High-compaction-density lithium iron phosphate resynthesized from waste lithium iron phosphate and preparation method of high-compaction-density lithium iron phosphate

By modifying waste lithium iron phosphate, using modified agents such as lithium dihydrogen phosphate, iron trioxide and titanium dioxide, high-pressure density lithium iron phosphate was prepared, which solved the extraction rate of lithium, iron, phosphorus and other substances and The problem of impurity content has achieved efficient reuse and performance optimization of waste lithium iron phosphate.

CN119079960APending Publication Date: 2024-12-06JIANGXI ZHILI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410894309.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The residual phosphate ferrous slag after lithium recovery in waste lithium iron phosphate positive electrode materials lacks effective treatment methods, resulting in waste of resources and environmental pollution, and the extraction rate and extracted impurities of lithium, iron, phosphorus and other substances are difficult to solve.

Method used

By modifying waste lithium iron phosphate, the formula includes waste lithium iron phosphate, lithium dihydrogen phosphate, iron trioxide, titanium dioxide and glucose, high temperature sintering and grinding, adjusting the element ratio and structure, and preparing high compaction density Lithium iron phosphate skips the extraction process of lithium, iron, phosphorus and other substances, and uses lithium dihydrogen phosphate, iron trioxide and titanium dioxide as modifiers to optimize the lattice structure and element ratio.

Benefits of technology

It has achieved efficient reuse of waste lithium iron phosphate, the powder compaction density reaches 2.5g/cm3 or above, meets industry standards, solves the extraction rate and impurity content of elements such as lithium, iron, phosphorus, etc., and optimizes lithium iron phosphate performance and structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079960A_ABST
    Figure CN119079960A_ABST
Patent Text Reader

Abstract

The invention discloses waste lithium iron phosphate resynthesized high-compaction-density lithium iron phosphate and a preparation method thereof.The waste lithium iron phosphate is modified, and the formula comprises, by mass, 95%-99% of waste lithium iron phosphate, 0-2% of lithium dihydrogen phosphate, 0-1% of ferric oxide, 0.1%-2% of titanium dioxide, 0.5%-5% of glucose and 25% of solid. According to the waste lithium iron phosphate resynthesized high-compaction-density lithium iron phosphate and the preparation method thereof disclosed by the invention, the lithium iron phosphate positive electrode material of which the powder compaction density is 2.5 g / cm < 3 > or above and each index meets the industrial standard can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to lithium iron phosphate with high compaction density synthesized from waste lithium iron phosphate and a preparation method thereof. Background Art

[0002] Lithium iron phosphate batteries have high specific capacity and working voltage, and have become the mainstream technology in the current electrochemical energy storage field. Compared with other battery positive electrode materials, lithium iron phosphate has the advantages of high safety, strong stability, low cost, abundant resources and long cycle life. Almost all energy storage batteries used in the domestic market are lithium iron phosphate batteries, among which lithium iron phosphate batteries account for as much as 88% in electric buses. The average service life of lithium iron phosphate batteries is 5 to 8 years. Considering the increasing number of lithium iron phosphate batteries in the entire market, the treatment of waste lithium iron phosphate batteries will become an urgent problem to be solved. Therefore, achieving efficient recycling of waste lithium iron phosphate batteries, turning them into treasure, and realizing resource utilization are of great significance to reducing environmental pollution and alleviating resource shortages.

[0003] At present, the recycling of waste lithium iron phosphate cathode materials is mainly through selective leaching to recover lithium, which has been realized in industrial operation. The main purpose of recycling lithium iron phosphate cathode materials is to extract lithium, iron, phosphorus and other substances from the materials and then synthesize lithium iron phosphate to obtain lithium iron phosphate materials with excellent performance. However, there is no effective treatment method for the phosphorus iron slag left after lithium recovery in waste lithium iron phosphate cathode materials, which needs to be solved urgently. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a method for resynthesizing waste lithium iron phosphate into lithium iron phosphate with high compaction density and a preparation method thereof, which can prepare powder with compaction density of 2.5g / cm 3 All the above indicators meet the industry standard for lithium iron phosphate positive electrode materials.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: In the first aspect, the present invention provides a waste lithium iron phosphate for resynthesizing lithium iron phosphate with high compaction density, which is modified by the waste lithium iron phosphate, and the formula consists of the following raw materials in percentage by mass: 95%-99% waste lithium iron phosphate, 0-2% lithium dihydrogen phosphate, 0-1% ferric oxide, 0.1%-2% titanium dioxide, 0.5-5% glucose, and 25% solid content.

[0006] Furthermore, the formula is 98% waste lithium iron phosphate, 0.2% lithium dihydrogen phosphate, 0.2% ferric oxide, 0.8% titanium dioxide, 1% glucose, and 25% solid content.

