printed non-absorptive printing medium, and preparation method and applications thereof
CN110804381A
Cited By
DTF pyrograph film and preparation method thereof