[0007] In a second aspect, the present invention provides a method for preparing lithium iron phosphate with high compaction density by resynthesizing waste lithium iron phosphate as described in any one of the above, wherein the waste lithium iron phosphate is modified, comprising the following steps: S1. Processing of recycled waste lithium iron phosphate, including but not limited to high temperature sintering, demagnetization, screening, testing, etc.; S2, prepare materials according to the formula ratio; S3, pouring water into a ball mill, adding waste lithium iron phosphate and stirring to obtain a slurry; S4, pouring lithium dihydrogen phosphate, glucose and ferric oxide into the slurry, and continuing to stir to obtain a slurry; S5, transferring the ball-milled slurry to a sand mill for grinding, and adding titanium dioxide to the sand mill for grinding; S6, spray drying the slurry obtained after grinding to obtain a yellow powder; S7, putting the sprayed material into a kiln for high-temperature sintering to obtain black powder; S8, performing air flow milling on the powder obtained after sintering, and adjusting the air flow milling parameters to achieve the target particle size; S9. Screen, demagnetize and package the crushed black powder to obtain the final product.

[0008] Furthermore, the stirring time in S3 is 30 minutes, and the stirring time in S4 is 1 hour.

[0009] Furthermore, the grinding particle size of the slurry in S5 is controlled at D50=0.7±0.05 μm.

[0010] Furthermore, the high temperature sintering of the material in S7 refers to heating the spray material in a nitrogen sealed atmosphere for 6 hours (room temperature-750°C), then sintering at a constant temperature of 750°C for 10 hours, and finally cooling the material out of the furnace.

[0011] In summary, the beneficial effects of the present invention are: The invention discloses a method for re-synthesizing waste lithium iron phosphate into lithium iron phosphate with high compaction density and a preparation method thereof. (1) The waste lithium iron phosphate is directly modified and researched, thereby skipping the extraction process of lithium, iron, phosphorus and other substances, and indirectly solving the problems of the extraction rate of lithium, iron, phosphorus and other substances and the high content of extracted impurities in the industry. (2) Lithium dihydrogen phosphate mainly contains two elements, Li and P, and ferric oxide mainly contains Fe. Both of them are used as modifiers. In waste lithium iron phosphate, the missing components can be identified through testing. By adding appropriate amounts of Li, P, Fe and other elements, the missing elements in the waste lithium iron phosphate are supplemented so that the original waste lithium iron phosphate element ratio meets the requirements. Then, the lithium iron phosphate grains are modified through a sintering process to finally obtain a high compaction density. Lithium iron phosphate, when adding Li, P, Fe and other elements, strictly follow the proportion. Adding too much or too little will lead to differences in the performance of lithium iron phosphate; (3) Titanium dioxide mainly contains Ti elements. As an additive, it is doped into waste lithium iron phosphate to optimize the lattice structure of lithium iron phosphate and widen the lithium ion migration channel, thereby achieving the purpose of modifying waste lithium iron phosphate; (4) The waste lithium iron phosphate recycling process has been innovated. The core technology lies in the use of composite modified additives and the addition ratio of various raw materials, especially the quantitative addition of Li, P, Fe, and Ti elements, so that the waste lithium iron phosphate with unbalanced elements can regain the performance of high-compacted lithium iron phosphate. The waste lithium iron phosphate was successfully used to prepare a powder with a compaction density greater than 2.5g / cm 3 , other indicators of the product meet industry standards. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 The present invention is a process flow chart of the method for preparing lithium iron phosphate with high compaction density by resynthesizing waste lithium iron phosphate. DETAILED DESCRIPTION

[0013] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0014] In the first aspect, the present invention provides a waste lithium iron phosphate for resynthesizing lithium iron phosphate with high compaction density, which is modified by the waste lithium iron phosphate, and the formula consists of the following raw materials in percentage by mass: 95%-99% waste lithium iron phosphate, 0-2% lithium dihydrogen phosphate, 0-1% ferric oxide, 0.1%-2% titanium dioxide, 0.5-5% glucose, and 25% solid content.

[0015] Furthermore, the formula can be 98% of waste lithium iron phosphate, 0.2% of lithium dihydrogen phosphate, 0.2% of ferric oxide, 0.8% of titanium dioxide, 1% of glucose, and 25% of solid content.

[0016] In a second aspect, the present invention provides a method for preparing the above waste lithium iron phosphate by resynthesizing lithium iron phosphate with high compaction density, wherein the waste lithium iron phosphate is modified, comprising the following steps: S1. Processing of recycled waste lithium iron phosphate, including but not limited to high temperature sintering, demagnetization, screening, testing, etc.; S2, prepare materials according to the formula ratio; S3, pouring water into a ball mill, adding waste lithium iron phosphate and stirring to obtain a slurry; S4, pouring lithium dihydrogen phosphate, glucose and ferric oxide into the slurry, and continuing to stir to obtain a slurry; S5, transferring the ball-milled slurry to a sand mill for grinding, and adding titanium dioxide to the sand mill for grinding; S6, spray drying the slurry obtained after grinding to obtain a yellow powder; S7, putting the sprayed material into a kiln for high-temperature sintering to obtain black powder; S8, performing air flow milling on the powder obtained after sintering, and adjusting the air flow milling parameters to achieve the target particle size; S9. Screen, demagnetize and package the crushed black powder to obtain the final product.

[0017] Furthermore, the stirring time in S3 is 30 minutes, and the stirring time in S4 is 1 hour.

[0018] Furthermore, the grinding particle size of the slurry in S5 is controlled at D50=0.7±0.05 μm.

[0019] Furthermore, the high temperature sintering of the material in S7 refers to heating the spray material in a nitrogen sealed atmosphere for 6 hours (room temperature-750°C), then sintering at a constant temperature of 750°C for 10 hours, and finally cooling the material out of the furnace.

[0020] In summary, the beneficial effects of the present invention are: The invention discloses a method for re-synthesizing waste lithium iron phosphate into lithium iron phosphate with high compaction density and a preparation method thereof. (1) The waste lithium iron phosphate is directly modified and researched, thereby skipping the extraction process of lithium, iron, phosphorus and other substances, and indirectly solving the problems of the extraction rate of lithium, iron, phosphorus and other substances and the high content of extracted impurities in the industry. (2) Lithium dihydrogen phosphate mainly contains two elements, Li and P, and ferric oxide mainly contains Fe. Both of them are used as modifiers. In waste lithium iron phosphate, the missing components can be identified through testing. By adding appropriate amounts of Li, P, Fe and other elements, the missing elements in the waste lithium iron phosphate are supplemented so that the original waste lithium iron phosphate element ratio meets the requirements. Then, the lithium iron phosphate grains are modified through a sintering process to finally obtain a high compaction density. Lithium iron phosphate, when adding Li, P, Fe and other elements, strictly follow the proportion. Adding too much or too little will lead to differences in the performance of lithium iron phosphate; (3) Titanium dioxide mainly contains Ti elements. As an additive, it is doped into waste lithium iron phosphate to optimize the lattice structure of lithium iron phosphate and widen the lithium ion migration channel, thereby achieving the purpose of modifying waste lithium iron phosphate; (4) The waste lithium iron phosphate recycling process has been innovated. The core technology lies in the use of composite modified additives and the addition ratio of various raw materials, especially the quantitative addition of Li, P, Fe, and Ti elements, so that the waste lithium iron phosphate with unbalanced elements can regain the performance of high-compacted lithium iron phosphate. The waste lithium iron phosphate was successfully used to prepare a powder with a compaction density greater than 2.5g / cm 3 , other indicators of the product meet industry standards.

[0021] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for resynthesizing waste lithium iron phosphate into lithium iron phosphate with high compaction density, characterized in that: It is modified by waste lithium iron phosphate, and the formula is composed of the following raw materials in percentage by mass: waste lithium iron phosphate 95%-99%, lithium dihydrogen phosphate 0-2%, ferric oxide 0-1%, titanium dioxide 0.1%-2%, glucose 0.5-5%, and solid content 25%.

2. The waste lithium iron phosphate according to claim 1 is used to synthesize lithium iron phosphate with high compaction density, characterized in that: The formula is 98% waste lithium iron phosphate, 0.2% lithium dihydrogen phosphate, 0.2% ferric oxide, 0.8% titanium dioxide, 1% glucose, and 25% solid content.

3. A method for preparing lithium iron phosphate with high compaction density by resynthesizing waste lithium iron phosphate as described in any one of claims 1 to 2, characterized in that: The modification is carried out by using waste lithium iron phosphate, including the following steps: S1. Process the recycled waste lithium iron phosphate, including high-temperature sintering, demagnetization, screening, testing, etc.; S2, prepare materials according to the formula ratio; S3, pouring water into a ball mill, adding waste lithium iron phosphate and stirring to obtain a slurry; S4, pouring lithium dihydrogen phosphate, glucose and ferric oxide into the slurry, and continuing to stir to obtain a slurry; S5, transferring the ball-milled slurry to a sand mill for grinding, and adding titanium dioxide to the sand mill for grinding; S6, spray drying the slurry obtained after grinding to obtain a yellow powder; S7, putting the sprayed material into a kiln for high-temperature sintering to obtain black powder; S8, performing air flow milling on the powder obtained after sintering, and adjusting the air flow milling parameters to achieve the target particle size; S9. Screen, demagnetize and package the crushed black powder to obtain the final product.

4. The method for preparing lithium iron phosphate with high compaction density by resynthesizing waste lithium iron phosphate as claimed in claim 3, characterized in that: The stirring time in S3 is 30 minutes, and the stirring time in S4 is 1 hour.

5. The method for preparing lithium iron phosphate with high compaction density by resynthesizing waste lithium iron phosphate as claimed in claim 4, characterized in that: The grinding particle size of the slurry in S5 is controlled at D50=0.7±0.05 μm.

6. The method for preparing lithium iron phosphate with high compaction density by resynthesizing waste lithium iron phosphate as claimed in claim 5, characterized in that: The high temperature sintering of the material in S7 refers to heating the spray material in a nitrogen sealed atmosphere for 6 hours, sintering it at a constant temperature of 750° C. for 10 hours, and finally cooling it down and taking it out of the furnace.

Citation Information

Cited By

  • Preparation method for improving compaction density of regenerated lithium iron phosphate and product application

    CN121790367A